Preparation method of rain stripping resistant asphalt rejuvenator
By controlling shear torque and temperature changes, the dispersion state of the blended modified precursor is monitored in real time, forming an asymmetric molecular skeleton. This solves the problem of thermal degradation of chemical bonds during high shear, enabling the efficient preparation of rainwater stripping-resistant asphalt recycling agents and improving interfacial bonding strength and pavement water stripping resistance.
Patent Information
- Application Number
- CN202611587879.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot effectively solve the chemical bonding problem between polar polymers and polyamine coupling agents in asphalt recycling agents during high-shear processes, leading to interfacial delamination problems and a contradiction that frictional heat generation causes thermal degradation of chemical bonds.
By controlling the changes in shear torque and temperature, the dispersion state of the blended modified precursor is monitored in real time during the shearing process. An asymmetric molecular framework is formed by the ring-opening reaction of the polyamine coupling agent and the polar plastic body, and the micro-phase is frozen in situ in the fluid base liquid to reduce the damage of amide bonds caused by frictional heat generation.
It achieves effective formation of micro-phase regions under high shear conditions, maintains the integrity of chemical bonds, improves interfacial bonding strength, reduces the probability of water stripping, and enhances the rain resistance of asphalt pavement.
Smart Images

Figure CN123152303A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing a rain-resistant stripping asphalt rejuvenator, belonging to the technical field of polymer and organic additive modification for plastomeric modified asphalt and self-adhesive rubber asphalt. Background Technology
[0002] In asphalt pavement maintenance, a common recycling method involves infiltrating aged asphalt with lightweight components such as heavy oil extracts rich in aromatics. This improves the rheological properties of the aged asphalt through physical softening between the components. However, in hot and humid regions, where the pavement is constantly exposed to high temperatures and repeated dynamic water pressure, relying solely on this physical softening method results in insufficient chemical bonding between the recycled asphalt and aggregate interface. Free water easily penetrates along the interfacial capillary pores and, under the influence of surface tension differences and dynamic water pressure, gradually replaces the asphalt film on the aggregate surface. This leads to localized water erosion developing into larger-scale delamination damage. To address this interfacial delamination... The problem is that existing improvement methods usually involve adding polar plastics containing active groups to the regeneration system to enhance interfacial bonding through chemical grafting of polymer chain segments. However, in actual dispersion, high-viscosity polar polymers need to undergo continuous and strong mechanical shearing to fully disentangle and form micro-phases in light oil fractions. As the shear rate increases, the frictional heat generated in the dispersion area also increases significantly, and the local temperature can easily rise rapidly. When the local temperature exceeds the range that the amide bonds can withstand, the asymmetric molecular skeleton is prone to irreversible thermal fracture during dispersion, making it difficult to fully retain the structure in the product that can play a chemical bonding role.
[0003] There are limitations in both mechanical shear dispersion and polar modification synthesis control. For example, Chinese invention patent CN117143273B discloses a maleic anhydride grafted onto SBS, its preparation method and application. It uses aluminum trichloride as a catalyst and grafts maleic anhydride onto the styrene benzene ring of SBS through Friedel-Crafts acylation in an organic solvent system. However, this scheme is essentially an offline static organic solvent synthesis route. It not only consumes a large amount of organic solvent and relies on ice-water quenching and acid washing post-treatment, but also has a cumbersome process and a heavy environmental burden. More importantly, when the modified polymer obtained offline is subsequently added to heavy oil base liquid for melt shear secondary dispersion, it still cannot solve the inherent contradiction of chemical bond thermal degradation caused by frictional heat generation under high shear field. It cannot achieve efficient deentanglement and in-situ freezing of micro-phase in solvent-free heavy oil base liquid for blending modification precursors.
[0004] Therefore, how to ensure the uniform formation of micro-phases in the precursor while reducing the damage to polar chemical bonds caused by local frictional heat during shearing, and how to fully utilize the interfacial bonding and self-adhesive reinforcement effects of polyamine coupling agents and silane coupling agents as non-molecular organic additives in plastogenic modified asphalt and self-adhesive rubber asphalt systems, has become a technical problem that needs to be solved in this field. Summary of the Invention
[0005] To address the problems in the background art, the technical solution of the present invention is as follows: A method for preparing a rainwater-resistant stripping asphalt recycling agent, comprising the following steps:
[0006] Step S101: Heat the heavy oil extract with an aromatic fraction of 45% to 55% by mass to 110°C to 120°C and maintain the temperature under continuous stirring to obtain a fluid base liquid.
[0007] Step S102: The polar plastic body containing maleic anhydride grafted segments is mixed with a polyamine coupling agent at a mass ratio of 4:1 to 6:1 and then fed into a mixing equipment. The mixing temperature is controlled at 160°C to 175°C, and the rotor shearing rate is set at 2800 rpm to 3500 rpm. The shearing is continued for 15 min to 25 min, so that the active amino groups of the polyamine coupling agent and the anhydride groups of the polar plastic body undergo a ring-opening reaction to construct an asymmetric molecular skeleton and output the blended modified precursor.
[0008] Step S103: Add 15% to 25% by mass of the blended modified precursor to the fluid base liquid, set the initial rotation speed to 4000 rpm to 5000 rpm and control the system temperature to 140°C to 150°C to start the shearing device, monitor the shearing torque of the shearing device in real time, and when the torque fluctuation variance in multiple consecutive acquisition cycles decreases to the predetermined convergence threshold, control the rotation speed of the shearing device to step down to 1500 rpm to 2000 rpm and simultaneously control the system temperature to drop to 120°C to 125°C, maintain shearing for 10 min to 15 min, so that the blended modified precursor freezes in situ into micro-phase in the fluid base liquid;
[0009] Step S104: Cool down to room temperature of 25°C and output rain-resistant stripping asphalt recycling agent; wherein, the shear time of the ring-opening reaction in step S102 is calculated and determined based on the initial dynamic viscosity of the polar plastic body at 160°C, the apparent activation energy constant of the ring-opening reaction, the rotor shear rate, and the mixing temperature according to a quantitative relationship proportional to the product of the initial dynamic viscosity and the apparent activation energy constant, and inversely proportional to the product of the rotor shear rate and the natural logarithm of the mixing temperature, so that the conversion rate of the amidation reaction reaches the critical threshold.
[0010] Preferably, in step S101, the heavy oil extract is catalytic cracking clarified oil, and the dynamic viscosity of the heavy oil extract at 25°C is 1.5 Pa·s to 2.5 Pa·s, and the saturated mass fraction is less than 15%. The heavy oil extract is heated to 115°C and the built-in anchor stirrer of the reactor is turned on, and the speed is set to 100 rpm to maintain a constant temperature, so as to keep the heavy oil extract in a homogeneous fluid base liquid state, which is used to provide a compatible swelling medium for the subsequent blending modification precursor.
