Method for preparing modified calcium carbonate powder and use thereof

By combining ultrasonic cleaning, vacuum drying, and chemical reaction steps in the preparation method of modified calcium carbonate powder, the problems of uneven adhesion of modifier and inconsistent particle size distribution were solved, achieving uniform particle size distribution and efficient solvent recovery of modified calcium carbonate powder, thus improving the performance and environmental friendliness of the composite material.

CN123152309APending Publication Date: 2026-11-24HENAN JIEBAO NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411661511.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for preparing modified calcium carbonate powder suffer from problems such as uneven adhesion of the modifier, inconsistent particle size distribution, and low solvent recovery efficiency. These issues result in poor dispersion and compatibility of the powder in the substrate, increasing production costs and environmental burden.

Method used

By employing steps such as ultrasonic cleaning, vacuum drying, chemical reaction, grinding, and dispersion, combined with ultrasonic dispersion and vacuum drying technologies, the modifier is ensured to adhere uniformly and the particle size distribution is controlled. At the same time, the solvent is recovered for use in the next batch preparation, thereby improving the stability of the modified layer and the solvent utilization rate.

Benefits of technology

This method achieves uniform particle size and no agglomeration of modified calcium carbonate powder, improving the filling effect and long-term performance of composite materials, reducing production costs and solvent consumption, and meeting environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152309A_ABST
    Figure CN123152309A_ABST
Patent Text Reader

Abstract

This invention relates to the field of materials science and discloses a method for preparing modified calcium carbonate powder and its application. The method includes the following steps: S1, pretreating the surface of calcium carbonate powder to remove surface impurities and increase surface activity, including ultrasonic cleaning of the calcium carbonate powder in a solvent followed by drying; S2, mixing the pretreated calcium carbonate powder with one or more modifiers to allow the modifiers to be initially adsorbed onto the surface of the calcium carbonate powder; S3, conducting a chemical reaction under specific temperature and stirring conditions to allow the modifiers to be uniformly adhered to the surface of the calcium carbonate powder, thereby enhancing the hydrophobicity, dispersibility, and compatibility with the substrate of the calcium carbonate powder. This invention, by combining ultrasonic dispersion, vacuum drying, and nitrogen protection technologies, achieves uniform particle size and non-agglomerated distribution characteristics in the modified calcium carbonate powder while maintaining the stability of the modified layer, thus improving the filling effect and long-term performance of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials science, specifically to a method for preparing modified calcium carbonate powder and its applications. Background Technology

[0002] Modified calcium carbonate powder, widely used as a filler in composite materials such as plastics, rubber, and coatings, plays a crucial role in improving the mechanical properties, durability, and stability of these materials through its preparation methods. By modifying the surface of calcium carbonate powder, its hydrophobicity and dispersibility can be enhanced, improving its compatibility with organic matrices and resulting in composite materials exhibiting superior physical properties and environmental resistance.

[0003] Currently, the main methods for preparing modified calcium carbonate powder include using coupling agents, surface treatment agents, and ultrasonic dispersion technology. Typically, calcium carbonate powder is mixed with a modifier, stirred, and then heated to allow the modifier molecules to adhere to the powder surface, forming a stable hydrophobic layer. This improves the dispersibility of the calcium carbonate powder and its adhesion to the substrate.

[0004] However, existing technologies generally suffer from problems such as uneven adhesion of modifiers, inconsistent particle size distribution, and solvent waste. Due to insufficient process control during the modification process, the modified layer may be unstable, resulting in poor dispersion and compatibility of the powder in the substrate. In addition, the efficiency of solvent use and recycling is not high, which increases production costs and environmental burden. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing modified calcium carbonate powder and its application, solving the problems of uneven modifier adhesion, inconsistent particle size distribution, and low solvent recovery efficiency in existing technologies.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing modified calcium carbonate powder, comprising the following steps:

[0007] S1. Surface pretreatment of calcium carbonate powder to remove surface impurities and increase surface activity, including ultrasonic cleaning of calcium carbonate powder in a solvent and then drying it.

[0008] S2. Mix the pretreated calcium carbonate powder with one or more modifiers to allow the modifiers to be initially adsorbed onto the surface of the calcium carbonate powder.

