Moisture-triggered viscosity-toughness-regulated drainage pavement asphalt binder and preparation method thereof
By using moisture-triggered polyurethane prepolymers and silane-terminated polyurethane prepolymers to form an elastic-toughness reinforcing network and interface anchoring structure in drainage asphalt pavement, the aging and construction problems of drainage asphalt pavement during long-term service are solved. This achieves easy mixing and compaction during the construction stage and adhesive-toughness enhancement after molding, thereby improving the pavement's resistance to scattering and water damage.
Patent Information
- Application Number
- CN202611573798.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-24
AI Technical Summary
Existing drainage asphalt pavements are prone to accelerated aging of binder, decreased toughness of membrane layer, reduced adhesion at the asphalt-aggregate interface, aggregate shedding, loosening and scattering under long-term service conditions. In addition, there are problems such as difficulty in mixing, uneven coating and high paving resistance caused by excessive viscosity during construction.
By employing the synergistic effect of moisture-triggered polyurethane prepolymer, silane-terminated polyurethane prepolymer, interfacial anchoring agent, reaction-regulating catalyst, nanosheet barrier material, and antioxidant stabilizing components, a viscosity-toughness regulation system is constructed that provides suitable viscosity during construction, enhanced viscosity and toughness after molding, and resistance to scattering after aging. The system forms an elastic-toughness-enhanced network and an interfacial anchoring structure through a moisture-triggered curing reaction.
It achieves easy mixing and compaction during the construction phase, enhanced adhesion and toughness after molding, and maintained anti-scattering performance after aging, thus improving the construction adaptability, anti-scattering ability, water damage resistance and long-term functional retention of drainage asphalt pavement.
Smart Images

Figure CN123152305A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of road engineering materials technology, specifically relating to a moisture-triggered, viscosity-regulating asphalt binder for drainage pavement and its preparation method. Background Technology
[0002] Drainage asphalt pavement typically employs a large-void, open-graded structure, offering excellent drainage in rainy weather, reduced water mist, reduced noise, improved skid resistance, and enhanced driving safety. It is suitable for highways, urban expressways, bridge deck paving, tunnel entrances and exits, long longitudinal slopes, and road sections with high requirements for driving safety in rainy weather.
[0003] However, drainage asphalt mixtures have high porosity, well-developed interconnected pores, few aggregate skeleton contact points, and a large exposed area of the binder film. Under long-term traffic loads, water intrusion, thermo-oxidative aging, ultraviolet radiation, temperature cycling, and abrasion, they are prone to problems such as accelerated aging of the binder, decreased toughness of the film, weakened adhesion at the asphalt-aggregate interface, aggregate shedding, loosening, scattering, and degradation of drainage, noise reduction, and anti-skid functions.
[0004] Existing drainage asphalt pavement binders mainly include ordinary modified asphalt, high-viscosity modified asphalt, rubber asphalt and their composite modification systems. Their basic technical approach is usually to improve the high-temperature stability, elastic recovery performance and aggregate adhesion of the binder by adding SBS, rubber powder, tackifying resin, anti-stripping agent or antioxidant components.
[0005] However, under the long-term service conditions of drainage asphalt pavement, the existing technology still has the following shortcomings.
[0006] (a) Ordinary SBS modified asphalt has insufficient resistance to scattering and durability. Ordinary SBS modified asphalt has a certain elastic recovery ability and high temperature stability, but drainage asphalt mixture has a high porosity structure, and the aggregates are mostly in point contact or local surface contact, which requires high adhesion strength, film toughness, cohesive strength and anti-aging retention ability of the binder.
[0007] Under long-term water intrusion, ultraviolet radiation and thermo-oxidative aging, the binder film of ordinary SBS modified asphalt is prone to hardening and embrittlement, resulting in the attenuation of asphalt-aggregate interface adhesion. This makes it difficult to effectively suppress particle shedding, loosening and scattering after traffic is opened, especially in heavy traffic, long longitudinal slopes, bridge deck drainage pavement and high humidity environments.
[0008] (II) Insufficient adaptability of traditional high-viscosity modified asphalt to construction Traditional high-viscosity modified asphalt typically increases its dynamic viscosity at 60°C and binder adhesion by adding polymers, tackifying resins, or rubber powder. While this method can reduce early dispersion losses in drainage asphalt mixtures to some extent, excessively high binder viscosity can lead to problems such as pumping difficulties, increased mixing energy consumption, uneven aggregate adhesion, increased paving resistance, narrowed compaction window, and fluctuations in construction quality.
[0009] Especially in drainage asphalt mixtures, if the mixing or compaction quality is insufficient, it can easily lead to abnormal local void ratio, unstable interconnected void structure, insufficient skeleton interlocking, and increased risk of later scattering, which in turn affects the long-term drainage, skid resistance, and anti-scattering performance of the pavement.
[0010] (III) The compatibility and single mechanism of action of ordinary polyurethane-asphalt composite systems Existing polyurethane-asphalt composite materials primarily focus on improving the elasticity, flexibility, crack repair capabilities of asphalt, or the compatibility between polyurethane and asphalt. These technologies typically enhance the compatibility of the polyurethane-asphalt system and the overall flexibility of the composite material through methods such as modification of lipophilic groups, adjustment with compatibilizers, or elastomer compounding.
[0011] However, existing conventional polyurethane-asphalt composite systems often fail to fully leverage the structural characteristics of drainage asphalt mixtures, such as high porosity, well-developed interconnected pores, easy contact with environmental moisture, and a large exposed area of the binder film. They also lack a comprehensive control mechanism encompassing controllable viscosity during construction, moisture-triggered curing after molding, and resistance to scattering during service life. Their technical effects are primarily manifested in general elasticity enhancement or compatibility improvement, making it difficult to address the targeted control of particle shedding, loosening, scattering, and functional degradation issues inherent in the high-porosity structure of drainage asphalt pavements.
[0012] (iv) Existing tack coat materials and drainage asphalt binders have different target applications. Existing polyurethane-modified emulsified asphalt or polyurethane composite tack coat materials are mainly used for interlayer bonding between different structural layers. Their application occurs at the interlayer interface between the upper and lower layers, and the key technical aspects typically include interlayer shear strength, pull-out strength, hydrolysis resistance, and enhanced interfacial bonding. However, they cannot solve the problems of scattering and functional degradation of the internal binder film layer in drainage asphalt mixtures during long-term service.
[0013] (v) Existing anti-aging and anti-water damage measures lack a synergistic mechanism of "post-curing - interface anchoring - layer barrier". Existing drainage asphalt binders typically improve durability by adding antioxidants, UV absorbers, and anti-stripping agents. However, their effects are mostly limited to single physical improvements, chemical stabilization, or interface enhancement. There is a lack of technical approaches that utilize the moisture environment in the interconnected pores of drainage asphalt to induce a post-curing reaction in the binder after molding.
[0014] Therefore, there is an urgent need to develop a special asphalt binder for drainage pavements that can balance controllable construction viscosity, enhanced toughness after molding, interfacial anchoring, water damage resistance, aging resistance, and anti-scattering properties. Summary of the Invention
[0015] The purpose of this invention is to provide a moisture-triggered viscosity-toughness regulated drainage pavement asphalt binder and its preparation method. Through the synergistic effect of moisture-triggered polyurethane prepolymer, silane-terminated polyurethane prepolymer, interface anchoring agent, reaction-regulating catalyst, nanosheet barrier material, construction viscosity regulator, and antioxidant stabilizing component, the binder maintains a suitable flow viscosity during the construction stage. After the drainage asphalt mixture is formed, the curing reaction is triggered by the ambient moisture in the interconnected pores, forming an elastic and tough reinforcing network and interface anchoring structure inside the binder film and at the asphalt-aggregate interface. This achieves the technical effects of easy mixing and compaction during construction, enhanced viscosity and toughness after forming, and maintenance of anti-scattering performance after aging.