[0011] Preferably, in step S102, the polar plastic body is a maleic anhydride-grafted ethylene-vinyl acetate copolymer, with a maleic anhydride grafting mass fraction of 0.8% to 1.2% and a melt index of 1.0 g / 10 min to 1.5 g / 10 min at 190°C and a load of 2.16 kg; the polyamine coupling agent is diethylenetriamine or N-aminoethyl-γ-aminopropyltrimethoxysilane; the mass ratio of the polar plastic body to the polyamine coupling agent is 5:1; the asymmetric molecular skeleton generated by the ring-opening reaction contains amide bonds formed by the reaction of anhydride groups and active amino groups, and extends at one end with a lithophilic silanol group or an amino group, and at the other end with a pitch-loving polyolefin segment.
[0012] Preferably, in step S103, the real-time monitoring sampling period for shear torque is 10s to 30s, and the number of consecutive sampling periods is 3; the variance of the shear torque value within the 3 consecutive sampling periods is calculated. When the torque fluctuation variance is continuously less than the set convergence threshold of 0.05N·m, it indicates that the disentanglement of the blended modified precursor in the fluid base liquid is completed and it is dispersed into micro-phase with a particle size of 0.5μm to 3.0μm, and the speed reduction and cooling control are triggered.
[0013] Preferably, step S103 includes the following deceleration and cooling sub-steps: Step S1031, when the deceleration and cooling control are triggered, the speed of the shearing device is reduced to 1800 rpm within 1 min to 2 min, and the system temperature is controlled to drop to 122°C. Shearing is maintained at 1800 rpm and 122°C for 10 min to 15 min.
[0014] Preferably, in step S102, the mixing equipment adopts a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1 and the ability to control temperature in zones, and the rotor shear rate is set by the screw speed; in step S103, the shearing equipment adopts a vertical high-shear emulsifier, which is installed at the bottom of the high-shear reaction tank, and the high-shear reaction tank is equipped with an external heat transfer oil bath circulation temperature control system with a temperature control accuracy of ±1℃.
[0015] Preferably, the prepared rain-resistant stripping asphalt recycling agent has a penetration of 150 dmm to 200 dmm at 25°C and a dynamic viscosity of 180 Pa·s to 260 Pa·s at 60°C.
[0016] Preferably, before step S104, a pump-out filtration step is also included: after the system temperature is maintained at 120°C to 125°C and shearing is maintained for 10 to 15 minutes, the shearing equipment is turned off, the product is pumped out from the high-shear reaction tank, filtered through a pipeline filter with a mesh size of 150 μm, and then naturally cooled to room temperature of 25°C to output the finished product, rain-resistant stripping asphalt recycling agent.
[0017] Preferably, after step S104, the method further includes the step of applying the anti-stripping asphalt recycling agent to the thermal recycling of aged asphalt mixture: the prepared anti-stripping asphalt recycling agent is added to the aged asphalt mixture heated to 150°C to 160°C at a mass ratio of 3% to 8%, and wet-mixed in a mixing tank for 60s to 90s.
[0018] Compared with the prior art, the beneficial effects of the present invention are:
[0019] 1. In the preparation of rain-resistant stripping asphalt recycling agents, the dispersion state of the blended modified precursor can be judged by the change of shear torque. This can more accurately determine the timing when it completes deentanglement and forms micro-phase, avoiding the continued high-intensity shearing after the desired dispersion state has been reached. Subsequently, the shear strength and system temperature are reduced, and the local heat generated during the dispersion process is absorbed by the fluid base liquid. This can reduce the thermal degradation of amide bonds due to excessive temperature, while maintaining the micro-phase dispersion state of the blended modified precursor in the fluid base liquid. Thus, the material dispersion effect and the complete preservation of the asymmetric molecular skeleton are taken into account.
[0020] 2. This scheme determines the shear time required for the ring-opening reaction based on the initial dynamic viscosity of the polar plastic, the apparent activation energy constant of the ring-opening reaction, the rotor shear rate, and the mixing temperature. This makes the mixing time no longer solely dependent on fixed empirical values, but adaptable to the material's own state and actual mixing conditions. This is beneficial for the polar plastic and the polyamine coupling agent to fully undergo the ring-opening reaction and form an asymmetric molecular skeleton, while also reducing the irreversible breakage of polymer chains caused by excessively long shear times, thus maintaining a good balance between the degree of ring-opening reaction and the shearing process. Attached Figure Description
[0021] Figure 1 This is a flowchart illustrating the preparation process of the asphalt recycling agent using shear blending according to the present invention.
[0022] Figure 2 This is a diagram showing the physical phase evolution of the modified precursor of this invention.
[0023] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0024] The technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application are within the scope of protection of this application.
[0025] A method for preparing a rain-resistant stripping asphalt recycling agent includes the following steps:
[0026] Step S101: Heat the heavy oil extract with an aromatic fraction of 45% to 55% by mass to 110°C to 120°C and maintain the temperature under continuous stirring to obtain a fluid base liquid.
[0027] Step S102: The polar plastic body containing maleic anhydride grafted segments is mixed with a polyamine coupling agent at a mass ratio of 4:1 to 6:1 and then fed into a mixing equipment. The mixing temperature is controlled at 160°C to 175°C, and the rotor shearing rate is set at 2800 rpm to 3500 rpm. The shearing is continued for 15 min to 25 min, so that the active amino groups of the polyamine coupling agent and the anhydride groups of the polar plastic body undergo a ring-opening reaction to construct an asymmetric molecular skeleton and output the blended modified precursor.
[0028] Step S103: Add 15% to 25% by mass of the blended modified precursor to the fluid base liquid, set the initial rotation speed to 4000 rpm to 5000 rpm and control the system temperature to 140°C to 150°C to start the shearing device, monitor the shearing torque of the shearing device in real time, and when the torque fluctuation variance in multiple consecutive acquisition cycles decreases to the predetermined convergence threshold, control the rotation speed of the shearing device to step down to 1500 rpm to 2000 rpm and simultaneously control the system temperature to drop to 120°C to 125°C, maintain shearing for 10 min to 15 min, so that the blended modified precursor freezes in situ into micro-phase in the fluid base liquid;
[0029] Step S104: Cool down to room temperature of 25°C and output rain-resistant stripping asphalt recycling agent; wherein, the shear time of the ring-opening reaction in step S102 is calculated and determined based on the initial dynamic viscosity of the polar plastic body at 160°C, the apparent activation energy constant of the ring-opening reaction, the rotor shear rate, and the mixing temperature according to a quantitative relationship proportional to the product of the initial dynamic viscosity and the apparent activation energy constant, and inversely proportional to the product of the rotor shear rate and the natural logarithm of the mixing temperature, so that the conversion rate of the amidation reaction reaches the critical threshold.