[0009] S3. Under specific temperature and stirring conditions, a chemical reaction is carried out to allow the modifier to adhere uniformly to the surface of the calcium carbonate powder, thereby enhancing the hydrophobicity, dispersibility and compatibility of the calcium carbonate powder with the substrate.

[0010] S4. After the reaction is complete, place the modified calcium carbonate powder in a vacuum drying oven to dry it in order to remove residual solvent and stabilize the surface modified layer.

[0011] S5. Grind the dried modified calcium carbonate powder to control the powder particle size and specific surface area so that it meets the predetermined dispersibility and particle size requirements.

[0012] S6. Disperse the ground modified calcium carbonate powder to avoid particle agglomeration and obtain modified calcium carbonate powder with uniform particle size distribution.

[0013] Preferably, the surface pretreatment includes the following steps:

[0014] Calcium carbonate powder was placed in anhydrous ethanol solution and surface impurities were removed by ultrasonic cleaning at a frequency of 40 kHz, a power of 100 W, and a cleaning time of 10 minutes.

[0015] The cleaned calcium carbonate powder was placed in a vacuum drying oven and dried at 65°C for 1 hour.

[0016] The dried calcium carbonate powder was transferred to a nitrogen-protected vacuum drying oven and dried at 90°C for 2 hours to ensure that there was no moisture on the powder surface.

[0017] Preferably, the preliminary adsorption includes stirring the pretreated calcium carbonate powder and the modifier at room temperature for 15 minutes to preliminarily adsorb the modifier.

[0018] Preferably, the chemical reaction includes the following steps:

[0019] The mixture was heated to 80°C and reacted for 30 minutes with a stirring speed of 700 rpm.

[0020] The system was heated to 120°C and the reaction continued for 20 minutes. The stirring speed was set to 1000 rpm to ensure that the modifier was uniformly attached to the surface of the calcium carbonate powder.

[0021] Preferably, the modifier includes any one of the following: titanate coupling agent, aminosilane coupling agent, methacryloxysilane coupling agent, and stearic acid.

[0022] Preferably, drying includes the following steps:

[0023] The modified calcium carbonate powder was dried in a vacuum drying oven at 80°C for 2 hours to remove residual solvent.

[0024] The dried powder was transferred to a nitrogen-protected vacuum drying oven at 100°C and dried for another hour to ensure the stability of the surface modified layer.

[0025] Preferably, the grinding process includes using an air jet mill to control the powder particle size to below 5 micrometers in order to obtain an ideal particle size distribution.

[0026] Preferably, the dispersion treatment includes adding the ground powder to anhydrous ethanol and treating it for 15 minutes using an ultrasonic disperser at a frequency of 60 kHz and a power of 200 W to reduce agglomeration and obtain modified calcium carbonate powder with a uniform particle size distribution.

[0027] Preferably, the method further includes a solvent recovery step, in which the solvent after the chemical reaction of S2 and S3 is recovered by distillation and condensation devices, so that the solvent recovery rate reaches more than 90%, and is used in the preparation process of the next batch.

[0028] This invention also provides the application of modified calcium carbonate powder in composite materials, including:

[0029] The product is used in plastics, rubber, or coatings to improve the hydrophobicity, mechanical strength, and thermal stability of composite materials.

[0030] This invention provides a method for preparing modified calcium carbonate powder and its applications. It has the following beneficial effects:

[0031] 1. This invention combines ultrasonic dispersion, vacuum drying and nitrogen protection technologies to modify calcium carbonate powder, achieving uniform particle size and no agglomeration distribution while maintaining the stability of the modified layer, thereby improving the filling effect and long-term performance of the composite material.

[0032] 2. The application of solvent recovery technology not only improves production efficiency but also significantly reduces production costs and solvent consumption, meets environmental protection requirements, has sustainable development advantages, and provides a guarantee for economic and environmental benefits in industrial production. Attached Figure Description

[0033] Figure 1 This is a flowchart of the preparation method of the present invention. Detailed Implementation

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0035] Please see the appendix Figure 1 This invention provides a method for preparing modified calcium carbonate powder, which includes the following steps:

[0036] S1. Surface pretreatment of calcium carbonate powder to remove surface impurities and increase surface activity, including ultrasonic cleaning of calcium carbonate powder in solvent and then drying. This pretreatment step can ensure that the subsequent modifier can be uniformly attached to the surface of calcium carbonate powder, improve the modification efficiency, and enhance the surface activity of the powder, so that it has a higher reaction rate and adhesion in the subsequent reaction.