[0016] This invention does not simply aim to increase the initial viscosity of the binder, but rather to construct a viscosity-toughness time-series control system that combines controllable construction viscosity, moisture-triggered curing, interface anchoring enhancement, and aging barrier maintenance throughout the entire process of drainage asphalt pavement from construction to forming to service.
[0017] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a moisture-triggered, viscosity-regulating asphalt binder for drainage pavements, comprising the following components by weight: 100 parts asphalt base material; 3-15 parts of moisture-triggered polyurethane prepolymer; 1-8 parts of silane-terminated polyurethane prepolymer; 0.2~2.0 parts of interface anchoring agent; 0.05~0.8 parts of reaction-regulating catalyst; 0.2~1.5 parts of hydrophobic anti-stripping component; 0.5~3.0 parts of nanosheet barrier material; 1-6 parts of construction viscosity modifier; 0.2 to 1.5 parts of antioxidant stabilizing component.
[0018] Furthermore, the asphalt base material is No. 70 road petroleum asphalt, No. 90 road petroleum asphalt, SBS modified asphalt, high viscosity modified asphalt, or a mixture thereof.
[0019] Furthermore, the moisture-triggered polyurethane prepolymer is one or a combination of isocyanate-terminated polyurethane prepolymer and polyurethane prepolymer containing moisture-reactive end groups; its NCO mass fraction is preferably 1.5% to 6.0%. This component is used to undergo a post-curing reaction with ambient moisture after the drainage asphalt mixture is formed, thereby improving the cohesive strength, elastic recovery ability, and bonding toughness of the binder film.
[0020] The moisture-triggered polyurethane prepolymer is preferably an isocyanate-terminated polyurethane prepolymer. Its preparation method is as follows: 100 parts by weight of polypropylene glycol (PPG-2000) with a number-average molecular weight of approximately 2000 are dehydrated for 1 hour at 105-115°C under a vacuum of not less than 0.09 MPa. The temperature is then lowered to 75-80°C and protected with dry nitrogen gas. 27-29 parts by weight of liquefied diphenylmethane diisocyanate (MDI) are slowly added, and the reaction is carried out at 80±2°C for approximately 3 hours. During the reaction, the NCO mass fraction of the system is measured. The reaction is stopped when the NCO mass fraction reaches 3.7%-4.3%, yielding the isocyanate-terminated polyurethane prepolymer. The obtained prepolymer is sealed and stored in a moisture-proof environment for later use.
[0021] Furthermore, the silane-terminated polyurethane prepolymer is one or a combination of polyurethane prepolymers containing trimethoxysilyl, triethoxysilyl, methyldimethoxysilyl, and methyldiethoxysilyl. This component undergoes a hydrolysis-condensation reaction under moisture, forming a post-cured reinforcing network within the binder film and at the asphalt-aggregate interface.
[0022] The silane-terminated polyurethane prepolymer is preferably a triethoxysilane-terminated polyurethane prepolymer. An NCO-terminated polyurethane prepolymer is first prepared using PPG-3000 and IPDI, and then end-capped using KH-550 (3-aminopropyltriethoxysilane).
[0023] The specific preparation method is as follows: 100 parts by mass of polypropylene glycol (PPG-3000) with a number-average molecular weight of approximately 3000 are dehydrated under vacuum at 110-120℃ for 30-60 minutes. After cooling, 12-13 parts of isophorone diisocyanate (IPDI) and 0.005-0.01 parts of dibutyltin dilaurate are added under nitrogen protection. The mixture is reacted at 95-105℃ for approximately 3 hours to obtain an isocyanate-terminated polyurethane prepolymer with an NCO mass fraction of approximately 1.5%-1.8%. Subsequently, the temperature is lowered to 30-40℃, and 9-10 parts of 3-aminopropyltriethoxysilane (KH-550 / APTES) are added. After stirring evenly, the temperature is raised to 55-65℃ and reacted for approximately 1 hour until the free NCO is basically completely reacted, yielding a triethoxysilane-terminated polyurethane prepolymer. The resulting product should be stored in a sealed, moisture-proof container.
[0024] Furthermore, the interface anchoring agent is one or more of the following: aminosilane coupling agent, epoxysilane coupling agent, mercaptosilane coupling agent, phosphate ester interface enhancer, catechol interface enhancer, or dopamine interface enhancer. This component can enhance the chemical or physical interface interaction between the binder and aggregates such as basalt, diabase, limestone, and steel slag.
[0025] The preferred aminosilane coupling agent is 3-aminopropyltriethoxysilane (KH-550); the preferred epoxysilane coupling agent is γ-glycidoxypropyltrimethoxysilane (KH-560); the preferred mercaptosilane coupling agent is γ-mercaptopropyltrimethoxysilane (KH-590); the preferred phosphate ester interface reinforcing agent is C12~C14 fatty alcohol polyoxyethylene ether phosphate (AEO-3P); the preferred catechol interface reinforcing agent is catechol (1,2-benzenediol); and the preferred dopamine interface reinforcing agent is 3,4-dihydroxyphenylethylamine.
[0026] Furthermore, the reaction-regulating catalyst is an organobismuth catalyst, an organozinc catalyst, a blocked amine catalyst, a microencapsulated catalyst, or a mixture thereof. This component is used to regulate the rate of the moisture-triggered curing reaction, preventing premature curing during the construction stage and ensuring that the post-curing reaction proceeds gradually after molding.
[0027] The preferred organobismuth catalyst is bismuth neodecanoate; the preferred organozinc catalyst is zinc neodecanoate.
[0028] Furthermore, the hydrophobic anti-stripping component is one or more of amine anti-stripping agents, non-amine anti-stripping agents, organosilicon hydrophobic agents, and phosphate ester anti-stripping agents. This component is used to enhance the cementitious material's resistance to water stripping and reduce the destructive effect of moisture on the asphalt-aggregate interface.
[0029] The preferred amine anti-stripping agent is octadecylamine or long-chain fatty amine anti-stripping agent; the preferred non-amine anti-stripping agent is fatty alcohol polyoxyethylene ether phosphate anti-stripping agent.
[0030] Furthermore, the nanosheet barrier material is organically modified montmorillonite, layered silicate, hydrotalcite, graphene oxide, sheet-like nano-silica, or a composite thereof. This component is used to form tortuous diffusion paths in the binder film layer, improving the binder film layer's ability to block the intrusion of water, oxygen, and ultraviolet factors.
[0031] Furthermore, the construction viscosity regulator is a naphthenic oil, aromatic oil, bio-based compatibilizer, low-viscosity polyether, reactive diluent or a compound thereof, used to reduce the viscosity of the system during the construction stage and improve its adaptability to mixing, coating, paving and compaction.
[0032] Furthermore, the antioxidant stabilizing component is one or more of hindered phenolic antioxidants, phosphite antioxidants, hindered amine light stabilizers, and ultraviolet absorbers, used to delay the thermo-oxidative aging and ultraviolet aging of the binder and improve its ability to retain viscous toughness after aging.