[0030] Preferably, in step S101, the heavy oil extract is catalytic cracking clarified oil, and the dynamic viscosity of the heavy oil extract at 25°C is 1.5 Pa·s to 2.5 Pa·s, and the saturated mass fraction is less than 15%. The heavy oil extract is heated to 115°C and the built-in anchor stirrer of the reactor is turned on, and the speed is set to 100 rpm to maintain a constant temperature, so as to keep the heavy oil extract in a homogeneous fluid base liquid state, which is used to provide a compatible swelling medium for the subsequent blending modification precursor.
[0031] Preferably, in step S102, the polar plastic body is a maleic anhydride-grafted ethylene-vinyl acetate copolymer, with a maleic anhydride grafting mass fraction of 0.8% to 1.2% and a melt index of 1.0 g / 10 min to 1.5 g / 10 min at 190°C and a load of 2.16 kg; the polyamine coupling agent is diethylenetriamine or N-aminoethyl-γ-aminopropyltrimethoxysilane; the mass ratio of the polar plastic body to the polyamine coupling agent is 5:1; the asymmetric molecular skeleton generated by the ring-opening reaction contains amide bonds formed by the reaction of anhydride groups and active amino groups, and extends at one end with a lithophilic silanol group or an amino group, and at the other end with a pitch-loving polyolefin segment.
[0032] Preferably, in step S103, the real-time monitoring sampling period for shear torque is 10s to 30s, and the number of consecutive sampling periods is 3; the variance of the shear torque value within the 3 consecutive sampling periods is calculated. When the torque fluctuation variance is continuously less than the set convergence threshold of 0.05N·m, it indicates that the disentanglement of the blended modified precursor in the fluid base liquid is completed and it is dispersed into micro-phase with a particle size of 0.5μm to 3.0μm, and the speed reduction and cooling control are triggered.
[0033] Preferably, step S103 includes the following deceleration and cooling sub-steps: Step S1031, when the deceleration and cooling control are triggered, the speed of the shearing device is reduced to 1800 rpm within 1 min to 2 min, and the system temperature is controlled to drop to 122°C. Shearing is maintained at 1800 rpm and 122°C for 10 min to 15 min.
[0034] Preferably, in step S102, the mixing equipment adopts a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1 and the ability to control temperature in zones, and the rotor shear rate is set by the screw speed; in step S103, the shearing equipment adopts a vertical high-shear emulsifier, which is installed at the bottom of the high-shear reaction tank, and the high-shear reaction tank is equipped with an external heat transfer oil bath circulation temperature control system with a temperature control accuracy of ±1℃.
[0035] Preferably, the prepared rain-resistant stripping asphalt recycling agent has a penetration of 150 dmm to 200 dmm at 25°C and a dynamic viscosity of 180 Pa·s to 260 Pa·s at 60°C.
[0036] Preferably, before step S104, a pump-out filtration step is also included: after the system temperature is maintained at 120°C to 125°C and shearing is maintained for 10 to 15 minutes, the shearing equipment is turned off, the product is pumped out from the high-shear reaction tank, filtered through a pipeline filter with a mesh size of 150 μm, and then naturally cooled to room temperature of 25°C to output the finished product, rain-resistant stripping asphalt recycling agent.
[0037] Preferably, after step S104, the method further includes the step of applying the anti-stripping asphalt recycling agent to the thermal recycling of aged asphalt mixture: the prepared anti-stripping asphalt recycling agent is added to the aged asphalt mixture heated to 150°C to 160°C at a mass ratio of 3% to 8%, and wet-mixed in a mixing tank for 60s to 90s.
[0038] Example 1: In this example, catalytic cracking clarified oil with an aromatic content of 45% to 55% by mass, a dynamic viscosity of 1.5 Pa·s to 2.5 Pa·s at 25°C, and a saturation content of less than 15% by mass was used as a heavy oil extract. The heavy oil extract was put into a high-shear reaction vessel equipped with an organic external heat transfer oil bath circulation temperature control system and heated to 115°C. The built-in anchor stirrer of the high-shear reaction vessel was turned on and the speed was set to 100 rpm to maintain a constant temperature, so as to prepare a homogeneous fluid base liquid, which was used to provide a compatible swelling medium for subsequent blending modification precursors.
[0039] A maleic anhydride-grafted ethylene-vinyl acetate copolymer with a maleic anhydride grafting mass fraction of 0.8% to 1.2% and a melt index of 1.0 g / 10 min to 1.5 g / 10 min at 190℃ and 2.16 kg load was selected as a polar plastic body. N-aminoethyl-γ-aminopropyltrimethoxysilane was weighed as a polyamine coupling agent. The polar plastic body and the polyamine coupling agent were added to a co-rotating twin-screw extruder with a length-to-diameter ratio of 5:1 and a zoned temperature control capability at a mass ratio of 40:1. The mixing temperature was controlled at 165℃, and the rotor shear rate was set. The shear time for the ring-opening reaction is 3000 rpm, and the initial dynamic viscosity of the polar plastic body at 160°C is taken. The apparent activation energy constant is 450 Pa·s. The rotor shear rate is 1.2. 3000 rpm, mixing temperature The equipment calibration coefficient is 165℃. It is 0.035 Pa·s·rpm⁻¹·min⁻¹, according to the formula The reaction time was calculated. The reaction time is 1.01 min, which corresponds to the intrinsic reaction time required for the anhydride groups of the polar plastic body to undergo a molecular-level ring-opening reaction with the active amino groups of the polyamine coupling agent; the continuous shear time in step S102 also includes the time required for the polymer melt to be conveyed, softened, and homogenized in the screw axis, and for the multiphase material to be homogenized and mixed. Based on this, viscosity fluctuation compensation was introduced, and the continuous shearing time was determined to be 18 min. During the continuous shearing process, the active amino groups of the polyamine coupling agent and the anhydride groups of the polar plastic body underwent a ring-opening reaction to generate amide bonds, constructing an asymmetric molecular skeleton with a lithophilic silanol group at one end and a pitch-philic polyolefin segment at the other end, outputting a blend-modified precursor; among which, For reaction time, This represents the initial dynamic viscosity of the polar plastic at 160°C. The apparent activation energy constant for the ring-opening reaction; For the set rotor shear rate, The mixing temperature, As the equipment calibration coefficient, in the actual engineering calculation and data substitution process, the mixing temperature is uniformly converted to thermodynamic absolute temperature for natural logarithmic calculation. The set mixing temperature of 165℃ plus 273.15 is converted to 438.15K and then substituted into the logarithmic function.