[0037] S2. The pretreated calcium carbonate powder is mixed with one or more modifiers, so that the modifiers are initially adsorbed on the surface of the calcium carbonate powder. Through the initial adsorption step, the modifiers are ensured to be evenly distributed on the powder surface, laying the foundation for subsequent chemical reactions and avoiding local excessive aggregation of modifiers, thereby improving the uniformity and stability of the final modification.

[0038] S3. Under specific temperature and stirring conditions, a chemical reaction is carried out to make the modifier uniformly adhere to the surface of calcium carbonate powder, thereby enhancing the hydrophobicity, dispersibility and compatibility of calcium carbonate powder with the substrate. Through specific temperature and stirring conditions, the modifier can be deeply bonded to the surface of calcium carbonate, improving the hydrophobicity and dispersibility of the powder and enhancing its compatibility in the composite material, further improving the overall performance of the composite material.

[0039] S4. After the reaction is complete, the modified calcium carbonate powder is placed in a vacuum drying oven to dry in order to remove residual solvent and stabilize the surface modification layer. Vacuum drying and nitrogen protection ensure the stability of the surface modification layer of the modified calcium carbonate powder, effectively improving the thermal stability and antioxidant properties of the powder in subsequent processing.

[0040] S5. Grind the dried modified calcium carbonate powder to control the powder particle size and specific surface area, so that it meets the predetermined dispersibility and particle size requirements. Through reasonable grinding control, modified calcium carbonate powder with uniform particle size can be obtained, which can improve its dispersibility and filling effect in composite materials and ensure the performance consistency and quality stability of the final product.

[0041] S6. The ground modified calcium carbonate powder is dispersed to avoid particle agglomeration and obtain modified calcium carbonate powder with uniform particle size distribution. Ultrasonic dispersion can further reduce the agglomeration of modified calcium carbonate powder, ensure the uniform dispersion of powder in composite materials, and improve the mechanical properties and structural stability of composite materials.

[0042] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the surface pretreatment includes the following steps:

[0043] Calcium carbonate powder was placed in anhydrous ethanol solution and ultrasonically cleaned to remove surface impurities. The ultrasonic frequency was 40 kHz, the power was 100 W, and the cleaning time was 10 minutes. Ultrasonic cleaning effectively removed organic impurities and other contaminants from the surface of the calcium carbonate powder, ensuring a clean powder surface, enhancing its surface activity, and creating conditions for the uniform adhesion of subsequent modifiers. The use of anhydrous ethanol further reduced the influence of moisture adsorption on the powder surface, thereby improving the modification efficiency in subsequent reactions.

[0044] The cleaned calcium carbonate powder was placed in a vacuum drying oven and dried at 65°C for 1 hour. Vacuum drying reduces the ambient pressure, thereby lowering the evaporation temperature of ethanol. This allows for rapid evaporation of ethanol at a lower temperature without damaging the powder structure, thus avoiding the influence of solvent residue on subsequent reactions, while maintaining the dryness and activity of the powder surface.

[0045] The dried calcium carbonate powder was transferred to a nitrogen-protected vacuum drying oven and dried at 90°C for 2 hours to ensure that the powder surface was free of moisture. Nitrogen protection can prevent moisture and oxygen in the air from reacting with or being adsorbed by the powder, thereby ensuring that the powder surface is in an anhydrous state and improving surface activity. At the same time, the combination of high temperature and vacuum ensures that residual moisture in the powder is completely removed, providing a stable chemical environment for subsequent modification processes.

[0046] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the preliminary adsorption includes stirring the pretreated calcium carbonate powder and the modifier at room temperature for 15 minutes to pre-adsorb the modifier. Through this preliminary adsorption step, the modifier can be uniformly distributed on the surface of the calcium carbonate powder to form a preliminary adsorption layer. This adsorption layer not only provides a good contact basis for subsequent chemical reactions, but also significantly improves the utilization efficiency of the modifier and avoids excessive modifier from accumulating locally. In addition, after the preliminary adsorption layer is formed, the hydrophobic end of the modifier faces outward, giving the powder preliminary hydrophobicity and dispersibility, which helps to further enhance the surface modification effect of the powder in subsequent chemical reactions.

