Heavy-load adaptive low-carbon composite warm-mixing agent, preparation method and application thereof

The heavy-duty adaptable low-carbon composite warm mix admixture, formulated with multi-components such as Fischer-Tropsch synthetic wax, solves the problems of poor compatibility and insufficient stability of existing warm mix admixtures in heavy traffic and high-temperature areas. It achieves efficient viscosity reduction, stable compatibility and green environmental protection, and is suitable for asphalt pavement construction in heavy traffic and high-temperature and rainy areas.

CN123152304APending Publication Date: 2026-11-24SHANDONG HUIDA NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611515061.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing warm mix asphalt additives cannot simultaneously meet the engineering requirements of efficient viscosity reduction, stable compatibility, green environmental protection, and wide applicability and durability under complex working conditions such as heavy traffic and high temperature regions, which limits the large-scale promotion of warm mix asphalt technology.

Method used

A heavy-duty adaptable low-carbon composite warm mix admixture for use as an asphalt modifier was prepared by compounding a multi-component compound of Fischer-Tropsch synthetic wax, polyoxyethylene polyoxypropylene ether, polyacrylamide, stearamide, antioxidants and organic amine modifiers through melt mixing, compound modification and high-pressure homogenization molding processes.

Benefits of technology

It achieves a synergistic improvement in efficient viscosity reduction, stable storage across the entire temperature range, green environmental protection, and long-lasting plasticity retention, enhancing Marshall stability, dynamic stability, freeze-thaw splitting strength, and low-temperature bending failure strain, thus meeting the complex working conditions required by heavy-duty transportation and high-temperature and rainy regions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152304A_ABST
    Figure CN123152304A_ABST
Patent Text Reader

Abstract

This invention discloses a heavy-duty adaptable low-carbon composite warm-mix admixture, its preparation method, and its application, belonging to the technical field of asphalt pavement materials for road engineering. The heavy-duty adaptable low-carbon composite warm-mix admixture comprises the following components: 40-50 parts of Fischer-Tropsch synthetic wax, 15-25 parts of polyoxyethylene polyoxypropylene ether, 8-12 parts of polyacrylamide, 6-10 parts of compatibility additive, 5-8 parts of antioxidant, 3-7 parts of organic amine modifier, and 3-7 parts of water. This invention overcomes the technical bottleneck of traditional warm-mix admixtures in simultaneously achieving "viscosity reduction, compatibility, stability, and environmental protection" through the synergistic compounding of multiple components. It simultaneously achieves a synergistic improvement in efficient viscosity reduction, full-temperature range storage stability, green environmental protection, and long-lasting plasticity retention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of asphalt pavement materials for road engineering, specifically relating to a heavy-duty adaptable low-carbon composite warm mix agent, its preparation method, and its application. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] In the field of road engineering, hot-mix asphalt mixtures are the mainstream material for pavement construction. However, their production process requires temperatures above 160°C, which not only consumes a large amount of fossil energy but also emits large amounts of CO2, VOCs, and asphalt fumes. Warm-mix asphalt technology can reduce the mixing temperature of the mixture by about 30°C, significantly reducing energy consumption and carbon emissions, and has become one of the core technologies for low-carbon road construction.

[0004] Currently, commercially available warm mix admixtures are mainly divided into three categories: surfactant-based, organic wax-based, and foamed asphalt-based. However, all of them have performance shortcomings: surfactant-based warm mix admixtures have high viscosity reduction efficiency, but they are prone to stratification during high-temperature storage and are not environmentally friendly; organic wax-based warm mix admixtures have good compatibility and are stable during storage, but their viscosity reduction efficiency is limited and they are prone to clumping at low temperatures; foamed asphalt-based warm mix admixtures are green and environmentally friendly, but their viscosity reduction effect is short, their high-temperature stability is poor, and they require additional foaming equipment, making them inconvenient to construct.

[0005] Meanwhile, most existing warm mix asphalt additives are designed only for a single type of asphalt or aggregate, and have poor adaptability to complex working conditions such as heavy traffic and high temperature areas. They cannot simultaneously meet the engineering requirements of "high efficiency viscosity reduction, stable compatibility, green environmental protection, and wide applicability and durability", which limits the large-scale promotion of warm mix asphalt technology. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the present invention aims to provide a heavy-duty adaptable low-carbon composite warm-mix agent, its preparation method, and its application. This low-carbon composite warm-mix agent exhibits excellent overall performance and is suitable for heavy-duty and complex working conditions.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows: In a first aspect, the present invention provides a heavy-duty adaptable low-carbon composite warm-mix agent, comprising the following components: 40-50 parts of Fischer-Tropsch synthetic wax, 15-25 parts of polyoxyethylene polyoxypropylene ether, 8-12 parts of polyacrylamide, 6-10 parts of stearamide, 5-8 parts of antioxidant, 3-7 parts of organic amine modifier, and 3-7 parts of water.

[0008] Secondly, the present invention provides a method for preparing the above-mentioned heavy-duty adaptable low-carbon composite warm-mix agent, comprising the following steps: Modified wax liquid is obtained by melt blending Fischer-Tropsch synthetic wax, stearamide, and antioxidant; Polyoxyethylene polyoxypropylene ether and organic amine modifiers were added to the modified wax liquid for compound modification; After cooling the compounded and modified material, add polyacrylamide and water, and stir to obtain a mixed system; The mixture is homogenized to obtain the final product.