[0040] A 20% mass fraction of the blended modified precursor was added to the fluid base liquid. A vertical high-shear emulsifier installed at the bottom of the high-shear reactor was started, with an initial rotation speed of 4500 rpm and a system temperature of 145℃. The shear torque was monitored in real-time using a sampling sensor at the bottom of the high-shear reactor at a 20-second sampling cycle. The variance of the shear torque values over three consecutive sampling cycles was calculated, and this calculation result was used as the torque fluctuation variance. A convergence threshold was set based on the torque background wave of the fluid base liquid at the same shear temperature and rotation speed. The torque fluctuation state of the modified precursor during the formation of 0.5μm to 3.0μm microphase regions was calibrated. When the torque fluctuation variance was continuously less than the set convergence threshold of 0.05 N·m, it was determined that the disentanglement of the modified precursor in the fluid base liquid was completed and it was dispersed into microphase regions with a particle size of 0.5μm to 3.0μm. This triggered speed reduction and temperature control, controlling the speed of the vertical high-shear emulsifier to stepwise decrease to 1800 rpm within 1.5 min, and simultaneously controlling the system temperature to decrease to 122℃. Shearing was maintained at 0 rpm and 122°C for 12 minutes. The overall specific heat capacity of the fluid-based liquid absorbed the local frictional heat peak at the micro-phase interface, freezing it in situ at the micro-phase interface before the asymmetric molecular framework thermally fractured. This maintained the micro-phase dispersion and improved the retention rate of intact amide bonds. In actual control, when the system temperature dropped to 122°C and the shearing speed decreased to 1800 rpm, the apparent viscosity of the fluid-based liquid increased rapidly with decreasing temperature. The increased flow resistance caused the micro-phase of the blended modified precursor to... Brownian diffusion rate decreases sharply; at the same time, precursor molecular chain segments undergo conformational freezing at 122°C, effectively isolating their excess surface free energy by the high-viscosity base liquid medium, preventing collisions and secondary aggregation between micro-phase droplets. Combined with the uniform kinetic energy input maintained by low-speed and mild shear at 1800 rpm, the micro-phase is physically locked in a suspended dispersion state with a particle size of 0.5 μm to 3.0 μm, thus maintaining the morphological stability of the micro-phase throughout the subsequent cooling to room temperature process, avoiding sedimentation or phase separation.
[0041] After maintaining the system temperature at 120℃ to 125℃ and sustaining shear for 12 minutes, the vertical high-shear emulsifier was shut down. The product was pumped out of the high-shear reaction tank, filtered through a pipe filter with a mesh size of 150μm, and allowed to cool naturally to room temperature of 25℃. The resulting rain-resistant stripping asphalt rejuvenator had a penetration of 150dmm to 200dmm at 25℃ and a dynamic viscosity of 180Pa·s to 260Pa·s at 60℃. (The last sentence appears to be incomplete and possibly refers to a specific product, "5%..."). The mass fraction is added to aged asphalt mixture heated to 155℃ and wet-mixed in a mixing tank for 75 seconds. The fluid base liquid carries the undegraded asymmetric molecular skeleton into the aggregate interface. The stone-loving end chemically adsorbs silicates on the aggregate surface, while the asphalt-loving end forms physical entanglement with the aged asphalt, reconstructing a three-dimensional interlocking anchoring network. This improves the interfacial adhesion work and self-adhesive toughness, and under the action of dynamic water pressure, it blocks the capillary penetration path of water to the interface, reduces the water replacement space, and lowers the probability of pavement water stripping under precipitation conditions.
[0042] Example 2: In this example, catalytic cracking clarified oil was selected as the heavy oil extract, with an aromatic content of 50% by mass, a dynamic viscosity of 2.1 Pa·s at 25°C, and a saturation content of 12.3% by mass. Maleic anhydride-grafted ethylene-vinyl acetate copolymer with a maleic anhydride grafting content of 1.0% and a melt index of 1.2 g / 10 min at 190°C and a load of 2.16 kg was selected as the polar plastic body. N-aminoethyl-γ-aminopropyltrimethoxysilane was weighed as the polyamine coupling agent. The test platform was equipped with a high-shear reaction vessel with a torque sensor and a vertical high-shear emulsifier installed at its bottom, as well as a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1. Using an instrument, Fourier transform infrared spectrometer, dynamic shear rheometer, and asphalt mixture freeze-thaw splitting test apparatus, the mass fraction of the blended modified precursor, the mass ratio of polar plastic body to polyamine coupling agent, shear rate, and cooling quenching freezing temperature were varied to prepare the present invention sample group, the missing control group, the out-of-range control group, and the conventional comparison sample group. The asphalt recycling agent samples prepared in each group were added to the aged asphalt mixture at a mass dosage of 5%, and a dynamic water pressure pulse of 10 Hz frequency and 0.5 MPa water pressure was applied to test the retention rate of amide bond characteristic peaks, the average particle size of micro-phase, the adhesion work of the recycled asphalt and aggregate interface, the freeze-thaw splitting strength ratio (TSR), and the water immersion Marshall residual stability.
[0043] Using a 20% blended modified precursor mass fraction and a 5:1 mass ratio of polar plastic body to polyamine coupling agent as the formulation of sample group 2 of this invention, the sample was sheared at 4500 rpm and 145℃. When the torque fluctuation variance decreased to the set convergence threshold of 0.05 N·m within three consecutive acquisition cycles, the rotation speed was reduced to 1800 rpm and the system temperature was simultaneously reduced to 122℃ and maintained. After this process, the retention rate of amide bond characteristic peaks was 93.6%, the average particle size of the microphase was 1.8 μm, the interfacial adhesion work was 56.8 mJ·m⁻², the freeze-thaw splitting strength ratio was 92.4%, and the water immersion Marshall residual stability was 93.5%.
[0044] Maintaining the same precursor dosage and the same mass ratio of polar plastic to polyamine coupling agent, the missing control group 1 was continuously sheared for 35 min at 4500 rpm and 145℃ without deceleration. The retention rate of the characteristic peak of the amide bond was 32.5%, the average particle size of the microphase was 0.8 μm, the interfacial adhesion work was 28.6 mJ·m⁻², the freeze-thaw splitting strength ratio was 72.1%, and the water immersion Marshall residual stability was 73.8%. This group was subjected to high-speed shearing and high temperature. The local heat peaks accumulated by the internal friction of shearing caused thermal degradation of the amide bonds in the asymmetric molecular skeleton. In the sample group 2 of this invention, the speed and system temperature were reduced after the torque fluctuation variance reached the set convergence threshold. The fluid base absorbed the local frictional heat peaks at the interface of the microphase, so that the microphase remained dispersed while reducing the thermal degradation of the amide bonds.
[0045] The missing control group 2 used the feeding conditions corresponding to the mass fraction of 20% blended modified precursor, with the mass ratio of polar plastic body to polyamine coupling agent set to 1:0. It was sheared at 4500 rpm and 145℃ without the addition of polyamine coupling agent. The retention rate of amide bond characteristic peaks in this group was recorded as --, the average particle size of the microphase was 3.8 μm, the interfacial adhesion work was 22.4 mJ·m⁻², the freeze-thaw splitting strength ratio was 68.5%, and the water immersion Marshall residual stability was 70.2%. Under the condition of lacking polyamine coupling agent, the polar plastic body could not form an asymmetric molecular skeleton through the corresponding ring-opening reaction. The resulting microphase particle size and interfacial adhesion work showed corresponding differences from the sample group 2 of the present invention.