[0047] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the chemical reaction includes the following steps:

[0048] The mixture was heated to 80°C and reacted for 30 minutes with a stirring speed of 700 rpm. Under the heating condition of 80°C, the activity of the modifier molecules was further activated, allowing them to diffuse more fully onto the surface of the calcium carbonate powder. This temperature falls precisely within the modifier's active temperature range, enabling the formation of weak chemical bonds between the modifier and the hydroxyl and polar groups on the powder surface. Simultaneously, stirring provided a uniform dispersion environment, ensuring that each powder particle could fully contact the modifier molecules and avoid localized concentration differences. This combination of heating and stirring promotes the uniform adhesion of the modifier to the powder surface, forming preliminary chemical bonds.

[0049] The system was heated to 120°C and the reaction continued for 20 minutes, with the stirring speed set to 1000 rpm to ensure that the modifier was uniformly adhered to the surface of the calcium carbonate powder. The high-temperature reaction at 120°C further enhanced the bonding strength between the modifier and the calcium carbonate powder, making the modified layer more stable and less prone to falling off, thus ensuring the durability of the modification effect in subsequent applications. At the same time, the uniform modified layer improved the hydrophobicity of the calcium carbonate powder and its compatibility with organic substrates, resulting in better dispersion in the composite material and further improving the mechanical properties and stability of the composite material.

[0050] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the modifier comprises any one of the following: titanate coupling agent, aminosilane coupling agent, methacryloxysilane coupling agent, and stearic acid.

[0051] Specifically: using titanate coupling agents as modifiers can enhance the hydrophobicity of calcium carbonate powder and its compatibility with organic phases, making it particularly suitable for organic substrates such as plastics and rubber. This allows the modified calcium carbonate to be uniformly dispersed in the substrate, improving the mechanical properties and water resistance of the composite material.

[0052] The use of aminosilane coupling agents can significantly enhance the compatibility of calcium carbonate powder in organic materials containing polar groups such as amino, hydroxyl or carboxyl groups, improve the adhesion and mechanical strength of composite materials, and is particularly suitable for engineering plastics, epoxy resins and polyurethanes.

[0053] By using methacryloxysilane coupling agents, modified calcium carbonate powder can be given better reactivity, enabling it to undergo polymerization reactions with organic substrates under ultraviolet light or heating conditions, thereby improving the crosslinking density and mechanical properties of composite materials, making it particularly suitable for use in UV-curable coatings and adhesives.

[0054] Stearic acid is a fatty acid whose long-chain hydrocarbon structure can form a hydrophobic layer on the surface of calcium carbonate powder, preventing the adsorption of water molecules and polar substances, thus giving the powder good hydrophobicity and dispersibility in non-polar organic substrates.

[0055] Please see the appendix Figure 1 In a preferred embodiment of the present invention, drying includes the following steps:

[0056] The modified calcium carbonate powder was placed in a vacuum drying oven at 80°C for 2 hours to remove residual solvent. The 80°C temperature setting can effectively accelerate the evaporation rate of the solvent without causing the decomposition of the modifier or the agglomeration of the calcium carbonate powder. Vacuum drying at 80°C can quickly and thoroughly remove the residual organic solvent in the modified calcium carbonate powder, avoiding the impact of solvent residue on the subsequent performance of the powder.

[0057] The dried powder was transferred to a nitrogen-protected vacuum drying oven at 100°C and dried for another hour to ensure the stability of the surface modification layer. The temperature of 100°C can completely remove residual trace moisture and solvents and enhance the stability of the modification layer at high temperatures.

[0058] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the grinding includes using an air jet mill to control the powder particle size to below 5 micrometers to obtain an ideal particle size distribution. Through the grinding process of the air jet mill, the particle size of the modified calcium carbonate powder can be controlled to below 5 micrometers, achieving refinement and uniform distribution. This micrometer-level particle size can improve the dispersibility of calcium carbonate powder in the substrate, avoid particle agglomeration, and thus improve the mechanical properties and surface smoothness of the composite material.