[0009] Thirdly, the present invention provides the application of the above-mentioned heavy-duty adaptable low-carbon composite warm mix agent or the heavy-duty adaptable low-carbon composite warm mix agent prepared by the above-mentioned preparation method as an asphalt modifier.

[0010] Fourthly, the present invention provides a warm-mix asphalt mixture, comprising an asphalt modifier and asphalt; The asphalt modifier is the heavy-duty adaptable low-carbon composite warm mix agent described above or the heavy-duty adaptable low-carbon composite warm mix agent prepared by the above preparation method.

[0011] One or more of the above technical solutions have the following advantages or beneficial effects: This invention overcomes the technical bottleneck of traditional warm-mixing agents, which cannot simultaneously achieve "viscosity reduction, compatibility, stability, and environmental protection," through the synergistic compounding of multiple components. It simultaneously achieves a synergistic improvement in efficient viscosity reduction, stable storage across the entire temperature range, environmental friendliness, and long-lasting plasticity retention.

[0012] This invention possesses exceptional adaptability to heavy-duty operating conditions, addressing the problem of existing warm-mix asphalt additives causing "viscosity reduction leading to deterioration of road performance." Compared to traditional hot-mix asphalt mixtures, warm-mix asphalt mixtures incorporating this invention exhibit a 4.9% increase in Marshall stability, a 10.6% increase in dynamic stability at 60°C, a 4.8% increase in freeze-thaw splitting strength ratio, a 4.7% increase in low-temperature flexural failure strain, and a 15.2% reduction in permeability coefficient. Furthermore, its high-temperature rutting resistance, water stability, low-temperature crack resistance, and water tightness are all superior to hot-mix asphalt mixtures, fully meeting the complex operating conditions required for heavy-duty traffic and hot, rainy regions.

[0013] This invention offers excellent ease of construction and wide applicability. It requires no additional specialized equipment for foaming or modification and is fully compatible with existing conventional asphalt mixture mixing processes.

[0014] This invention offers significant low-carbon, environmentally friendly, and economic benefits. It substantially reduces fossil fuel consumption and emissions of CO2, VOCs, and asphalt fumes; the preparation process is controllable, product performance is stable across batches, no complex equipment is required, it is suitable for industrial mass production, and it possesses excellent economic, environmental, and social benefits. Attached Figure Description

[0015] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0016] Figure 1 For the road performance testing of asphalt mixtures.

[0017] Figure 2 The warm-mix asphalt mixture specimens prepared for the example are shown. Detailed Implementation

[0018] This invention aims to overcome the technical bottleneck of existing warm mix agents that cannot simultaneously achieve "viscosity reduction, compatibility, stability, and environmental protection," and to solve the problems of poor adaptability to heavy-duty working conditions, insufficient storage stability, and weak construction convenience of existing warm mix agents.

[0019] While common organic wax-based warm mix additives (such as Sasobit) can reduce viscosity, some wax components soften at high temperatures, limiting their improvement in high-temperature stability. Surfactant-based warm mix additives can even reduce the high-temperature modulus of the mixture, leading to a decrease in dynamic stability. For heavy-duty applications, warm mix additives can improve the high-temperature shear resistance of asphalt mixtures. In this invention, the addition of a warm mix additive resulted in a dynamic stability of 4260 cycles / mm at 60°C, a 10.6% improvement over hot mix mixtures, far exceeding similar products on the market, and capable of resisting continuous rolling deformation from heavy vehicles.

[0020] Most traditional warm mix additives interfere with the interfacial interaction between asphalt and aggregates, resulting in a lower freeze-thaw splitting strength ratio compared to hot mix additives, making them highly susceptible to water damage under heavy loads and flowing water. Heavy-load adaptability requires warm mix additives to simultaneously enhance asphalt-aggregate adhesion. This invention strengthens the interfacial interaction through components such as polyacrylamide, achieving a freeze-thaw splitting strength ratio of 92.5%, a 4.8% increase compared to hot mix additives, thus resisting erosion from heavy loads and flowing water.

[0021] Ordinary warm-mix additives often suffer from the drawback of "improving at high temperatures but becoming brittle at low temperatures." Excessive wax components can reduce low-temperature toughness, making them prone to cracking under heavy and repeated loading. Heavy-load adaptability requires synergistic improvement in both high-temperature and low-temperature performance. In this invention, the bending failure strain at -10℃ reaches 2680με, which is 4.7% higher than that of hot-mix additives. It still has sufficient deformation capacity under heavy fatigue loading, avoiding brittle cracking.

[0022] After the warm mix technology lowers the construction temperature, if the workability of the mixture is insufficient, it can easily lead to low compaction and high porosity, making it prone to water seepage and deformation under heavy loads. The heavy-load adaptability requirement is that the warm mix agent can still ensure the compaction effect of the mixture under the premise of cooling construction. This invention reduces the permeability coefficient by 15.2% compared to hot mix, resulting in a denser pavement, which can block water damage paths and is suitable for long-term service under heavy loads.