[0046] Further altering the mass fraction of the blended modified precursor and the mass ratio of the polar plastic body to the polyamine coupling agent, sample group 1 of this invention used a 15% blended modified precursor mass fraction and a 4:1 mass ratio. Shearing was performed at 4000 rpm and 140℃. After the torque fluctuation variance converged, the rotational speed was reduced to 1500 rpm and the system temperature was lowered to 120℃ and maintained. The resulting amide bond characteristic peak retention rate was 91.2%, the average particle size of the microphase was 1.2 μm, the interfacial adhesion work was 51.4 mJ·m⁻², and the freeze-thaw splitting strength ratio was 88.3%. The water-immersed Marshall residual stability was 89.1%. Sample 3 of this invention used a 25% blended modified precursor mass fraction and a 6:1 mass ratio. It was sheared at 5000 rpm and 150℃. After the torque fluctuation variance converged, the speed was reduced to 2000 rpm and the system temperature was reduced to 125℃ and maintained. The retention rate of the characteristic peak of the amide bond was 90.8%, the average particle size of the microphase was 2.5 μm, the interfacial adhesion work was 54.2 mJ·m⁻², the freeze-thaw splitting strength ratio was 90.1%, and the water-immersed Marshall residual stability was 91.2%.
[0047] The mass fraction of the blended modified precursor was reduced to 10% to form an out-of-range control group 1. The mass ratio of polar plastic body to polyamine coupling agent was maintained at 5:1. Shearing was performed at 4500 rpm and 145℃. After the torque fluctuation variance converged, the temperature was reduced to 1800 rpm and maintained at 122℃. The retention rate of the characteristic peak of the amide bond was 92.1%, the average particle size of the microphase was 1.6 μm, the interfacial adhesion work was 33.5 mJ·m⁻², the freeze-thaw splitting strength ratio was 75.4%, and the water immersion Marshall residual stability was 76.8%. At this dosage, the number of aggregate-loving ends and bituminous ends entering the aggregate interface decreased, and the interfacial adhesion work and water stability index decreased accordingly.
[0048] The mass fraction of the blended modified precursor was increased to 30% to form an out-of-range control group 2. The mass ratio of polar plastic body to polyamine coupling agent remained at 5:1. Shearing was performed at 4500 rpm and 145℃. After the torque fluctuation variance converged, the temperature was reduced to 1800 rpm and maintained at 122℃. The retention rate of the characteristic peak of the amide bond was 88.4%, the average particle size of the microphase was 5.4 μm, the interfacial adhesion work was 42.1 mJ·m⁻², the freeze-thaw splitting strength ratio was 79.2%, and the water immersion Marshall residual stability was 80.5%. At this dosage, the high-concentration polymer microphase aggregated and overlapped, the average particle size of the microphase increased, and the thermal storage stability decreased accordingly.
[0049] The out-of-range control group 3 used a 20% blended modified precursor mass fraction and a 5:1 mass ratio, and sheared at 4500 rpm and 145℃. After the torque fluctuation variance converged, it was maintained at 135℃ and sheared again. The retention rate of the characteristic peak of the amide bond was 58.3%, the average particle size of the microphase was 2.1 μm, the interfacial adhesion work was 38.2 mJ·m⁻², the freeze-thaw splitting strength ratio was 78.6%, and the water immersion Marshall residual stability was 79.1%. After increasing the holding temperature after cooling, the retention rate of the characteristic peak of the amide bond decreased in this group.
[0050] The out-of-range control group 4 used a 20% blended modified precursor mass fraction, increasing the mass ratio of polar plastic body to polyamine coupling agent to 8:1. Shearing was performed at 4500 rpm and 145℃. After the torque fluctuation variance converged, the temperature was reduced to 1800 rpm and maintained at 122℃. The resulting amide bond characteristic peak retention rate was 76.4%, the average particle size of the microphase was 2.8 μm, the interfacial adhesion work was 41.5 mJ·m⁻², the freeze-thaw splitting strength ratio was 81.3%, and the water immersion Marshall residual stability was 82.0%. Under this ratio, the increased amount of polar plastic body relative to the polyamine coupling agent resulted in unreacted anhydride residues and a corresponding decrease in interfacial adhesion work.
[0051] The conventional comparative sample group had a precursor mass fraction of 0, a polar plastic body to polyamine coupling agent mass ratio of --, no precursor blending modification was performed, only fluid-based liquid softening was used, the amide bond characteristic peak retention rate and microphase average particle size of this group were both recorded as --, the interfacial adhesion work was 18.2 mJ·m⁻², the freeze-thaw splitting strength ratio was 62.4%, and the water immersion Marshall residual stability was 65.1%.
[0052] The test results corresponding to the proportions and process conditions of each group show that when the mass fraction of the blended modified precursor is less than 15%, the number of stone-loving and bituminous ends is insufficient; when it is increased to 30%, the polymer microphases aggregate and overlap; when the maintenance temperature after cooling is increased to 135°C, the retention of amide bonds decreases; when the mass ratio of polar plastic body to polyamine coupling agent is increased to 8:1, the unreacted anhydride increases. Therefore, the mass ratio of 4:1 to 6:1, the mass fraction of the blended modified precursor of 15% to 25%, and the maintenance temperature of 120°C to 125°C after cooling used in this embodiment correspond to the appropriate process range for ensuring interfacial chemical bonding and rainwater stripping resistance.
[0053] In continuous twin-screw extrusion compounding production, the control of the amidation reaction conversion rate reaching the critical threshold of 85% is achieved through a closed-loop interlock of process parameters. Specifically, a near-infrared spectral absorption sensor is equipped at the extruder outlet to collect the intensity change of the characteristic absorption peak of amide at 1650 cm⁻¹ in real time. When the amidation reaction conversion rate measured online by infrared spectroscopy reaches 85%, the system automatically maintains the current feeding rate, screw speed, and temperature control. If the conversion rate is detected to be lower than 85%, the control system reduces the screw feed rate through closed-loop feedback, prolonging the residence and shearing time of the material inside the extruder, so that the amidation reaction conversion rate reaches and is maintained above the critical threshold of 85% at the discharge.