[0059] Please see the appendix Figure 1 In a preferred embodiment of the present invention, the dispersion treatment includes adding the ground powder to anhydrous ethanol and treating it for 15 minutes using an ultrasonic disperser at a frequency of 60 kHz and a power of 200 W to reduce agglomeration and obtain modified calcium carbonate powder with a uniform particle size distribution. Ultrasonic dispersion utilizes the cavitation effect and strong shear force of ultrasound to vibrate and impact the particles in the solution. When the ultrasonic frequency reaches 60 kHz, the tiny bubbles generated by the ultrasound in the liquid grow rapidly and burst violently, forming a shock wave with local high temperature and high pressure, which strongly vibrates and disperses the particles on the surface of the calcium carbonate powder. Through ultrasonic dispersion treatment, the modified calcium carbonate powder can effectively reduce the agglomeration between particles, ensure the uniform distribution of powder particles, thereby improving its dispersibility and filling effect in composite materials. This not only simplifies the dispersion process but also significantly improves the efficiency and effect of dispersion.

[0060] Please see the appendix Figure 1In a preferred embodiment of the present invention, the method further includes a solvent recovery step. The solvent after the chemical reactions S2 and S3 is recovered using a distillation and condensation apparatus, achieving a solvent recovery rate of over 90%, and is then used in the next batch preparation process. Distillation is a physical separation method based on boiling point differences. During heating, anhydrous ethanol preferentially evaporates into the gas phase and then enters the condensation pipe. In the condensation apparatus, a cooling water circulation system rapidly cools the vapor to a liquid state, thereby separating the ethanol from the reaction system. Since ethanol does not participate in the chemical reaction in steps S2 and S3, the ethanol recovered after distillation has high purity and can be directly reused, thus reducing solvent consumption costs in the production process, making the entire preparation process more economical, and reducing organic solvent emissions into the environment, meeting the requirements of environmental protection and green production.

[0061] This invention also provides the application of modified calcium carbonate powder in composite materials, including:

[0062] The product is used in plastics, rubber, or coatings to improve the hydrophobicity, mechanical strength, and thermal stability of composite materials.

[0063] To better understand the present invention, the above content will be described in detail below with reference to specific embodiments.

[0064] Example 1: Preparation and application of modified calcium carbonate powder using titanate coupling agent

[0065] Preparation method:

[0066] Surface pretreatment: Place the calcium carbonate powder in anhydrous ethanol and ultrasonically clean it (40kHz, 100W, 10 minutes). Then dry it in a vacuum drying oven at 65℃ for 1 hour, followed by drying it in a vacuum drying oven at 90℃ under nitrogen protection for 2 hours.

[0067] Preliminary adsorption: The dried calcium carbonate powder is uniformly mixed with titanate coupling agent (2% of the mass of calcium carbonate) and stirred at room temperature for 15 minutes.

[0068] Chemical reaction: Heat the mixture to 80°C and react for 30 minutes with a stirring speed of 700 rpm. Then raise the temperature to 120°C and continue the reaction for 20 minutes (stirring speed of 1000 rpm).

[0069] Drying: The modified powder was placed in a vacuum drying oven at 80°C and dried for 2 hours, followed by drying in a nitrogen-protected environment at 100°C for 1 hour.

[0070] Grinding and dispersion: The powder particle size was controlled to below 5 micrometers using an air jet mill, and then the powder was added to anhydrous ethanol and treated under ultrasonic conditions of 60 kHz and 200 W for 15 minutes.

[0071] Application: The prepared modified calcium carbonate powder was added to polypropylene (10% addition), and plastic products were formed by injection molding. The results showed that the impact strength of the products increased by 15%, and the heat resistance and hydrophobicity were significantly enhanced.

[0072] Example 2: Preparation and application of modified calcium carbonate powder using aminosilane coupling agent

[0073] Preparation method:

[0074] Surface pretreatment: The calcium carbonate powder was ultrasonically cleaned in anhydrous ethanol (40kHz, 100W, 10 minutes), then vacuum dried at 65℃ for 1 hour, and then dried in a nitrogen-protected environment at 90℃ for 2 hours.

[0075] Preliminary adsorption: The pretreated powder is uniformly mixed with aminosilane coupling agent (1.5% of the mass of calcium carbonate) and stirred at room temperature for 15 minutes.