[0023] Therefore, the present invention provides a heavy-duty adaptable low-carbon composite warm mix admixture that can achieve synergistic improvement of multiple properties of a single product, adapt to complex working conditions of heavy traffic, and be compatible with conventional asphalt mixture mixing processes. It requires no additional construction equipment and has both excellent environmental benefits and road performance.

[0024] In one typical embodiment, the present invention provides a heavy-duty adaptable low-carbon composite warm-mix agent, comprising the following components: 40-50 parts of Fischer-Tropsch synthetic wax, 15-25 parts of polyoxyethylene polyoxypropylene ether, 8-12 parts of polyacrylamide, 6-10 parts of stearamide, 5-8 parts of antioxidant, 3-7 parts of organic amine modifier, and 3-7 parts of water.

[0025] Furthermore, in order to achieve better technical results, the heavy-duty adaptable low-carbon composite warm-mix agent includes the following components: 43-47 parts of Fischer-Tropsch synthetic wax, 18-22 parts of polyoxyethylene polyoxypropylene ether, 9-11 parts of polyacrylamide, 7-9 parts of stearamide, 6-7 parts of antioxidant, 4-6 parts of organic amine modifier, and 4-6 parts of water.

[0026] In some embodiments of this implementation, the Fischer-Tropsch synthetic wax is a straight-chain saturated alkane Fischer-Tropsch wax with a melting point of 80~110℃, a penetration of ≤1.0mm at 25℃, and a dropping point of ≥100℃. As a matrix component, it can quickly melt at the mixing temperature to form a lubricating film, reduce the friction between asphalt and aggregate, and at the same time give the warm mix additive excellent storage compatibility and high-temperature stability.

[0027] (1) Melting point 80~110℃, dropping point ≥100℃; (2) Penetration ≤1.0mm at 25℃; (3) Molecular structure is high-purity straight-chain saturated alkane with extremely low content of branched chains and unsaturated bonds. Only Fischer-Tropsch wax that meets the above conditions can rapidly melt at the mixing temperature to form a continuous lubricating film, while ensuring sufficient hardness at room temperature and no softening or sticking at high temperature, ultimately achieving the effect of "reducing viscosity without sacrificing high-temperature stability".

[0028] The mass fraction of Fischer-Tropsch synthetic wax is 40-50 parts. When it is less than 40 parts, the high-temperature stability is insufficient and the dynamic stability decreases by more than 15%; when it is greater than 50%, the viscosity-reducing effect decreases by more than 10%.

[0029] In some embodiments of this implementation, the polyoxyethylene polyoxypropylene ether is a block polyether with an HLB value of 8-12 and a number average molecular weight of 1000-3000. As a core viscosity-reducing component, it can quickly penetrate into the asphalt molecules, break the intermolecular hydrogen bonds, reduce the internal friction of the asphalt, and achieve efficient viscosity reduction.

[0030] (1) Molecular structure: saturated block polyoxyethylene polyoxypropylene ether, without active unsaturated double bonds; (2) HLB value: 8~12; (3) Number average molecular weight: 1000~3000. Block polyethers that meet the above parameter range can quickly penetrate into the gaps between asphalt molecules and break the intermolecular hydrogen bonds to achieve efficient viscosity reduction. They can also form a good compatibility system with the Fischer-Tropsch wax matrix to ensure that they do not separate at high temperature. At the same time, the saturated structure without double bonds can resist oxidative degradation under high temperature mixing and maintain long-term viscosity reduction effect.

[0031] The mass fraction of polyoxyethylene polyoxypropylene ether is 15-25 parts. When it is less than 15 parts, the viscosity reduction rate is less than 30%; when it is more than 25 parts, it will separate into layers during high-temperature storage, with a separation rate of more than 8%.

[0032] In some embodiments of this implementation, the polyacrylamide is a nonionic polyacrylamide with a molecular weight of 3 million to 8 million. As a stabilizing and reinforcing component, it can improve the high-temperature stability of the system, prolong the viscosity reduction time, and enhance the interfacial adhesion between asphalt and aggregates, thus significantly improving the water stability of the mixture.

[0033] Heavy-duty roads require warm-mix additives to maintain stable performance and long-lasting viscosity reduction at high mixing temperatures. Nonionic PAM exhibits excellent thermal stability of its amide groups, resisting degradation at mixing temperatures of 130-140°C and maintaining a long-lasting viscosity reduction effect for up to 12 hours. In contrast, anionic PAM is prone to decarboxylation at high temperatures, and cationic PAM's quaternary ammonium salts are easily decomposed at high temperatures, both leading to rapid performance degradation and significantly shortened viscosity reduction time, failing to meet the demands of long-distance transportation and large-scale construction.

[0034] The mass fraction of polyacrylamide is 8-12 parts. When it is less than 8 parts, the improvement in water stability is not significant, and the freeze-thaw splitting strength ratio is less than 85%; when it is greater than 12 parts, the viscosity of the system increases, and the viscosity-reducing effect decreases.

[0035] In some embodiments of this implementation, stearamide is used as a compatibility aid, which can improve the compatibility between wax components and asphalt, prevent wax crystal agglomeration, and further enhance the storage stability of the system.