[0033] The preferred hindered phenolic antioxidant is antioxidant 1010; the preferred phosphite antioxidant is antioxidant 168; the preferred hindered amine light stabilizer is light stabilizer 770; and the preferred ultraviolet absorber is UV-326.
[0034] Preferably, the moisture-triggered viscosity-regulating asphalt binder for drainage pavement comprises, by weight: 100 parts of petroleum asphalt or SBS modified asphalt for Route 70. 5-10 parts of isocyanate-terminated polyurethane prepolymer; 2-5 parts of silane-terminated polyurethane prepolymer; 0.4-1.2 parts of a compound of aminosilane coupling agent and phosphate ester interface enhancer; 0.1–0.4 parts of an organobismuth reaction control catalyst; 0.3~0.8 parts of hydrophobic anti-stripping component; 1.0~2.0 parts of organically modified montmorillonite or hydrotalcite; 2-4 parts of bio-based compatibilizing oil or naphthenic oil; 0.4 to 1.0 parts of the compound of hindered phenolic antioxidant and hindered amine light stabilizer.
[0035] This preferred solution reduces the viscosity of the binder during the construction stage by using a construction viscosity modifier, constructs a post-curing elastic-tough network using moisture-triggered polyurethane prepolymer and silane-terminated polyurethane prepolymer, enhances the adhesion between the binder and the aggregate surface using an interface anchoring agent, delays the intrusion of water, oxygen and ultraviolet rays into the binder film using a nanosheet barrier material, and improves the retention rate of viscosity and toughness performance after aging using antioxidant stabilizing components, thereby achieving synergistic regulation of viscosity and toughness during the construction, molding and service stages.
[0036] This invention also provides a method for preparing any of the above-described moisture-triggered, viscosity-regulating asphalt binders for drainage pavements, the process flow of which is as follows: Figure 1 As shown, this process can be represented as follows: preheating of asphalt base material → pre-dispersion of nanosheet barrier material → addition of moisture-triggered polyurethane prepolymer → addition of silane-terminated polyurethane prepolymer and interface anchoring agent → addition of reaction-regulating catalyst and hydrophobic anti-stripping component → addition of antioxidant stabilizing component → stabilization development → finished binder.
[0037] Specifically, the following steps are included: Step 1: Preheating of asphalt base material Heat the asphalt base material to 150~170℃ and stir it at a low speed of 300~800r / min for 20~40min to fully dehydrate it and form a uniform flow state.
[0038] Step 2: Pre-dispersion of nanosheet barrier materials The nanosheet barrier material is premixed with all or part of the construction viscosity modifier to form a predispersed slurry. The predispersed slurry is added to the preheated asphalt base material, or the nanosheet barrier material is directly added to the preheated asphalt base material. The mixture is sheared at 150~170℃ and 2000~4000r / min for 20~50min to make the nanosheet barrier material uniformly dispersed in the asphalt phase. If the construction viscosity modifier is not added or is not fully added to the system during the above dispersion process, the construction viscosity modifier or the remaining construction viscosity modifier shall be added to the system separately.
[0039] Step 3: Add moisture-triggered polyurethane prepolymer The system temperature is controlled at 145~165℃. Moisture-triggered polyurethane prepolymer is slowly added and sheared at 1000~3000r / min for 20~40min to uniformly disperse the polyurethane prepolymer in the asphalt system and form a preliminary viscosity-toughness regulation system.
[0040] Step 4: Add silane-terminated polyurethane prepolymer and interface anchoring agent Adjust the system temperature to 140~160℃, add silane-terminated polyurethane prepolymer and interface anchoring agent, and stir at 800~2500r / min for 15~40min to ensure uniform dispersion of silane-terminated polyurethane prepolymer and interface anchoring agent, and to maintain the reactivity of interface anchoring components in the binder system.
[0041] Step 5: Add reaction control catalyst and hydrophobic anti-stripping component The system temperature was controlled at 135~155℃, and the reaction regulating catalyst and hydrophobic anti-stripping component were added, and stirred for 10~30 min. The reaction regulating catalyst is used to regulate the subsequent moisture-triggered curing reaction rate, and the hydrophobic anti-stripping component is used to enhance the binder's resistance to water peeling.
[0042] Step Six: Addition of Antioxidant Stabilizing Components and Stabilization of Development The system temperature was lowered to 130~150℃, antioxidant stabilizing components were added, and the mixture was stirred at low speed for 20~60 minutes to allow the system to stabilize and develop, thus obtaining a moisture-triggered, viscosity- and toughness-regulated drainage pavement asphalt binder.
[0043] How to use The prepared binder can be used in OGFC open-graded anti-skid wear course, PA drainage asphalt, and other high-porosity asphalt mixtures with a porosity of 18% to 25%. After the mixture is mixed, paved, and compacted, ambient moisture in the interconnected pores of the drainage asphalt mixture gradually enters the surface of the binder film, triggering the hydrolysis and condensation of silane-terminated components and the post-curing reaction of the polyurethane prepolymer. This causes the binder film to gradually transform from a workable viscoelastic state during the construction stage to a bond-reinforced, elastic-toughened, and interfacial anchoring-reinforced state during the service stage.
[0044] The process principle of this invention is as follows: This invention adopts a composite control approach of "construction viscosity control - moisture-triggered curing - interface anchoring enhancement - layer barrier anti-aging".
[0045] During the construction phase, the construction viscosity modifier reduces the high-temperature viscosity of the binder, enabling the binder to uniformly coat the aggregate and improve the adaptability of the drainage asphalt mixture for mixing, paving, and compaction. The reaction control catalyst controls the post-curing reaction rate, preventing the binder from curing prematurely during mixing, transportation, and paving, thus ensuring the construction window.
[0046] After molding, the drainage asphalt mixture has an interconnected porous structure, allowing ambient moisture to penetrate the mixture and contact the binder film layer. Moisture-triggered polyurethane prepolymers and silane-terminated polyurethane prepolymers undergo post-curing reactions under moisture, forming an elastic-toughening network that improves the cohesive strength, elastic recovery, and anti-scattering ability of the binder film layer.
[0047] Interface anchoring agents can chemically or physically interact with hydroxyl groups, metal oxides, calcium and magnesium active sites on the surface of aggregates, and simultaneously form interfacial connections with polar components in the binder, thereby improving the adhesion strength of the asphalt-aggregate interface and reducing interfacial delamination caused by water intrusion.
[0048] Nanosheet barrier materials form tortuous diffusion paths in the binder film, delaying the intrusion of water, oxygen and ultraviolet factors into the binder, reducing the aging and embrittlement rate, and improving the long-term resistance to scattering.
[0049] That is, Figure 2 As shown, the binder of this invention exhibits a workable viscoelastic system with suitable viscosity during the construction stage. After the drainage asphalt mixture is formed, ambient moisture enters the binder film layer through interconnected pores, triggering the hydrolysis and condensation of silane-terminated components and the post-curing reaction of polyurethane prepolymer, forming an elastic and toughened network. The interface anchoring agent acts on the aggregate surface to improve the adhesion strength of the asphalt-aggregate interface. The nanosheet barrier material delays the intrusion of water, oxygen, and ultraviolet rays, thereby improving the resistance to scattering, water damage, and the ability to retain functions after aging.