[0054] Example 3: Current equipment calibration coefficients for different mixing equipment The test was conducted using a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1 and zoned temperature control capabilities. The initial dynamic viscosity was measured. The apparent activation energy constant is 450 Pa·s. A 1.2-mass anhydride-grafted ethylene-vinyl acetate copolymer was fed into a co-rotating twin-screw extruder with N-aminoethyl-γ-aminopropyltrimethoxysilane at a mass ratio of 5:1, and the mixing temperature was controlled. The temperature is 165℃, and the rotor shear rate is... At a speed of 3000 rpm, extrudate samples were taken at 2-minute discrete time intervals during operation. The area ratio of the amide carbonyl absorption peak at 1650 cm⁻¹ to the acid anhydride carbonyl absorption peak at 1785 cm⁻¹ was measured using a Fourier transform infrared spectroscopy (FTIR) instrument. The reaction time was measured when the amidation reaction conversion rate reached the critical threshold of 85%. It is 1.01 min. and the corresponding , , and Substitute into the following formula: The equipment calibration coefficient of the co-rotating twin-screw extruder was calculated. The value is 0.035 Pa·s·rpm⁻¹·min⁻¹. The aforementioned 1.01 min corresponds to the intrinsic reaction half-life of the ring-opening chemical reaction of the active functional groups under the calibration conditions, and is used as the calibration value for the ring-opening reaction shear time. In the actual mixing process of the equipment, there is overall entanglement and fluid retention distribution of polymer chain segments. Under high shear, the local melt viscosity fluctuates. Therefore, viscosity fluctuation compensation is used to determine the overall duration of shear in step S102 without changing the reaction time. The calculation relationship is as follows: the viscosity fluctuation compensation time is obtained by multiplying the intrinsic reaction time by the overall mixing amplification factor of 17.8, which is determined based on the melt viscosity shear thinning coefficient and the length-to-diameter ratio of the flow channel. The compensation time is 16.99 min. After adding it to the intrinsic reaction time of 1.01 min, the actual continuous shear time inside the extruder is determined to be 18 min.
[0055] To calibrate the convergence threshold of torque fluctuation variance during the dynamic shear dispersion process of the blended modified precursor, a high-shear reaction tank equipped with an externally heated oil bath temperature control system was used. Before adding 20% by mass of the blended modified precursor, the vertical high-shear emulsifier at the bottom of the reaction tank was started, and the pure catalytic cracking clarified oil fluid base was sheared for 10 min at 145℃ and 4500 rpm. Fifty sets of torque data were collected at a sampling period of 20 s, and the background fluctuation variance was calculated. The torque was initially set at 0.012 N²·m². Subsequently, the blending-modified precursor was introduced to initiate shearing. The blend system exhibited an increase in apparent torque accompanied by fluctuations due to polymer chain entanglement. As the blending-modified precursor gradually de-entangled and dispersed to form microphases with particle sizes ranging from 0.5 μm to 3.0 μm, the torque fluctuation variance was calculated using a sliding window comprising three acquisition cycles. In this embodiment, the convergence judgment always uses the torque fluctuation variance as the comparison object. When three consecutive acquisition cycles... When the temperature drops below the set convergence threshold of 0.05 N·m, the speed of the vertical high-shear emulsifier is triggered to drop to 1800 rpm within 1.5 min. At the same time, the system temperature is lowered to 122℃ and maintained at shear for 12 min. The local frictional heat peak of the micro-phase interface is absorbed by the fluid base liquid, so that the micro-phase is frozen in situ.
[0056] During the high-speed shearing process at 4500 rpm, the internal frictional heat generated between polymer molecular chain segments is concentrated in the micron-scale interface thin layer. The thickness of the fluid base liquid thin layer is several microns. The heat conduction response time between the interface micro-region and the surrounding base liquid is less than 0.1 ms, and the interface heat is then conducted to the surrounding fluid base liquid. When the deentanglement of the blended modified precursor is completed and the rotation speed is triggered to drop to 1800 rpm, the mechanical kinetic energy input decreases with the decrease in rotation speed. The interface heat continues to diffuse to the fluid base liquid, causing the micro-region phase interface temperature to drop below the amide bond thermal degradation threshold within milliseconds. Subsequently, the external heat transfer oil bath circulation temperature control system completes the overall cooling of the system within minutes.
[0057] The dynamic viscosity of the heavy oil extract at 25℃ ranges from 1.5 Pa·s to 2.5 Pa·s. When a fluid base liquid is prepared using a heavy oil extract with a dynamic viscosity of 2.5 Pa·s at 25℃, the additional shear resistance generated by the fluid base liquid causes a temperature drift of 0.8℃ / min at 145℃. The external heat transfer oil bath circulation temperature control system reduces the circulating oil temperature by 3℃ to offset the heat generated by internal friction. When the shearing is maintained at 4500 rpm for 40 min and the torque fluctuation variance is maintained in the range of 0.05 N·m to 0.08 N·m, the control system extends the high shear maintenance time by 4 min. When the torque fluctuation variance drops to 0.05 N·m, the speed of the vertical high shear emulsifier is triggered to drop stepwise to 1800 rpm, while the system temperature is reduced to 122℃ and maintained at shearing for 12 min. In the obtained rain-resistant stripping asphalt rejuvenator, the retention rate of amide bond characteristic peaks is 91.5%, and the average particle size of the microphase is 2.1 μm.
[0058] Example 4: This example combines Figures 1 to 2 This paper describes a method for preparing a rainwater-resistant stripping asphalt recycling agent, such as... Figure 1 As shown, firstly, step S101 is performed, heating a heavy oil extract with an aromatic content of 45% to 55% by mass to 110°C to 120°C and maintaining a constant temperature under continuous stirring to obtain a fluid base liquid; then, step S102 is performed, mixing a polar plastic body containing maleic anhydride grafted segments with a polyamine coupling agent at a mass ratio of 4:1 to 6:1 and feeding the mixture into a mixing device, controlling the mixing temperature at 160°C to 175°C, setting the rotor shear rate at 2800 rpm to 3500 rpm, and continuously shearing for 15 min to 25 min, causing the active amino groups of the polyamine coupling agent to undergo a ring-opening reaction with the anhydride groups of the polar plastic body to construct an asymmetric molecular skeleton, outputting a blended modified precursor; then, step S103 is performed. A blend of 15% to 25% by mass of the modified precursor is added to the fluid base liquid. The initial rotation speed is set to 4000 to 5000 rpm and the system temperature is controlled at 140°C to 150°C. The shearing equipment is started, and the shearing torque of the shearing equipment is monitored in real time. When the torque fluctuation variance within several consecutive acquisition cycles decreases to the predetermined convergence threshold, the rotation speed of the shearing equipment is stepped down to 1500 to 2000 rpm, and the system temperature is simultaneously controlled to drop to 120°C to 125°C. Shearing is maintained for 10 to 15 minutes, so that the blend of modified precursor is frozen in situ into micro-phase in the fluid base liquid. Finally, step S104 is executed to cool down to room temperature of 25°C, and the rain-resistant stripping asphalt recycling agent is output.