[0076] Chemical reaction: Heat the system to 80°C and react for 30 minutes with a stirring speed of 700 rpm. Then raise the temperature to 120°C and react for another 20 minutes (stirring speed of 1000 rpm).

[0077] Drying and grinding: After vacuum drying at 80°C for 2 hours, further dry at 100°C under nitrogen protection for 1 hour. Use an air jet mill to control the particle size to below 5 micrometers.

[0078] Dispersion treatment: The powder was added to anhydrous ethanol and ultrasonically dispersed for 15 minutes at 60 kHz and 200 W.

[0079] Application: Modified calcium carbonate powder was added to a natural rubber mixture (15% addition), and after uniform mixing, it was vulcanized. Results showed that the tensile strength and tear resistance of the rubber increased by 20%, and its aging resistance was significantly improved.

[0080] Example 3: Preparation and application of modified calcium carbonate powder using methacryloxysilane coupling agent: Preparation method:

[0081] Surface pretreatment: Calcium carbonate powder was ultrasonically cleaned in anhydrous ethanol (40kHz, 100W, 10 minutes), vacuum dried at 65℃ for 1 hour, and then dried in a nitrogen-protected environment at 90℃ for 2 hours.

[0082] Preliminary adsorption: Mix the powder with methacryloyloxysilane coupling agent (1% of the mass of calcium carbonate) and stir at room temperature for 15 minutes.

[0083] Chemical reaction: React at 80℃ and 700 rpm for 30 minutes, then raise the temperature to 120℃ and react at 1000 rpm for 20 minutes.

[0084] Drying and grinding: Vacuum drying for 2 hours, followed by drying for another hour under nitrogen protection at 100°C, and then grinding with an air jet mill to a particle size of less than 5 micrometers.

[0085] Dispersion treatment: The powder was added to anhydrous ethanol and treated under ultrasonic conditions of 60kHz and 200W for 15 minutes.

[0086] Application: Modified calcium carbonate powder was added to acrylic resin coating (10% addition), mixed thoroughly, and then applied to the metal surface. The dried coating exhibited excellent waterproof and abrasion resistance, and the coating adhesion was improved by 30%.

[0087] Comparative Experiment 1: Hydrophobicity Test of Modified Calcium Carbonate Powder

[0088] Experimental objective: To compare the hydrophobicity of the modified calcium carbonate powder prepared in this invention with that of different control groups by measuring the water contact angle, thereby verifying the advantages of this invention in improving the hydrophobic properties of powder.

[0089] Experimental setup

[0090] Experimental group:

[0091] Experimental Group A: Modified calcium carbonate powder prepared according to this invention.

[0092] Control group:

[0093] Control group B: Unmodified calcium carbonate powder.

[0094] Control group C: Calcium carbonate powder modified with traditional titanate coupling agents.

[0095] Control group D: Calcium carbonate powder modified with traditional aminosilane coupling agents.

[0096] Experimental steps

[0097] Sample preparation: The calcium carbonate powder of experimental group A and control groups B, C and D were evenly spread on a glass slide and gently pressed to form a uniform surface layer.

[0098] Contact angle measurement: Using a contact angle meter, add an equal volume of water droplets (approximately 5 μL) to the surface of each sample and record the contact angle data.

[0099] Repeated measurements: Perform 5 measurements on each sample and take the average value to reduce experimental error.

[0100] The comparative experimental data are shown in Table 1:

[0101] Table 1. Measurement results of water contact angle for each group of samples.

[0102]

[0103] From the data in Table 1, we can obtain:

[0104] The experimental data show that the average water contact angle of the modified calcium carbonate powder prepared in this invention (experimental group A) is 114.0°, significantly higher than that of the unmodified calcium carbonate powder (control group B) at 76.0°, indicating a significant improvement in hydrophobic properties. Compared with traditional titanate coupling agents (control group C, 98.0°) and aminosilane coupling agents (control group D, 88.0°), experimental group A also has a larger contact angle, showing superior hydrophobicity. This verifies the advantages of the modification process in this invention, effectively improving the performance of calcium carbonate powder in composite materials.