[0036] The core function of stearamide is as a molecular bridge: one end is miscible with the nonpolar Fischer-Tropsch wax matrix through an alkane chain, and the other end is combined with polyoxyethylene polyoxypropylene ether through a polar amide group, thereby solving the compatibility problem between the wax phase and the surfactant phase and achieving zero stratification during high-temperature storage. To play this role, the product must meet the following hard thresholds: (1) Molecular structure: saturated linear monoamide (mainly octadecyl stearamide), without double bonds or diamide skeleton; (2) Purity: amide content ≥98%, free fatty acid content is extremely low; (3) Melting point: 98~105℃, precisely matching the melting temperature range of Fischer-Tropsch wax; (4) Low impurity index: acid value ≤1mgKOH / g, iodine value ≤1gI2 / 100g, ash and moisture content are extremely low.

[0037] The mass fraction of stearamide is 6 to 10 parts. When it is less than 6 parts, the compatibility is poor and stratification occurs; when it is more than 10 parts, the viscosity-reducing effect is diluted.

[0038] In some embodiments of this implementation, the organic amine modifier is at least one of diethanolamine, triethanolamine, and ethylenediamine, preferably diethanolamine, used to adjust the pH value of the system, improve the compatibility of the surfactant and asphalt, and reduce high-temperature stratification.

[0039] In some embodiments of this implementation, the antioxidant is a hindered phenolic antioxidant, preferably at least one of antioxidant 1010 and antioxidant 1076, used to delay the thermo-oxidative aging of the components and extend the storage period of the warm-mixing agent.

[0040] In some embodiments of this implementation, water is used as a system regulator to adjust the fluidity of the system and improve the homogeneous dispersion of each component.

[0041] In one typical embodiment, the present invention provides a method for preparing the above-mentioned heavy-duty adaptable low-carbon composite warm-mix agent, comprising the following steps: Modified wax liquid is obtained by melt blending Fischer-Tropsch synthetic wax, stearamide, and antioxidant; Polyoxyethylene polyoxypropylene ether and organic amine modifiers were added to the modified wax liquid for compound modification; After cooling the compounded and modified material, add polyacrylamide and water, and stir to obtain a mixed system; The mixture is homogenized to obtain the final product.

[0042] In some embodiments of this implementation, the specific preparation steps of the modified wax liquid are as follows: Fischer-Tropsch synthetic wax and stearamide are added to a closed reactor, heated to melt, and then an antioxidant is added and stirred to obtain the modified wax liquid.

[0043] Further, the temperature is increased to 100~110℃. During the melting process, the stirring speed is 200-300 r / min.

[0044] Furthermore, after adding the antioxidant, continue stirring for 25-35 minutes.

[0045] In some embodiments of this implementation, the specific preparation steps for the compound modification are as follows: polyoxyethylene polyoxypropylene ether and organic amine modifier are added to the modified wax liquid, the temperature is raised to 120~130℃, and the mixture is continuously stirred to achieve uniform compounding and synergistic modification of the wax matrix and surfactant. Further, the stirring speed is 200-300 r / min, and the stirring is continued for 60~80 min.

[0046] In some embodiments of this implementation, the temperature is lowered to 60-70°C before adding polyacrylamide and water. Furthermore, the stirring speed is 200-300 rpm. Stirring is continued for 40-50 minutes.

[0047] In some embodiments of this implementation, the specific preparation steps of the homogenization molding process are as follows: the mixed system is passed into a high-pressure homogenizer for homogenization, and then granulation is carried out by dual cooling of air cooling and water cooling. Finally, the particle size is screened to obtain the finished product of the heavy-duty adaptable low-carbon composite warm mixing agent.

[0048] Furthermore, the homogenization conditions are: homogenization treatment for 20-30 min under a pressure of 20-30 MPa.

[0049] Furthermore, the cooling rate is 5-10℃ / min.

[0050] Furthermore, uniform particles with a particle size of 20-30 mm, preferably 25 mm, are selected.

[0051] Furthermore, in the air-cooled section: the cooling medium is clean air at room temperature, with an inlet air temperature of 15~30℃ and an average wind speed of 2~5 m / s in the cross section of the tower; at the air-cooled outlet, the surface temperature of the particles drops to 70~80℃, forming a complete solidified shell, while the interior remains in a semi-molten state.

[0052] Furthermore, in the water-cooled section: the cooling medium is circulating cooling water with a temperature of 10~25℃ and a water flow velocity of 0.3~0.8m / s in the tank, using a counter-current contact method; at the water-cooled outlet, the overall temperature of the particles drops to 30~40℃, and the inside is completely solidified with no adhesion on the surface.

[0053] This invention employs a step-by-step preparation process of "melt mixing - compound modification - system stabilization - high-pressure homogenization molding" to ensure that each component is fully dispersed and works synergistically, avoids performance degradation caused by component agglomeration, achieves batch-to-batch product performance stability, and is suitable for industrial mass production.