[0050] Therefore, the present invention does not simply increase the initial viscosity of the binder, but rather enables the binder to exhibit different performance characteristics at different stages, namely, suitable low viscosity during construction, enhanced adhesion and toughness after molding, and maintained toughness during service.
[0051] By adopting the above technical solution, the beneficial effects of the present invention are as follows: (a) Improve construction adaptability This invention uses a construction viscosity regulator and a reaction-controlled reaction system to maintain the appropriate viscosity of the binder during the mixing, transportation, paving and compaction stages, thus avoiding problems such as mixing difficulties, uneven adhesion, high paving resistance, narrow compaction window and construction quality fluctuations caused by excessively high viscosity of traditional high-viscosity binders.
[0052] (ii) Improve the resistance to scattering after molding This invention utilizes the environmental moisture in the interconnected voids of the drainage asphalt mixture to trigger a post-curing reaction, causing the binder film layer to gradually form an elastic and toughened network after molding. This improves the cohesive strength, aggregate adhesion, and bonding toughness of the binder, and reduces Kentucky scattering losses, Kentucky scattering losses after immersion in water, scattering losses after hygrothermal cycling, and scattering losses after UV aging.
[0053] (III) Improve water damage resistance and interfacial adhesion properties This invention enhances the chemical or physical anchoring of the binder and aggregate surface through the synergistic effect of interface anchoring agent and hydrophobic anti-stripping component, reduces the stripping effect of moisture on the asphalt-aggregate interface, and improves the performance retention rate after water immersion, freeze-thaw splitting and wet heat cycling.
[0054] (iv) Improve the ability to retain viscoelastic properties after aging This invention utilizes the combined action of a post-cured polyurethane elastic-tough network and nanosheet barrier materials to delay the thermo-oxidative aging and UV aging of the binder film, reduce the degree of embrittlement after aging, and improve the ability to maintain elasticity, bond strength, anti-scattering performance, texture depth, and frictional properties after aging.
[0055] (V) Achieving performance synergy between the construction and service phases Traditional high-viscosity binders often present a contradiction between "difficult construction" and "high service durability requirements." This invention addresses this by using stage-responsive viscosity-toughness regulation to maintain suitable fluidity during the construction phase and gradually enhance it under moisture after molding, achieving a synergistic improvement in both construction and service performance.
[0056] (vi) Applicable to functional pavements with high porosity This invention is particularly suitable for drainage asphalt pavements, open-graded anti-skid wear layers, bridge deck drainage pavements, tunnel entrances and exits, long longitudinal slopes, road sections with heavy traffic and high requirements for driving safety in rainy weather, and can improve the long-term service durability and surface function retention of high-porosity functional asphalt pavements. Attached Figure Description
[0057] Figure 1 This is a flowchart illustrating the preparation process of the moisture-triggered, viscosity-regulating asphalt binder for drainage pavement according to the present invention. Figure 2 This is a schematic diagram of the moisture-triggered viscoelastic transformation mechanism of the present invention. Detailed Implementation
[0058] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described below with reference to specific embodiments. These embodiments are merely preferred implementations and are not intended to limit the scope of protection of this invention.
[0059] Example 1 This embodiment discloses a basic moisture-triggered, viscous-toughened, and controlled drainage asphalt binder. By weight, it includes 100 parts of No. 70 road petroleum asphalt, 6 parts of isocyanate-terminated polyurethane prepolymer, 3 parts of silane-terminated polyurethane prepolymer, 0.4 parts of aminosilane coupling agent, 0.3 parts of phosphate ester interface reinforcing agent, 0.15 parts of organic bismuth reaction regulating catalyst, 0.4 parts of amine anti-stripping agent, 1.2 parts of organic modified montmorillonite, 3 parts of naphthenic oil, 0.4 parts of hindered phenolic antioxidant, and 0.2 parts of hindered amine light stabilizer.
[0060] In this embodiment, the preparation method of the terminal isocyanate-type polyurethane prepolymer is as follows: 100 parts by weight of (PPG-2000) are dehydrated for 1 hour at 110°C under a vacuum of not less than 0.09 MPa. The temperature is then lowered to 80°C and protected with dry nitrogen gas. ~28 parts of liquefied diphenylmethane diisocyanate (MDI) are slowly added, and the reaction is carried out at 80°C for 3 hours. During the reaction, the NCO mass fraction of the system is measured. The reaction is stopped when the NCO mass fraction reaches ~4.0%, yielding the terminal isocyanate-type polyurethane prepolymer. The obtained prepolymer is sealed and stored in a moisture-proof environment for later use.
[0061] The preparation method of silane-terminated polyurethane prepolymer is as follows: 100 parts by mass of PPG-3000 are vacuum dehydrated at 1150℃ for 50 min. After cooling, 12 parts of isophorone diisocyanate (IPDI) and 0.005 parts of dibutyltin dilaurate are added under nitrogen protection. The mixture is reacted at 100℃ for 3 h to obtain isocyanate-terminated polyurethane prepolymer. Then, the temperature is lowered to 35℃, and 10 parts of 3-aminopropyltriethoxysilane (KH-550 / APTES) are added. After stirring evenly, the temperature is raised to 60℃ and reacted until the free NCO is basically completely reacted to obtain triethoxysilane-terminated polyurethane prepolymer.
[0062] The aminosilane coupling agent is 3-aminopropyltriethoxysilane (KH-550); the phosphate ester interface enhancer is C12~C14 fatty alcohol polyoxyethylene ether phosphate (AEO-3P); the organic bismuth reaction regulating catalyst is bismuth neodecanoate; the amine anti-stripping agent is octadecylamine; the hindered phenolic antioxidant is antioxidant 1010; and the hindered amine light stabilizer is light stabilizer 770.
[0063] The organically modified montmorillonite used is hexadecyltrimethylammonium bromide-modified montmorillonite (CTAB-MMT). Its preparation method is as follows: 100 parts by mass of sodium-based montmorillonite are dispersed in approximately 1600 parts by mass of deionized water, the temperature is raised to 80°C, approximately 44 parts by mass of hexadecyltrimethylammonium bromide are added, and the mixture is stirred and reacted at 80°C for 8 hours. After the reaction, the mixture is filtered and repeatedly washed with deionized water until the filtrate no longer produces obvious silver bromide precipitate when tested with silver nitrate solution. Subsequently, it is vacuum dried at 90°C, ground, and passed through a 320-mesh sieve to obtain the organically modified montmorillonite.
[0064] The preparation method of moisture-triggered, viscous, and ductile-controlled drainage asphalt binder in this embodiment is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir it at a low speed of 500r / min for 30min to fully dehydrate the asphalt and keep it in a uniform flow state; 2. Organically modified montmorillonite and naphthenic oil are premixed to form a uniform pre-dispersed slurry, which is then added to hot asphalt. The slurry is then subjected to high-speed shearing at 160℃ and 3000r / min for 30min to ensure that the nanosheet barrier material is uniformly dispersed in the asphalt system. 3. Control the system temperature at 155℃, slowly add the isocyanate-terminated polyurethane prepolymer, and shear at 2000r / min for 30min to make the polyurethane prepolymer uniformly dispersed and form a preliminary composite viscoelastic system with the asphalt. 4. Reduce the system temperature to 150℃, add silane-terminated polyurethane prepolymer, aminosilane coupling agent and phosphate ester interface reinforcing agent, and continue stirring at 1800r / min for 25min to ensure uniform dispersion of post-curing components and interface anchoring components. 5. Add organic bismuth reaction regulating catalyst and amine anti-stripping agent, stir at 145~150℃ for 20min to regulate the subsequent moisture-triggered curing reaction rate of the binder and improve the water stripping resistance of the asphalt-aggregate interface. 6. Add hindered phenolic antioxidants and hindered amine light stabilizers, and stir at low speed for 40 minutes at 145℃ to allow the system to fully stabilize and develop, thus obtaining a basic moisture-triggered viscosity-toughness-controlled drainage asphalt binder.