[0059] like Figure 2As shown, a homogeneous fluid-based liquid provides a compatible swelling medium. The blended modified precursor is added to the fluid-based liquid, and a shearing device is activated to shear the system, causing it to enter a disentangled state. In the disentangled state, the shearing torque is monitored in real time. When the torque fluctuation variance decreases to a predetermined convergence threshold, the rotational speed is controlled to decrease stepwise, and the system temperature is simultaneously controlled to decrease, causing the system to migrate from the disentangled state to the suspended and dispersed state. After entering the suspended and dispersed state, shearing is maintained to freeze the blended modified precursor in situ into a micro-phase. As the system naturally cools to room temperature, the suspended and dispersed state eventually transforms into a stable micro-phase morphology.
[0060] Example 5: Using an ultrasonic gap sensor installed on the shear chamber wall of a vertical high-shear emulsifier to collect the actual physical gap between the rotor and stator. Before immersing a 20% mass fraction of the blended modified precursor in a 115°C fluid base, the rotor-stator clearance was measured and the initial rotational speed was compensated; when the clearance... As wear increases from the initial calibration value of 0.20 mm to 0.23 mm, the shear energy density decreases. Therefore, a speed compensation is added to the initial speed setting of 4500 rpm based on the clearance deviation. Calculate according to the following formula: The speed compensation amount is calculated. The initial speed of the vertical high-shear emulsifier was adjusted to 5175 rpm for dynamic shearing, starting at 675 rpm. This is the speed compensation amount. This is the initial speed setting value. To measure the rotor-stator clearance, As the initial calibration gap, when the torque fluctuation variance within three consecutive acquisition cycles drops to less than the set convergence threshold of 0.05 N·m, the rotation speed of the vertical high-shear emulsifier is controlled to step down to 1800 rpm within 1.5 min. At the same time, the system temperature is lowered to 122℃ and maintained at shear for 12 min. The local frictional heat peak of the micro-phase interface is absorbed by the fluid base liquid, and the micro-phase with a particle size of 0.5 μm to 3.0 μm is frozen in situ, reducing the impact of equipment mechanical wear on the phase dispersion of the blended modified precursor.
[0061] The 1.01 min calculated from the reaction time relationship corresponds to the minimum intrinsic reaction half-life required for the polar plastic anhydride group and the active amino group of the polyamine coupling agent to undergo a molecular-level ring-opening chemical reaction at a specific shear rate and temperature. The actual mixing uses a shear time of 15 min to 25 min, which includes the conveying time of the polymer melt in the screw axis, the overall melting and softening time, the homogenization and mixing time of the multiphase materials, and the intrinsic chemical reaction time of 1.01 min. Therefore, the intrinsic reaction time of 1.01 min is included in the total mixing shear time of 15 min to 25 min.
[0062] Aged asphalt mixture heated to 155℃ and with a penetration reduced to 11 dmm at 25℃ was added to the mixing tank. Based on its dynamic viscosity of 850 Pa·s at 60℃, the mass dosage of the anti-stripping asphalt recycling agent was determined to be 6%. The anti-stripping asphalt recycling agent was added at a 6% mass dosage, and the mixing blade speed was set to 75 rpm and wet mixing was maintained for 80 s. The fluid base liquid penetrated and softened the high-viscosity asphalt phase, while simultaneously carrying away the asymmetric molecular skeleton with stone-loving silanol groups at one end and asphalt-loving polyolefin segments at the other end, which diffused to... At the aggregate interface, the silanol groups of the aggregate undergo chemical adsorption with the silicates on the aggregate surface, while the asphalt-loving polyolefin segments physically entangle with the aged asphalt, reconstructing a three-dimensional interlocking anchoring network. Under the dynamic water pressure pulse action of 10Hz frequency and 0.5MPa water pressure, the freeze-thaw splitting strength ratio (TSR) of the recycled asphalt mixture is 90.5%, and the water immersion Marshall residual stability is 91.8%. The intrusion path of water replacing the asphalt film along the capillary pores of the interface is blocked, thereby reducing the probability of delamination failure between the recycled asphalt and aggregate interface under precipitation conditions.
[0063] Example 6: In an industrial-grade high-shear reactor with a capacity of 1000L and equipped with an external heat transfer oil bath circulation temperature control system, a blend system containing micro-phases with particle sizes of 0.5μm to 3.0μm, formed by shearing at 1800rpm and a system temperature of 122℃ for 12min, was maintained at a temperature range of 120℃ to 125℃. The screw pump at the bottom of the reactor was turned on, and the product was pumped out from the bottom of the reactor at a flow rate of 25L / min and sent into a double-pipe filter with a mesh size of 150μm. Pressure sensors were installed on both sides of the inlet and outlet of the pipe filter to collect the filtration pressure difference. When a small amount of undissolved impurities accumulates on the filter screen, it causes a pressure difference in the filter. When the pressure rises from the initial value of 0.02 MPa to the preset switching threshold of 0.08 MPa, the control switching valve switches to the backup pipeline filter and backwashes the original filter to prevent the high-viscosity fluid from stagnating at low flow rates and causing heat accumulation. The pumped product is naturally cooled at room temperature of 25°C. During the discharge process, the micro-phase state of the blended modified precursor remains stable and the amide bonds are intact.
[0064] The apparent activation energy constant 1.2 was obtained by measuring the reaction rate of the ring-opening reaction of the polar plastomeric anhydride under a gradient of 140℃ to 180℃ using differential scanning calorimetry and dynamic rheology. The actual apparent activation energy was measured to be 50.4 kJ / mol. This value was normalized to a dimensionless value by dividing it by the basic activation energy of the degradation of the unmodified polyethylene copolymer, which was 42 kJ / mol, resulting in the apparent activation energy constant 1.2. This value characterizes the increase in the ring-opening activation energy of the maleic anhydride graft structure under a shear thermal field relative to the basic polymer system, and is used as a dimensionless correction factor in the reaction time calculation.
[0065] The finished rain-resistant stripping asphalt recycling agent, naturally cooled to 25°C, was sampled. The penetration at 25°C was measured to be 168 dmm, falling within the range of 150 to 200 dmm. The dynamic viscosity at 60°C was measured to be 215 Pa·s using a rotating thin-film oven and a dynamic viscometer, falling within the range of 180 to 260 Pa·s. The finished sample was then placed in an aluminum tube with a diameter of 25 mm and a height of 140 mm, sealed, and placed in an oven at 163°C for 48 hours. The softening point was measured at the top and bottom of the aluminum tube. The difference between the softening points at the top and bottom was recorded. The thermal storage stability criterion is 1.2℃, below 2.5℃; the micro-phase physically frozen in the fluid base liquid remains compatible with the compatible swelling medium, and no polymer stratification or amide bond decomposition occurs, resulting in a rain-resistant stripping asphalt recycling agent product.