[0054] Specifically, the preparation method of heavy-duty adaptable low-carbon composite warm-mix agent includes the following steps: (1) Melt mixing: Add the Fischer-Tropsch synthetic wax and stearamide in the formula to a closed melting kettle, heat to 100-110℃, and stir at a speed of 200-300r / min until the material is completely melted to form a uniform wax liquid; add the antioxidant in the formula and continue stirring for 25-35min to obtain the modified wax liquid.

[0055] (2) Compound modification: Add the formulated amount of polyoxyethylene polyoxypropylene ether and organic amine modifier to the modified wax liquid, heat to 120-130℃, and stir continuously at a speed of 200-300r / min for 60-80min to achieve uniform compounding and synergistic modification of wax matrix and surfactant; (3) System stabilization: The obtained material is cooled to 60-70℃, and the formula amount of polyacrylamide and deionized water are added. The mixture is stirred continuously at a speed of 200-300r / min for 40-50min to obtain a uniformly dispersed mixed system.

[0056] (4) Homogenization: The mixed system is fed into a high-pressure homogenizer and homogenized for 20-30 min under a pressure of 20-30 MPa. Then, it is granulated by air cooling and water cooling, and the cooling rate is controlled at 5-10℃ / min. Finally, uniform particles with a particle size of 20-30 mm (preferably 25 mm) are screened to obtain the finished product of the heavy-duty adaptable low-carbon composite warm mixing agent.

[0057] The cooling section consists of two parts: The air-cooled section uses clean air at room temperature as the cooling medium, with an inlet temperature of 18-22℃ (preferably 20℃) and an average wind speed of 2-5 m / s (preferably 3 m / s) within the tower cross-section. At the air-cooled outlet, the particle surface temperature drops to 74-76℃ (preferably 75℃), forming a completely solidified outer shell while the interior remains in a semi-molten state. The water-cooled section uses circulating cooling water as the cooling medium, with a water temperature of 18-22℃ (preferably 20℃) and a water flow velocity of 0.4-0.6 m / s (preferably 0.5 m / s) within the tank. A counter-current contact method is used. At the water-cooled outlet, the overall particle temperature drops to 34-36℃ (preferably 35℃), resulting in complete internal solidification and no surface adhesion.

[0058] In one typical embodiment, the present invention provides the application of the above-mentioned heavy-duty adaptable low-carbon composite warm mix agent or the heavy-duty adaptable low-carbon composite warm mix agent prepared by the above preparation method as an asphalt modifier.

[0059] In one typical embodiment, the present invention provides a warm-mix asphalt mixture, comprising the above-mentioned asphalt modifier and asphalt; The asphalt modifier is the above-mentioned heavy-duty adaptable low-carbon composite warm mix agent or the heavy-duty adaptable low-carbon composite warm mix agent prepared by the above preparation method.

[0060] In some embodiments of this implementation, aggregates are also included. The aggregates include coarse aggregates, coarse aggregates, and mineral powder.

[0061] Preferably, the proportion of asphalt mass to the total mass of aggregate is 2-10%, and more preferably 4-5%.

[0062] Preferably, the aggregate comprises, by weight, 45-50 parts of 10-25mm coarse aggregate, 25-30 parts of 5-10mm coarse aggregate, 15-25 parts of 0-5mm fine aggregate, and 4-8 parts of mineral powder.

[0063] The warm mix additive works synchronously with the asphalt during the mixing process, rather than being added to the finished hot mix.

[0064] In some embodiments of this implementation, the method for preparing warm-mix asphalt mixture includes: (1) Preheating of raw materials: Coarse aggregate and fine aggregate are heated to 135~145℃ in the drying drum, and then screened and metered in the hot material silo for later use; limestone mineral powder is stored separately with heat preservation, and the temperature is not lower than 120℃ to ensure dryness and no lumps; asphalt is heated to 130~140℃ and kept warm for later use.

[0065] (2) Dry mixing of aggregates and mineral powder: The metered coarse aggregates, fine aggregates and mineral powder are simultaneously put into the preheated mixing tank and dry mixed together for 5~8 seconds to ensure that the aggregates of each particle size and the mineral powder are fully mixed and uniform to form a continuous gradation skeleton.

[0066] (3) Asphalt-warm mix coating: Hot asphalt heated to 130~140℃ is injected into the mixing tank simultaneously with the metered composite warm mix particles and wet-mixed for 40~50s to make the asphalt and warm mix uniformly coat the aggregate and mineral powder surface; the total mixing time is 45~60s, the discharge temperature of the mixture is controlled at 130~140℃, and it is transported to the construction site for paving and compaction by insulated transport vehicle.

[0067] In some embodiments of this implementation, the dosage of the asphalt modifier is 1.5%-4.0% of the asphalt mass, preferably 2.0%-3.0%, and more preferably 2.5%.

[0068] In some embodiments of this implementation, during the asphalt mixture mixing process, hot asphalt is added to the mixing pot simultaneously, without the need to adjust the existing mixing equipment and construction process. The mixing temperature is reduced by 25-35°C compared to hot-mix asphalt mixture, and the compaction temperature is reduced by 20-30°C compared to hot-mix asphalt mixture.

[0069] In this invention, unless otherwise specified, all other test materials and instruments are conventional test materials in the field and can be purchased through commercial channels.

[0070] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.