[0065] This embodiment utilizes the synergistic effect of isocyanate-terminated polyurethane prepolymer and silane-terminated polyurethane prepolymer to maintain the appropriate viscosity of the binder during the construction stage. After the drainage asphalt mixture is formed, the environmental moisture in the interconnected pores can be used to trigger the post-curing reaction, gradually forming an elastic and toughened binder film, thereby improving the drainage asphalt mixture's resistance to scattering and water damage.
[0066] Example 2: High water loss resistant moisture-triggered, viscous, and regulated drainage asphalt binder By weight, take 100 parts of SBS modified bitumen, 7 parts of isocyanate-terminated polyurethane prepolymer, 4 parts of silane-terminated polyurethane prepolymer, 0.5 parts of epoxy silane coupling agent, 0.5 parts of phosphate ester interface reinforcing agent, 0.2 parts of organozinc reaction regulating catalyst, 0.6 parts of non-amine anti-stripping agent, 1.5 parts of hydrotalcite, 3 parts of bio-based compatibilizing oil, 0.5 parts of hindered phenolic antioxidant, and 0.3 parts of ultraviolet absorber.
[0067] In this embodiment, the isocyanate-terminated polyurethane prepolymer and the silane-terminated polyurethane prepolymer are the same as in Example 1.
[0068] The epoxy silane coupling agent is γ-glycidoxypropyltrimethoxysilane (KH-560); the phosphate ester interface enhancer is AEO-3P; the organozinc reaction regulating catalyst is zinc neodecanoate; the non-amine anti-stripping agent is a phosphate ester type non-amine anti-stripping agent; the hydrotalcite is a Mg-Al type layered double hydroxide with a Mg / Al molar ratio of approximately 3:1 and an average particle size of no more than 10 μm; the bio-based compatibilizing oil is epoxidized soybean oil; the hindered phenolic antioxidant is antioxidant 1010; and the ultraviolet absorber is UV-326.
[0069] The preparation method is as follows: 1. Heat the SBS modified asphalt to 160℃ and stir at low speed at 600r / min for 30min to soften it fully and maintain a uniform flow state; 2. The hydrotalcite and bio-based compatibilizer oil are premixed to form a uniform dispersion system, which is then added to hot asphalt. The mixture is then subjected to high-speed shearing at 170℃ and 3000r / min for 30min to ensure that the hydrotalcite sheet material is uniformly dispersed in the asphalt system. 3. Control the system temperature at 155℃, add the isocyanate-terminated polyurethane prepolymer, and shear at 2000r / min for 30min to fully combine the polyurethane prepolymer with the modified asphalt. 4. Reduce the system temperature to 150℃, add silane-terminated polyurethane prepolymer, epoxy silane coupling agent and phosphate ester interface reinforcing agent, and continue stirring at 2000 r / min for 30 min to ensure uniform dispersion of the interface anchoring components. 5. Add the organic zinc reaction regulating catalyst and the non-amine anti-stripping agent, and stir at 145~150℃ for 20 min to fully disperse the catalytic regulating component and the water loss prevention component; 6. Add hindered phenolic antioxidants and UV absorbers, and stir at low speed for 40 minutes at 145℃ to stabilize the binder system and obtain a highly water-resistant, moisture-triggered, viscosity-tuning, and drainage asphalt binder.
[0070] Based on the moisture-triggered curing system jointly constructed by isocyanate-terminated polyurethane prepolymers and silane-terminated polyurethane prepolymers, this embodiment uses an epoxy silane coupling agent and a phosphate ester interface reinforcing agent to further enhance the interfacial anchoring effect between the binder and the aggregate surface. At the same time, through the synergistic effect of hydrotalcite lamellae material and non-amine anti-stripping agents, the interfacial adhesion retention ability of the binder under immersion, freeze-thaw and humid heat cycling conditions is improved, making it suitable for drainage asphalt pavements in rainy, humid, bridge deck paving or areas with high risk of water damage.
[0071] Example 3: Anti-aging and moisture-retaining moisture-triggered, viscosity-regulating, and toughening drainage asphalt binder By weight, take 100 parts of No. 70 road petroleum asphalt, 8 parts of isocyanate-terminated polyurethane prepolymer, 5 parts of silane-terminated polyurethane prepolymer, 0.4 parts of aminosilane coupling agent, 0.3 parts of catechol interface reinforcing agent, 0.3 parts of reaction regulating catalyst, 0.5 parts of organosilicon hydrophobic agent, 1.5 parts of layered silicate, 2.5 parts of low viscosity polyether, 0.5 parts of hindered phenolic antioxidant, 0.3 parts of phosphite antioxidant, and 0.3 parts of hindered amine light stabilizer.
[0072] In this embodiment, the isocyanate-terminated polyurethane prepolymer and the silane-terminated polyurethane prepolymer are the same as in Example 1; the aminosilane coupling agent is KH-550; the catechol interface enhancer is catechol (1,2-benzenediol); the reaction regulating catalyst is bismuth neodecanoate; the organosilicon hydrophobic agent is methyl hydrogen silicone oil; the layered silicate is organically modified montmorillonite; the low viscosity polyether is PPG-400; the hindered phenolic antioxidant is antioxidant 1010; the phosphite antioxidant is antioxidant 168; and the hindered amine light stabilizer is light stabilizer 770.
[0073] The preparation method is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir it at low speed at 400r / min for 30min to fully dehydrate it and keep it in a uniform flow state; 2. The layered silicate is premixed with low-viscosity polyether to form a pre-dispersed slurry, which is then added to hot asphalt and subjected to high-speed shearing at 150℃ and 3000r / min for 35min to ensure that the layered silicate is uniformly dispersed in the asphalt system. 3. Control the system temperature at 155℃, add the blocked isocyanate type polyurethane prepolymer, and shear at 2000r / min for 30min to make the polyurethane prepolymer uniformly dispersed in the asphalt system; 4. Reduce the system temperature to 150℃, add silane-terminated polyurethane prepolymer, aminosilane coupling agent and catechol interface reinforcing agent, and continue stirring at 1500r / min for 30min to fully disperse the post-curing component and interface reinforcing component. 5. Add microencapsulation reaction control catalyst and organosilicon hydrophobic agent, and stir at 145~150℃ for 20 min to enable the binder to have subsequent moisture-triggered curing ability and hydrophobic anti-peeling ability. 6. Add hindered phenolic antioxidants, phosphite antioxidants and hindered amine light stabilizers, and stir at low speed for 45 minutes at 145℃ to allow the system to fully stabilize and develop, thus obtaining an anti-aging and moisture-triggered viscosity-tuning drainage asphalt binder.