[0105] Comparative Experiment 2: Heat Resistance and Thermal Stability Test

[0106] Experimental objective: To evaluate the stability and heat resistance of the modified calcium carbonate powder-filled composite material prepared in this invention under high-temperature conditions through comparative tests of heat resistance and thermal stability.

[0107] Experimental setup

[0108] Experimental group:

[0109] Composite materials filled with modified calcium carbonate powder prepared according to the present invention.

[0110] Control group setup:

[0111] Control group 1: Calcium carbonate powder composite material without filler.

[0112] Control group 2: Composite material filled with calcium carbonate powder modified by traditional titanate coupling agent.

[0113] Control group 3: Composite material filled with traditional stearic acid modified calcium carbonate powder.

[0114] Experimental steps

[0115] Sample preparation: Each group of samples was prepared into composite material specimens of the same mass and volume to ensure the comparability of experimental results.

[0116] Thermogravimetric analysis:

[0117] Each group of samples was placed into the thermogravimetric analyzer (TGA) in sequence.

[0118] The temperature range was set from room temperature to 600℃, the heating rate was 10℃ / min, and the process was carried out under nitrogen protection.

[0119] During the test, the mass change curve of each sample with temperature was recorded, and the percentage of mass loss of each group was recorded at specific temperature points (such as 100℃, 300℃, and 500℃).

[0120] Data recording: Organize the data from each group into tables for subsequent analysis and comparison.

[0121] The comparative experimental data are shown in Table 2:

[0122] Table 2. Test results of heat resistance and thermal stability of composite materials

[0123]

[0124] From the data in Table 2, we can obtain:

[0125] The modified calcium carbonate powder-filled composite material (experimental group) prepared in this invention exhibits lower mass loss under high temperature conditions, demonstrating excellent thermal stability and heat resistance.

[0126] At 100℃, the mass loss of the experimental group was only 0.5%, which was significantly lower than the 1.0% of the unmodified calcium carbonate powder composite material (control group 1).

[0127] At high temperatures of 300℃ and 500℃, the mass loss of the experimental group was 2.1% and 7.8%, respectively, both significantly lower than that of the other control groups.

[0128] Comparative Experiment 3: Mechanical Property Testing of Composite Materials

[0129] Experimental objective: To evaluate the effect of the modified calcium carbonate powder prepared in this invention on improving the tensile strength, flexural strength and impact strength of composite materials by comparing the mechanical properties of different groups of composite materials.

[0130] Experimental setup

[0131] Experimental group:

[0132] Composite materials filled with modified calcium carbonate powder prepared according to the present invention.

[0133] Control group setup:

[0134] Control group 1: Composite material filled with unmodified calcium carbonate powder.

[0135] Control group 2: Composite material filled with calcium carbonate powder modified by traditional titanate coupling agent.

[0136] Control group 3: Composite material filled with calcium carbonate powder modified by traditional aminosilane coupling agent.

[0137] Experimental steps

[0138] Sample preparation: Each group of samples is prepared into composite material specimens of the same size and thickness to ensure that the results of mechanical property tests are comparable.

[0139] Mechanical property testing:

[0140] Tensile strength test: Tensile tests were performed on each group of samples using a universal testing machine, and the tensile strength at fracture was recorded.

[0141] Bending strength test: The bending strength of each group of samples was tested using a three-point bending test device.

[0142] Impact strength test: The impact strength of each group of samples was tested using an impact tester, and the energy absorption capacity of the material under impact was recorded.

[0143] Data recording: Record and organize the mechanical property data of each group into tables for comparative analysis.

[0144] The comparative experimental data are shown in Table 3:

[0145] Table 3. Measurement results of water contact angle for each group of samples.

[0146]

[0147]

[0148] From the data in Table 3, we can obtain:

[0149] The modified calcium carbonate powder-filled composite material (experimental group) prepared in this invention showed significant improvements in tensile strength, flexural strength, and impact strength. Specific results are as follows:

[0150] In the tensile strength test, the experimental group achieved a tensile strength of 58.2 MPa, which was higher than the 42.7 MPa of the unmodified powder-filled composite material (control group 1) and the composite material modified with traditional titanate coupling agent (control group 2) and aminosilane coupling agent (control group 3).