[0071] Example 1 The composite warm mix agent, by mass fraction, includes the following components: 45 parts Fischer-Tropsch synthetic wax, 20 parts polyoxyethylene polyoxypropylene ether, 10 parts polyacrylamide, 8 parts stearamide, 7 parts antioxidant, 5 parts organic amine modifier, and 5 parts water.

[0072] Preparation process design: The step-by-step preparation process of "melt mixing - compound modification - system stabilization - high pressure homogenization" is adopted to ensure that each component is fully dispersed and works synergistically, avoids performance degradation caused by component agglomeration, achieves batch-to-batch product performance stability, and is suitable for industrial mass production.

[0073] (1) Melt mixing: Add the Fischer-Tropsch synthetic wax and stearamide in the formula to a closed melting vessel, heat to 100°C, and stir at 250 r / min until the material is completely melted to form a uniform wax liquid; add the antioxidant in the formula and continue stirring for 30 min to obtain the modified wax liquid.

[0074] (2) Compound modification: Add the formulated amount of polyoxyethylene polyoxypropylene ether and organic amine modifier to the modified wax liquid, heat to 125℃, and stir continuously at a speed of 250r / min for 70min to achieve uniform compounding and synergistic modification of wax matrix and surfactant; (3) System stabilization: The obtained material is cooled to 65°C, and the formula amount of polyacrylamide and deionized water are added. The mixture is stirred continuously at a speed of 250 r / min for 45 min to obtain a uniformly dispersed mixed system.

[0075] (4) Homogenization: The mixed system is fed into a high-pressure homogenizer and homogenized for 25 minutes at 25 MPa. Then, it is granulated by dual cooling of air and water, with the cooling rate controlled at 8℃ / min. Finally, uniform particles with a particle size of 25 mm are screened to obtain the finished heavy-duty adaptable low-carbon composite warm-mix agent. Among them, the air-cooling section: the cooling medium is clean air at room temperature, the inlet air temperature is 20℃, and the average wind speed in the cross section of the tower is 3 m / s; the surface temperature of the particles at the air-cooling outlet drops to 75℃, forming a complete solidified shell, while the inside remains in a semi-molten state. The water-cooling section: the cooling medium is circulating cooling water, the water temperature is 20℃, the water flow velocity in the tank is 0.5 m / s, and a counter-current contact method is adopted; the overall temperature of the particles at the water-cooling outlet drops to 35℃, the inside is completely solidified, and the surface is not adhered.

[0076] Example 2 This embodiment uses the AC-20C dense-graded asphalt mixture system, commonly used in the lower layers of heavy-duty roads, consisting of coarse aggregate, fine aggregate, limestone powder, No. 70 Grade A road petroleum asphalt, and warm mix additive. 1. Specific proportions of each component (based on a total aggregate mass of 100 parts) 10~25mm coarse aggregate: 48 parts; 5~10mm coarse aggregate: 27 parts; 0~5mm fine aggregate: 20 parts; Mineral powder: 5 parts; Grade A road petroleum asphalt No. 70: 4.5 parts (corresponding to an asphalt-aggregate ratio of 4.5%, i.e., the proportion of asphalt mass to total aggregate mass); The composite warm mix admixture prepared in Example 1: 0.11 parts (admixture amount is 2.5% of the mass of asphalt); 2. Aggregate and mineral powder particle size and technical parameter limits (the synthetic gradation meets the AC-20C gradation range requirements in the "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40-2017)). (1) Coarse aggregate Particle size classification: 10~25mm, 5~10mm; Core performance: Crushing value ≤26%, Los Angeles abrasion loss ≤28%, needle-like and flaky particle content ≤15%, adhesion to asphalt ≥5, water absorption ≤2.0%, apparent relative density ≥2.60 t / m³ 3 .

[0077] (2) Fine aggregate Particle size range: 0~5mm; Core performance: Sand equivalent ≥65%, angularity (flow time) ≥30s, particle content smaller than 0.075mm ≤12%, apparent relative density ≥2.50 t / m³ 3 .

[0078] (3) Mineral powder Particle size parameters: 100% passing rate through 0.6mm sieve, ≥75% passing rate through 0.075mm sieve; Core performance: hydrophilicity coefficient ≤1.0, water content ≤1%, apparent relative density ≥2.50 t / m³ 3 The appearance is free of granules and lumps.

[0079] 3. Mixing and preparation process of the mixture (mineral powder and aggregate are added simultaneously) Raw material preheating: Coarse and fine aggregates are heated to 140°C in a drying drum, then screened and metered in a hot material silo for later use; limestone powder is stored separately with insulation at a temperature not lower than 120°C to ensure it is dry and free of lumps; asphalt is heated to 135°C and kept warm for later use.

[0080] Aggregate-mineral powder dry mixing: The metered coarse aggregate, fine aggregate, and mineral powder are simultaneously put into the preheated mixing tank and dry mixed together for 8 seconds to ensure that the aggregates of each particle size and the mineral powder are fully and evenly mixed to form a continuous gradation skeleton.