[0074] This embodiment employs a moisture-responsive post-curing system constructed from both isocyanate-terminated polyurethane prepolymers and silane-terminated polyurethane prepolymers. The reaction rate during the construction phase of the binder is controlled by a reaction-regulated catalyst, ensuring sufficient construction time during mixing, transportation, and paving. After the mixture is formed, ambient moisture gradually enters the binder film layer through interconnected pores, promoting moisture-responsive post-curing of the isocyanate-terminated polyurethane prepolymer and facilitating the hydrolysis and condensation of the silane-terminated components, forming a viscous and toughened reinforcing network. Simultaneously, layered silicates, antioxidant 1010, antioxidant 168, and hindered amine light stabilizer 770 collectively delay the thermo-oxidative and photo-oxidative aging of the binder, improving its anti-scattering properties and surface function retention after aging.
[0075] To illustrate the technical effects of the moisture-triggered, viscosity-regulating, and toughness-controlled drainage asphalt binder of the present invention, the following comparative examples are provided.
[0076] Comparative Example 1: Ordinary SBS modified asphalt binder By weight, take 100 parts of No. 70 road petroleum asphalt and 5 parts of SBS modifier. The SBS modifier used is YH-791 linear SBS produced by Sinopec Baling Petrochemical.
[0077] The preparation method is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir at low speed for 30 minutes to fully dehydrate it and maintain a uniform flow state; 2. Heat to 180℃, add SBS modifier, and shear at high speed at 4500r / min for 60min to ensure that SBS modifier is uniformly dispersed in the asphalt system; 3. Reduce the system temperature to 165℃ and stir at low speed for 60 minutes to obtain ordinary SBS modified asphalt binder.
[0078] This comparative example uses a conventional SBS-modified asphalt system to evaluate the basic properties of ordinary polymer-modified asphalt in drainage asphalt mixtures. This system exhibits some elastic recovery and high-temperature stability, but lacks moisture-triggered curing components, silane-terminated polyurethane prepolymers, interfacial anchoring agents, nanosheet barrier materials, and a construction viscosity control system, making it difficult to form an elastic-toughened cementitious film after the drainage asphalt mixture is formed. Therefore, this comparative example primarily illustrates the improved performance of this invention compared to ordinary SBS-modified asphalt in terms of anti-scattering, anti-water loss, anti-aging, and long-term functional retention.
[0079] Comparative Example 2: Conventional High-Viscosity Modified Asphalt Binder By weight, take 100 parts of No. 70 road petroleum asphalt, 5 parts of SBS modifier, and 8 parts of C5 / C9 copolymer tackifying resin. The C5 / C9 copolymer tackifying resin is HC-110 type C5 / C9 copolymer petroleum resin, with a ring and ball softening point of 105~115℃.
[0080] The preparation method is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir at low speed for 30 minutes to fully dehydrate it and maintain a uniform flow state; 2. Heat to 180℃, add SBS modifier, and shear at high speed at 4500r / min for 60min to allow the SBS modifier to fully swell, shear and disperse in the asphalt system; 3. Add C5 / C9 copolymer tackifying resin and continue shearing at 170~180℃ for 40 minutes to ensure uniform dispersion of the tackifying resin and improve the adhesion performance of the binder; 4. Reduce the system temperature to 165℃ and stir at low speed for 60 minutes to obtain conventional high-viscosity modified asphalt binder.
[0081] This comparative example is a traditional high-viscosity modified asphalt system, which mainly improves the initial viscosity of the binder and the aggregate adhesion capacity through SBS modifiers and tackifying resins. This system can reduce early dispersion loss in drainage asphalt mixtures to some extent, but its technical approach relies primarily on increasing initial viscosity to achieve anti-dispersion, which easily leads to high construction viscosity during mixing, paving, and compaction stages. Furthermore, it lacks the ability to achieve post-curing through moisture triggering, interface anchoring enhancement, and toughness retention after aging. Therefore, this comparative example illustrates that the present invention does not simply rely on increasing binder viscosity, but rather achieves comprehensive performance improvement through controllable viscosity during the construction stage and enhanced viscosity and toughness after molding.
[0082] Comparative Example 3: Cementitious material without silane-terminated polyurethane prepolymer By weight, take 100 parts of No. 70 road petroleum asphalt, 6 parts of isocyanate-terminated polyurethane prepolymer (preparation method is the same as in Example 1), 0.4 parts of aminosilane coupling agent, 0.3 parts of phosphate ester interface reinforcing agent, 0.15 parts of organic bismuth reaction regulating catalyst, 0.4 parts of amine anti-stripping agent, 1.2 parts of organic modified montmorillonite, 3 parts of naphthenic oil, 0.4 parts of hindered phenolic antioxidant, and 0.2 parts of hindered amine light stabilizer.
[0083] The preparation method is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir it at low speed of 500r / min for 30min to fully dehydrate it and keep it in a uniform flow state; 2. Organically modified montmorillonite and naphthenic oil are premixed to form a uniform pre-dispersed slurry, which is then added to hot asphalt. The slurry is then subjected to high-speed shearing at 160℃ and 3000r / min for 30min to ensure that the nanosheet barrier material is uniformly dispersed in the asphalt system. 3. Control the system temperature at 155℃, slowly add the isocyanate-terminated polyurethane prepolymer, and shear at 2000r / min for 30min to ensure that the polyurethane prepolymer is uniformly dispersed in the asphalt system. 4. Reduce the system temperature to 150℃, add aminosilane coupling agent and phosphate ester interface enhancer, and continue stirring at 1800r / min for 25min to ensure uniform dispersion of the interface anchoring components. 5. Add the organic bismuth reaction regulating catalyst and the amine anti-stripping agent, and stir at 145~150℃ for 20 min to fully disperse the catalytic regulating component and the anti-stripping component; 6. Add hindered phenolic antioxidants and hindered amine light stabilizers, and stir at low speed for 40 minutes at 145℃ to allow the system to stabilize and develop, thus obtaining a binder containing silane-terminated polyurethane prepolymer.
[0084] The main difference between this comparative example and Example 1 is the absence of silane-terminated polyurethane prepolymer. Due to the lack of silane-terminated components that can undergo hydrolysis and condensation reactions under ambient moisture, the post-curing network building ability of the binder is weakened, and the degree of transformation of the binder film from a viscoelastic state during construction to a more viscous and tougher state during service is insufficient. Therefore, this comparative example is used to illustrate the role of silane-terminated polyurethane prepolymer in moisture-triggered post-curing, improved bond strength, enhanced elasticity and toughness, and improved anti-scattering properties after immersion in water.
[0085] Comparative Example 4: Cementitious material without interfacial anchoring agent and nanosheet barrier material By weight, take 100 parts of No. 70 road petroleum asphalt, 6 parts of isocyanate-terminated polyurethane prepolymer (preparation method is the same as in Example 1), 3 parts of silane-terminated polyurethane prepolymer (preparation method is the same as in Example 1), 0.15 parts of organic bismuth reaction regulating catalyst, 0.4 parts of amine anti-stripping agent, 3 parts of naphthenic oil, 0.4 parts of hindered phenolic antioxidant, and 0.2 parts of hindered amine light stabilizer.