[0066] In the process of mapping from overall torque fluctuation to micro-phase particle size, Taylor instability flow field theory and rheological Taylor number are used for calculation. In a specific shear flow field, the maximum stable particle size of dispersed phase droplets is inversely proportional to the shear stress and interfacial tension of the fluid. The real-time collected torque data reflects the apparent viscosity disturbance caused by suspended phase particles passing through the high shear zone of the rotor and stator. By normalizing the torque fluctuation variance over three consecutive sampling periods, the correspondence between torque fluctuation variance and fluid rheological inhomogeneity is determined. When the torque fluctuation variance drops below 0.05 N·m, the critical shear stress in the corresponding flow field will break up the dispersed phase and homogenize it to a micro-phase size range of 0.5 μm to 3.0 μm. The torque fluctuation variance is used to characterize the micro-phase particle size distribution.
[0067] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the present invention.
[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a rainwater-resistant stripping-resistant asphalt recycling agent, characterized in that, Includes the following steps: Step S101: Heat the heavy oil extract with an aromatic fraction of 45% to 55% by mass to 110°C to 120°C and maintain the temperature under continuous stirring to obtain a fluid base liquid. Step S102: The polar plastic body containing maleic anhydride grafted segments is mixed with a polyamine coupling agent at a mass ratio of 4:1 to 6:1 and then fed into a mixing equipment. The mixing temperature is controlled at 160°C to 175°C, and the rotor shearing rate is set at 2800 rpm to 3500 rpm. The shearing is continued for 15 min to 25 min, so that the active amino groups of the polyamine coupling agent and the anhydride groups of the polar plastic body undergo a ring-opening reaction to construct an asymmetric molecular skeleton and output the blended modified precursor. Step S103: Add 15% to 25% by mass of the blended modified precursor to the fluid base liquid, set the initial rotation speed to 4000 rpm to 5000 rpm and control the system temperature to 140°C to 150°C to start the shearing device, monitor the shearing torque of the shearing device in real time, and when the torque fluctuation variance in multiple consecutive acquisition cycles decreases to the predetermined convergence threshold, control the rotation speed of the shearing device to step down to 1500 rpm to 2000 rpm and simultaneously control the system temperature to drop to 120°C to 125°C, maintain shearing for 10 min to 15 min, so that the blended modified precursor freezes in situ into micro-phase in the fluid base liquid; Step S104: Cool down to room temperature of 25°C and output rain-resistant stripping asphalt recycling agent; wherein, the shear time of the ring-opening reaction in step S102 is calculated and determined based on the initial dynamic viscosity of the polar plastic body at 160°C, the apparent activation energy constant of the ring-opening reaction, the rotor shear rate, and the mixing temperature according to a quantitative relationship proportional to the product of the initial dynamic viscosity and the apparent activation energy constant, and inversely proportional to the product of the rotor shear rate and the natural logarithm of the mixing temperature, so that the conversion rate of the amidation reaction reaches the critical threshold.
2. The method for preparing a rain-resistant stripping-type asphalt recycling agent according to claim 1, characterized in that, In step S101, the heavy oil extract is catalytic cracking clarified oil, and the dynamic viscosity of the heavy oil extract at 25°C is 1.5 Pa·s to 2.5 Pa·s, and the saturated mass fraction is less than 15%. The heavy oil extract is heated to 115°C and the built-in anchor stirrer of the reactor is turned on. The speed is set to 100 rpm to maintain a constant temperature, keeping the heavy oil extract in a homogeneous fluid base liquid state, which is used to provide a compatible swelling medium for the subsequent blending modification precursor.
3. The method for preparing a rain-resistant stripping asphalt recycling agent according to claim 1, characterized in that, In step S102, the polar plastic body is a maleic anhydride-grafted ethylene-vinyl acetate copolymer with a maleic anhydride grafting mass fraction of 0.8% to 1.2% and a melt index of 1.0 g / 10 min to 1.5 g / 10 min at 190 °C and a load of 2.16 kg; the polyamine coupling agent is diethylenetriamine or N-aminoethyl-γ-aminopropyltrimethoxysilane; the mass ratio of polar plastic body to polyamine coupling agent is 5:1; the asymmetric molecular skeleton generated by the ring-opening reaction contains amide bonds formed by the reaction of anhydride groups and active amino groups, and extends at one end with a lithophilic silanol group or amino group, and at the other end with a pitch-loving polyolefin segment.
4. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 1, characterized in that, In step S103, the real-time monitoring sampling period for shear torque is 10s to 30s, and the number of consecutive sampling periods is 3. The variance of the shear torque value within the 3 consecutive sampling periods is calculated. When the torque fluctuation variance is continuously less than the set convergence threshold of 0.05N·m, it indicates that the disentanglement of the blended modified precursor in the fluid base liquid is completed and it is dispersed into micro-phase with a particle size of 0.5μm to 3.0μm, and the speed reduction and cooling control are triggered.
5. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 4, characterized in that, Step S103 includes the following deceleration and cooling sub-steps: Step S1031, when the deceleration and cooling control are triggered, the speed of the shearing device is reduced to 1800 rpm within 1 min to 2 min, and the system temperature is controlled to drop to 122℃. Shearing is maintained at 1800 rpm and 122℃ for 10 min to 15 min.
6. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 1, characterized in that, In step S102, the mixing equipment adopts a co-rotating twin-screw extruder with a length-to-diameter ratio of 40:1 and the ability to control temperature in zones. The rotor shear rate is set by the screw speed. In step S103, the shearing equipment adopts a vertical high-shear emulsifier, which is installed at the bottom of the high-shear reaction tank. The high-shear reaction tank is equipped with an external heat transfer oil bath circulation temperature control system with a temperature control accuracy of ±1℃.
7. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 1, characterized in that, The prepared rain-resistant stripping asphalt recycling agent has a penetration of 150 dmm to 200 dmm at 25°C and a dynamic viscosity of 180 Pa·s to 260 Pa·s at 60°C.
8. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 1, characterized in that, Before step S104, a pump-out filtration step is also included: after the system temperature is maintained at 120°C to 125°C and shearing is maintained for 10 to 15 minutes, the shearing equipment is turned off, the product is pumped out from the high-shear reaction tank, filtered through a pipeline filter with a mesh size of 150 μm, and then naturally cooled to room temperature of 25°C to output the finished product, rain-resistant stripping asphalt recycling agent.
9. The method for preparing a rain-resistant stripping-resistant asphalt recycling agent according to claim 1, characterized in that, After step S104, the process further includes the step of applying the anti-stripping asphalt recycling agent to the thermal recycling of aged asphalt mixture: the prepared anti-stripping asphalt recycling agent is added to the aged asphalt mixture heated to 150°C to 160°C at a mass ratio of 3% to 8%, and wet-mixed in a mixing tank for 60s to 90s.
Citation Information
Patent Citations
A kind of maleic anhydride grafted SBS and its preparation method and application
CN117143273B