[0081] Asphalt-warm mix coating: Hot asphalt heated to 135℃ is simultaneously injected into the mixing tank along with metered composite warm mix granules, and wet-mixed for 42 seconds to ensure that the asphalt and warm mix are evenly coated on the surface of the aggregate and mineral powder; the total mixing time is 50 seconds, and the discharge temperature of the mixture is controlled at 135℃. The mixture is then transported to the construction site by insulated transport vehicle for paving and compaction.

[0082] Table 1. Basic Performance Tests of Warm Mixing Agent

[0083] Viscosity reduction rate (%) = η0 η1 / η0 × 100%. Where: η0: Apparent rotational viscosity of blank reference asphalt (without warm mix additives) at 135℃, unit: Pa s; η1: Apparent rotational viscosity of asphalt sample with a specified proportion of warm mix additive at 135℃, unit: Pa s.

[0084] Among them, the blank No. 70 Class A road petroleum asphalt (η0): 0.47 Pa s. Asphalt mixed with 2.5% composite warm mix admixture (η1): 0.257 Pa s.

[0085] Table 2. Road Performance Tests of Asphalt Mixtures

[0086] Note: The “composite warm mix agent” in Table 2 refers to the warm mix asphalt mixture with composite warm mix agent in Example 2, and the “hot mix mixture” refers to the “ordinary asphalt mixture” without composite warm mix agent in Example 2 (the rest is the same as in Example 2).

[0087] Comparative Example 1 Unlike Example 1, a different type of wax was used. Specifically, it includes: Plant waxes: soybean wax, palm wax; Animal wax: beeswax; Pyrolysis wax: Polyethylene pyrolysis wax; Petroleum waxes: 58# fully refined paraffin wax, 70# microcrystalline wax; Synthetic waxes: Low-density polyethylene wax (LDPE wax), Fischer-Tropsch synthetic wax.

[0088] Keeping all other components and preparation processes completely consistent, only the wax matrix was replaced. The basic properties of the warm mix additive and the corresponding asphalt mixture road performance were tested, and the results are shown in Table 3.

[0089] Table 3. Performance Comparison of Different Waxes

[0090] Screening of different waxes revealed that Fischer-Tropsch synthetic wax has a molecular structure of high-purity straight-chain alkanes, without branches or unsaturated bonds, exhibits excellent compatibility with asphalt, does not separate during high-temperature storage, and its melting point range perfectly matches the mixing temperature of asphalt mixtures (130-140℃). It can quickly melt to form a continuous lubricating film, has low penetration and high hardness, and will not reduce the high-temperature rutting resistance of asphalt mixtures. Other waxes cannot simultaneously meet the triple requirements of "highly efficient viscosity reduction, high-temperature stability, and low-temperature non-caking".

[0091] Comparative Example 2 Unlike Example 1, a different compatibility additive was used. All other components and preparation processes remained identical; only the compatibility additive was replaced (at a dosage of 8%). The test results are shown in Table 4.

[0092] Table 4. Performance Comparison of Different Compatible Additives

[0093] A comparison of the performance of different compatibility additives reveals that stearamide does not have the same effect as other amide additives. Stearamide has a moderate molecular weight, allowing it to simultaneously form intermolecular forces with the alkane chains of Fischer-Tropsch waxes and the polar groups of polyethers, acting as a "bridge." While diamide additives such as EBS can also improve compatibility, their large molecular weight and high melting point increase preparation energy consumption and slightly reduce viscosity reduction efficiency. Unsaturated amides such as oleamide are prone to oxidation and precipitation, severely affecting the storage stability of warm-mix additives.

[0094] Comparative Example 3 Unlike Example 1, a different viscosity-reducing component was used. All other components and preparation processes remained identical, only the viscosity-reducing component was replaced (at a dosage of 20%). Details are shown in Table 5.

[0095] Table 5 Comparison of the performance of different viscosity-reducing components

[0096] A comparison of the performance of different viscosity-reducing components shows that: There is a significant difference in performance between polyoxyethylene polyoxypropylene ether and allyl alcohol-based polyoxyethylene-propylene ether. Polyoxyethylene polyoxypropylene ether is a saturated block polyether with no active double bonds, exhibiting good high-temperature stability and a viscosity-reducing effect lasting up to 12 hours, meeting the requirements for long-distance transportation and construction. Allyl alcohol-based polyether, containing unsaturated double bonds, is prone to oxidative cross-linking at mixing temperatures above 130°C, leading to a rapid decline in its viscosity-reducing effect, with a viscosity-reducing effect lasting only 4 hours.

[0097] Furthermore, when allyl alcohol polyether (allyl alcohol polyoxyethylene-propylene ether) replaces PEO-PPO (polyoxyethylene polyoxypropylene ether) in Example 1, the dynamic stability at 60°C is 4050 cycles / mm, and the freeze-thaw splitting strength ratio is 89.2%.

[0098] Comparative Example 4 Unlike Example 1, this one lacks the polyacrylamide component, but the remaining components and preparation process are completely identical.

[0099] Comparative Example 5 Unlike Example 1, the stearamide component is missing, but the other components and preparation process are completely the same.

[0100] Table 6

[0101] Fischer-Tropsch synthetic wax provides basic lubrication and high-temperature stability, while polyoxyethylene polyoxypropylene ether provides the core viscosity reduction effect. Together, they achieve "no viscosity reduction at high temperatures and no clumping at low temperatures".