[0086] The preparation method is as follows: 1. Heat the No. 70 road petroleum asphalt to 160℃ and stir it at low speed of 500r / min for 30min to fully dehydrate it and keep it in a uniform flow state; 2. Add naphthenic oil and stir at 150~160℃ for 20 minutes to ensure that the construction viscosity modifier is evenly dispersed in the asphalt system; 3. Control the system temperature at 155℃, slowly add the isocyanate-terminated polyurethane prepolymer, and shear at 2000r / min for 30min to make the polyurethane prepolymer uniformly dispersed and form a composite viscoelastic system with the asphalt. 4. Reduce the system temperature to 150℃, add silane-terminated polyurethane prepolymer, and continue stirring at 1800 r / min for 25 min to ensure uniform dispersion of the post-curing components; 5. Add organic bismuth reaction regulating catalyst and amine anti-stripping agent, stir at 145~150℃ for 20min to enable the binder to have certain moisture-triggered curing ability and water-resistant peeling ability. 6. Add hindered phenolic antioxidants and hindered amine light stabilizers, and stir at low speed for 40 minutes at 145℃ to allow the system to stabilize and develop, thus obtaining a binder without interfacial anchoring agents and nanosheet barrier materials.
[0087] The main difference between this comparative example and Example 1 is the absence of aminosilane coupling agents, phosphate ester interface reinforcing agents, and organically modified montmorillonite. Although this system contains isocyanate-terminated polyurethane prepolymers and silane-terminated polyurethane prepolymers, which can provide some post-curing reinforcement, it lacks interface anchoring components for the aggregate surface. Asphalt-aggregate interfaces are more prone to adhesion degradation under immersion, freeze-thaw cycles, and humid heat cycles. Simultaneously, due to the lack of nanosheet barrier materials, moisture, oxygen, and UV factors can more easily penetrate the binder film, accelerating binder aging, embrittlement, and interface deterioration. Therefore, this comparative example illustrates the synergistic effect of interface anchoring agents and nanosheet barrier materials in improving resistance to water loss, aging, post-aging scattering, and long-term surface function retention.
[0088] The performance test results of the above embodiments and comparative examples are as follows: Table 1. Test results of binder properties
[0089] The rotational viscosity at 135℃ was determined according to T0625-2011 "Asphalt Rotational Viscosity Test (Rotational Viscometer Method)" in JTG3410-2025. The dynamic viscosity at 60℃ was determined according to T0620—2025 "Dynamic Viscosity of Asphalt (Vacuum Capillary Method)". Elastic recovery was determined according to T0662—2000 "Asphalt Elastic Recovery Test"; The difference in segregation softening point was determined according to T0661—2025 "Segregation Test of Polymer Modified Asphalt".
[0090] The method for determining the elastic recovery retention rate after aging is as follows: First, perform rotational heating aging of the thin film according to T0610-2011 in JTG3410-2025, then determine the elastic recovery rate after aging according to T0662-2000, and calculate the retention rate according to "elastic recovery rate after aging / elastic recovery rate before aging × 100%".
[0091] The moisture treatment conditions were as follows: the binder-aggregate bonded sample was placed in an environment with a temperature of 25℃ and a relative humidity of 90%±5% for 72 hours before testing.
[0092] The bond strength after moisture treatment was determined using the BBS test approach for asphalt binder bond strength. A basalt substrate was selected as the aggregate substrate, and binder-aggregate bond specimens were prepared according to AASHTOT 361-22. The specimens were cured at 25℃ and 90% ± 5% relative humidity for 72 hours, and then the pull-out tensile strength was measured using a pull-out bond strength tester. The results are expressed in MPa. AASHTOT 361 refers to the pull-out bond strength between asphalt binder and a solid substrate.
[0093] The method for determining the bond strength retention rate after UV aging is as follows: The binder-aggregate bond specimen is placed in a UVA-340 UV aging chamber with a control wavelength of 340 nm and an irradiation intensity of 1.0 W / (m²·nm). An aging cycle consists of 8 hours of UV irradiation at 60℃ followed by 4 hours of condensation at 50℃, for a total of 9 cycles. After aging, the bond strength is determined according to the aforementioned BBS method, and the retention rate is calculated as "bond strength after UV aging / unaged bond strength × 100%". This UVA-340 irradiation + 4-hour condensation cycle has been used in UV aging studies of drainage asphalt.
[0094] As shown in Table 1, compared with ordinary SBS modified asphalt and conventional high-viscosity modified asphalt, the embodiments of the present invention have lower rotational viscosity at 135℃ than conventional high-viscosity modified asphalt, indicating that they have better fluidity during the construction stage. Meanwhile, the bond strength, elastic recovery, elastic recovery retention rate after aging, and bond strength retention rate after UV aging of the embodiments are all significantly improved after moisture treatment, indicating that the binder can achieve enhanced adhesion and toughness through moisture-triggered post-curing after molding. Comparative Example 3, which does not contain silane-terminated polyurethane prepolymer, has a lower bond strength after moisture treatment than Example 1, indicating that the silane-terminated component plays an important role in moisture-triggered post-curing. Comparative Example 4, which does not contain interface anchoring agent and nanosheet barrier material, shows a decrease in performance retention rate after aging and bond strength retention rate after UV aging, indicating that the interface anchoring and sheet barrier system helps improve the durability of the binder.
[0095] The dynamic viscosity at 60℃ reflects the viscous resistance and bond retention capacity of the binder under higher service temperature conditions. Table 1 shows that the dynamic viscosities at 60℃ for Examples 1-3 of this invention are 72000 Pa·s, 76000 Pa·s, and 74000 Pa·s, respectively, which are higher than the 28000 Pa·s of Comparative Example 1 of ordinary SBS modified asphalt and the 65000 Pa·s of Comparative Example 2 of conventional high-viscosity modified asphalt. Meanwhile, the rotational viscosity at 135℃ for these examples is only 3.2-3.5 Pa·s, lower than the 4.8 Pa·s of conventional high-viscosity modified asphalt. These results indicate that the binder of this invention has good fluidity at construction temperatures while maintaining high viscous resistance and bond retention capacity under service temperature conditions, demonstrating a balance between construction adaptability and service bond performance.
[0096] The difference in segregation softening point reflects the compatibility and stability of multi-component modified binders under high-temperature storage conditions. The differences in segregation softening points of Examples 1-3 were 1.8℃, 1.6℃, and 1.7℃, respectively, which were lower than the differences of 2.0-4.2℃ of Comparative Examples 1-4. This indicates that the moisture-triggered component, the interface-reinforcing component, and the nanosheet material have good dispersion and storage stability in the asphalt system, and the multi-component composite did not cause significant high-temperature segregation.
[0097] Table 2. Performance Test Results of Drainage Asphalt Mixture
[0098] Porosity, Kentenberg scattering loss and immersion Kentenberg scattering loss, freeze-thaw splitting strength ratio, and dynamic stability were determined according to the method in JTG3410-2025.
[0099] The scattering loss after damp heat cycling was determined by the following method: a standard Marshall specimen was immersed in water at 60°C for 24 hours, and then placed in an environment at 25°C for 24 hours, which was considered as one damp heat cycle. A total of 5 cycles were performed. After the treatment, the Kentucky scattering test was carried out in accordance with T0733-2025, and the obtained mass loss rate was taken as the scattering loss after damp heat cycling.
[0100] The scattering loss after UV aging was determined using the following method: the specimen was placed in a UVA-340 UV aging chamber, with one cycle consisting of 8 hours of UV irradiation at 60℃ and 4 hours of condensation at 50℃, for a total of 9 cycles; after aging, the Kentucky scattering loss was tested according to T0733—2025. These UV cycling conditions are consistent with commonly used methods in accelerated UV aging studies of drainage asphalt.