[0151] In the flexural strength and impact strength tests, the experimental group also achieved results of 82.5 MPa and 15.8 kJ / m, respectively. 2 The results showed significant advantages in mechanical properties, exceeding those of all control groups, thus verifying the innovative advantages of this invention in modified calcium carbonate powder technology and providing a strong scientific basis for its application in composite material reinforcement.

[0152] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. Process for the preparation of modified calcium carbonate powder, characterized in that, The method includes the following steps: S1. Surface pretreatment of calcium carbonate powder to remove surface impurities and increase surface activity, including ultrasonic cleaning of calcium carbonate powder in a solvent and then drying it. S2. Mix the pretreated calcium carbonate powder with one or more modifiers to allow the modifiers to be initially adsorbed onto the surface of the calcium carbonate powder. S3. Under specific temperature and stirring conditions, a chemical reaction is carried out to allow the modifier to adhere uniformly to the surface of the calcium carbonate powder, thereby enhancing the hydrophobicity, dispersibility and compatibility of the calcium carbonate powder with the substrate. S4. After the reaction is complete, place the modified calcium carbonate powder in a vacuum drying oven to dry it, so as to remove residual solvent and stabilize the surface modified layer. S5. Grind the dried modified calcium carbonate powder to control the powder particle size and specific surface area so that it meets the predetermined dispersibility and particle size requirements. S6. Disperse the ground modified calcium carbonate powder to avoid particle agglomeration and obtain modified calcium carbonate powder with uniform particle size distribution.

2. The method for producing a modified calcium carbonate powder according to claim 1, characterized by, Surface pretreatment includes the following steps: Calcium carbonate powder was placed in anhydrous ethanol solution and surface impurities were removed by ultrasonic cleaning at a frequency of 40 kHz, a power of 100 W, and a cleaning time of 10 minutes. The cleaned calcium carbonate powder was placed in a vacuum drying oven and dried at 65°C for 1 hour. The dried calcium carbonate powder was transferred to a nitrogen-protected vacuum drying oven and dried at 90°C for 2 hours to ensure that there was no moisture on the powder surface.

3. The method of producing modified calcium carbonate powder according to claim 1, characterized by, Preliminary adsorption involves stirring the pretreated calcium carbonate powder and the modifier at room temperature for 15 minutes to preliminarily adsorb the modifier.

4. The method of producing modified calcium carbonate powder according to claim 1, characterized by, A chemical reaction includes the following steps: The mixture was heated to 80°C and reacted for 30 minutes with a stirring speed of 700 rpm. The system was heated to 120°C and the reaction continued for 20 minutes. The stirring speed was set to 1000 rpm to ensure that the modifier was uniformly attached to the surface of the calcium carbonate powder.

5. The method of producing modified calcium carbonate powder according to claim 1, characterized by, Modifiers may be selected from the following: titanate coupling agents, aminosilane coupling agents, methacryloxysilane coupling agents, and stearic acid.

6. The method of producing modified calcium carbonate powder according to claim 1, characterized by, Drying includes the following steps: The modified calcium carbonate powder was dried in a vacuum drying oven at 80°C for 2 hours to remove residual solvent. The dried powder was transferred to a nitrogen-protected vacuum drying oven at 100°C and dried for another hour to ensure the stability of the surface modified layer.

7. The method of producing modified calcium carbonate powder according to claim 1, characterized by, Grinding involves using an air jet mill to control the powder particle size to below 5 micrometers in order to obtain an ideal particle size distribution.

8. The method of producing modified calcium carbonate powder according to claim 1, characterized by, The dispersion process involves adding the ground powder to anhydrous ethanol and using an ultrasonic disperser at a frequency of 60 kHz and a power of 200 W for 15 minutes to reduce agglomeration and obtain modified calcium carbonate powder with a uniform particle size distribution.

9. The method of producing modified calcium carbonate powder according to claim 1, characterized by, The method also includes a solvent recovery step, in which the solvent after the chemical reaction of S2 and S3 is recovered by distillation and condensation devices, so that the solvent recovery rate reaches more than 90% and is used in the preparation process of the next batch.

10. Use of modified calcium carbonate powder in a composite material, characterized in that, The method for preparing modified calcium carbonate powder according to any one of claims 1-9 includes: The product is used in plastics, rubber, or coatings to improve the hydrophobicity, mechanical strength, and thermal stability of composite materials.