[0102] Stearamide improves the compatibility between wax and polyether, while polyacrylamide enhances the stability of the system and the water stability of the mixture. Together, they improve the problem of traditional warm mix agents that "reduce viscosity and degrade road performance".

[0103] Antioxidants and organic amine modifiers further enhance the storage stability and environmental friendliness of the system.

[0104] Comparative Example 6 Unlike Example 1, a commercially available warm-mixing agent was used for performance comparison. Specific results are shown in Tables 7 and 8.

[0105] Organic wax type, Sasobit, model number Sasobit H8.

[0106] Surfactant type, Evotherm, model number Evotherm DAT.

[0107] Foamed asphalt type, WAM-Foam, model name Shell WAM-Foam.

[0108] Table 7

[0109] Table 8

[0110] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A heavy load adapted low carbon composite warm-mixing agent, characterized in that, Includes the following components: 40-50 parts of Fischer-Tropsch synthetic wax, 15-25 parts of polyoxyethylene polyoxypropylene ether, 8-12 parts of polyacrylamide, 6-10 parts of stearamide, 5-8 parts of antioxidant, 3-7 parts of organic amine modifier, and 3-7 parts of water.

2. The heavy duty adaptive low carbon compound warm mix agent according to claim 1, wherein, Heavy-duty adaptable low-carbon composite warm mix agent, comprising the following components: 43-47 parts of Fischer-Tropsch synthetic wax, 18-22 parts of polyoxyethylene polyoxypropylene ether, 9-11 parts of polyacrylamide, 7-9 parts of stearamide, 6-7 parts of antioxidant, 4-6 parts of organic amine modifier, and 4-6 parts of water.

3. The heavy-duty adaptable low-carbon composite warm-mix agent according to claim 1 or 2, characterized in that, Fischer-Tropsch synthetic wax is a straight-chain saturated alkane Fischer-Tropsch wax with a melting point of 80~110℃, a penetration of ≤1.0mm at 25℃, and a dropping point of ≥100℃. Preferably, the polyoxyethylene polyoxypropylene ether is a block polyether with an HLB value of 8-12 and a number average molecular weight of 1000-3000; Preferably, the polyacrylamide is a nonionic polyacrylamide, and preferably, the molecular weight is 3 million to 8 million. Preferably, the organic amine modifier is at least one of diethanolamine, triethanolamine, and ethylenediamine, with diethanolamine being the most preferred; Preferably, the antioxidant is a hindered phenolic antioxidant, and more preferably at least one of antioxidant 1010 and antioxidant 1076.

4. A method for preparing a heavy-duty adaptable low-carbon composite warm-mix agent according to any one of claims 1 to 3, characterized in that, Includes the following steps: Modified wax liquid is obtained by melt blending Fischer-Tropsch synthetic wax, stearamide, and antioxidant; Polyoxyethylene polyoxypropylene ether and organic amine modifiers were added to the modified wax liquid for compound modification; After cooling the compounded and modified material, add polyacrylamide and water, and stir to obtain a mixed system; The mixture is homogenized to obtain the final product.

5. The preparation method according to claim 4, characterized in that, The specific preparation steps of the modified wax liquid are as follows: Fischer-Tropsch synthetic wax and stearamide are added to a closed reactor, heated to the melting point, and then an antioxidant is added and stirred to obtain the modified wax liquid; more preferably, the temperature is raised to 100~110℃; Alternatively, the specific preparation steps for compound modification are as follows: add polyoxyethylene polyoxypropylene ether and organic amine regulator to the modified wax liquid, heat to 120~130℃, and stir continuously for 60~80min.

6. The preparation method according to claim 4, characterized in that, Cool down to 60-70℃, then add polyacrylamide and water, and stir continuously for 40-50 minutes.

7. The preparation method according to claim 4, characterized in that, The specific preparation steps of the homogenization molding process are as follows: the mixed system is passed into a high-pressure homogenizer for homogenization, and then granulation is carried out by dual cooling of air cooling and water cooling. Finally, the particle size is screened to obtain the finished product of the heavy-duty adaptable low-carbon composite warm mixing agent. Preferably, the homogenization conditions are: homogenization treatment at 20-30 MPa pressure for 20-30 min; Preferably, the cooling rate is 5-10℃ / min.

8. The application of a heavy-duty adaptable low-carbon composite warm mix agent according to any one of claims 1 to 3 or a heavy-duty adaptable low-carbon composite warm mix agent prepared by the preparation method according to any one of claims 4 to 7 as an asphalt modifier.

9. A warm-mix asphalt mixture, characterized in that, Includes asphalt modifiers and asphalt; The asphalt modifier is the heavy-duty adaptable low-carbon composite warm mix agent according to any one of claims 1 to 3 or the heavy-duty adaptable low-carbon composite warm mix agent prepared by the preparation method according to any one of claims 4 to 7.

10. The asphalt mixture according to claim 9, characterized in that the asphalt... The modifier dosage is 1.5%-4.0% of the asphalt mass, preferably 2.0%-3.0%; Preferably, during the mixing process of warm-mix asphalt, the asphalt modifier is added to the mixing pot simultaneously with the hot asphalt.