[0101] The retention rates of surface texture depth, friction coefficient after wear, and permeability coefficient were evaluated using a unified wheel-rolling wear treatment. 300mm×300mm×50mm wheel-rolling slab specimens were prepared and subjected to reciprocating wheel rolling at 25℃±2℃ using a rubber test wheel, with a wheel load of 780N±20N, for 5000 cycles. The surface texture depth, pendulum friction coefficient, and permeability coefficient were measured before and after treatment. Surface texture depth was measured according to T0731—2000; pendulum friction coefficient was measured according to T0964—2008 "Method for Testing Road Surface Friction Coefficient with Pendulum Tester" in JTG3450—2019; and permeability coefficient was measured according to T0730—2025. All retention rates were calculated as "index value after wear treatment / index value before wear treatment × 100%". The current standard for the pendulum tester BPN (pendulum value) test method is T0964—2008 in JTG3450—2019.
[0102] As shown in Table 2, the drainage asphalt mixture prepared using the binder of this invention exhibits significantly reduced Kentaburg scattering loss, Kentaburg scattering loss after immersion in water, scattering loss after wet heat cycling, and scattering loss after UV aging, all under conditions of similar porosity. Furthermore, the freeze-thaw splitting strength ratio, dynamic stability, texture depth retention rate, friction coefficient retention rate after abrasion, and permeability coefficient retention rate are all significantly improved. This indicates that the present invention can effectively enhance the drainage asphalt mixture's resistance to scattering, water loss, aging, and long-term surface function retention.
[0103] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical aspects of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A moisture-triggered adhesion-toughness-regulated drainage pavement asphalt binder, characterized in that, By weight, it includes the following components: The composition includes 100 parts asphalt base material, 3-15 parts moisture-triggered polyurethane prepolymer, 1-8 parts silane-terminated polyurethane prepolymer, 0.2-2.0 parts interface anchoring agent, 0.05-0.8 parts reaction regulating catalyst, 0.2-1.5 parts hydrophobic anti-stripping component, 0.5-3.0 parts nanosheet barrier material, 1-6 parts construction viscosity regulator, and 0.2-1.5 parts antioxidant stabilizing component.
2. The drain pavement asphalt binder of claim 1, wherein, The moisture-triggered polyurethane prepolymer is one or a combination of isocyanate-terminated polyurethane prepolymer and polyurethane prepolymer containing moisture-reactive end groups.
3. The asphalt binder for drainage pavement according to claim 1, characterized in that, The silane-terminated polyurethane prepolymer is one or a combination of polyurethane prepolymers containing trimethoxysilyl, triethoxysilyl, methyldimethoxysilyl and methyldiethoxysilyl.
4. The asphalt binder for drainage pavement according to claim 1, characterized in that, The reaction-regulating catalyst is one or a combination of several of the following: organobismuth catalyst, organozinc catalyst, blocked amine catalyst, and microencapsulated catalyst.
5. The asphalt binder for drainage pavement according to claim 1, characterized in that, The interface anchoring agent is one or a combination of aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, phosphate ester interface enhancers, catechol interface enhancers, and dopamine interface enhancers. And / or, the hydrophobic anti-stripping component is one or a combination of amine anti-stripping agents, non-amine anti-stripping agents, organosilicon hydrophobic agents, and phosphate ester anti-stripping agents; And / or, the nanosheet barrier material is one or a composite of several of the following: organically modified montmorillonite, layered silicate, hydrotalcite, graphene oxide, and sheet-like nano silica.
6. The asphalt binder for drainage pavement according to claim 1, characterized in that, By weight, it includes the following components: 100 parts of petroleum asphalt or SBS modified asphalt for No. 70 road, 5-10 parts of isocyanate-terminated polyurethane prepolymer, 2-5 parts of silane-terminated polyurethane prepolymer, 0.4-1.2 parts of a compound of aminosilane coupling agent and phosphate ester interface reinforcing agent, 0.1-0.4 parts of organic bismuth reaction regulating catalyst, 0.3-0.8 parts of hydrophobic anti-stripping component, 1.0-2.0 parts of organic modified montmorillonite or hydrotalcite, 2-4 parts of bio-based compatibilizing oil or naphthenic oil, and 0.4-1.0 parts of a compound of hindered phenolic antioxidant and hindered amine light stabilizer.
7. A method for preparing a moisture-triggered, viscosity-regulating asphalt binder for drainage pavement as described in any one of claims 1 to 6, characterized in that, Includes the following steps: Step 1: Preheating the asphalt base material; Step 2: Premix the nanosheet barrier material with all or part of the construction viscosity modifier to form a pre-dispersed slurry. Add the pre-dispersed slurry to the preheated asphalt base material, or directly add the nanosheet barrier material to the preheated asphalt base material and shear disperse at 150~170℃. Add the remaining or all of the construction viscosity modifier to the system; Step 3: Control the temperature of the system obtained in Step 2 at 145~165℃, slowly add the moisture-triggered polyurethane prepolymer, and shear disperse. Step 4: Adjust the temperature of the system obtained in Step 3 to 140~160℃, add silane-terminated polyurethane prepolymer and interface anchoring agent, and stir to disperse. Step 5: Control the temperature of the system obtained in Step 4 at 135~155℃, add the reaction regulating catalyst and hydrophobic anti-stripping component, and stir to disperse; Step 6: Control the temperature of the system obtained in Step 5 at 130~150℃, add antioxidant stabilizing components, stir, and obtain moisture-triggered viscosity-tuning asphalt binder for drainage pavement.
8. The preparation method according to claim 7, characterized in that, The moisture-triggered polyurethane prepolymer is an isocyanate-terminated polyurethane prepolymer, and the preparation method of the isocyanate-terminated polyurethane prepolymer is as follows: By mass, 100 parts of PPG-2000 were dehydrated at 105~115℃ under a vacuum of not less than 0.09MPa, cooled to 75~80℃ and protected with dry nitrogen, and 27~29 parts of liquefied diphenylmethane diisocyanate were slowly added. The reaction was carried out at 80±2℃. The mass fraction of NCO in the system was measured during the reaction. The reaction was stopped when the mass fraction of NCO reached 3.7%~4.3% to obtain the isocyanate-terminated polyurethane prepolymer.
9. The preparation method according to claim 7, characterized in that, The silane-terminated polyurethane prepolymer is a triethoxysilane-terminated polyurethane prepolymer, and the preparation method of the triethoxysilane-terminated polyurethane prepolymer is as follows: By weight, 100 parts of PPG-3000 were vacuum dehydrated at 110-120℃. After cooling, 12-13 parts of isophorone diisocyanate and 0.005-0.01 parts of dibutyltin dilaurate were added under nitrogen protection. The mixture was reacted at 95-105℃ to obtain a polyurethane prepolymer with an NCO mass fraction of 1.5%-1.8%. The temperature was then lowered to 30-40℃, and 9-10 parts of 3-aminopropyltriethoxysilane were added. After stirring evenly, the temperature was raised to 55-65℃ to react until the free NCO was completely reacted, thus obtaining a triethoxysilane-terminated polyurethane prepolymer.
10. The preparation method according to claim 7, characterized in that, Step one specifically involves heating the asphalt base material to 150~170℃ and stirring it at 300~800r / min for 20~40min; And / or, the shearing conditions in step two are: shearing at 2000~4000 r / min for 20~50 min; And / or, the shearing conditions in step three are: shearing at 1000~3000 r / min for 20~40 min; And / or, the stirring conditions in step four are: stirring at 800~2500 r / min for 15~40 min.