Underwater diatom self-repairing coating and preparation method thereof

By combining an alkali-resistant crescent-shaped algae with a magnesium phosphate cement matrix and alginate microspheres, along with intelligent responsive additives and buffers, the survival and release issues of underwater diatom self-healing coatings in extreme environments were solved, achieving highly efficient underwater repair effects.

CN123152318APending Publication Date: 2026-11-24QINGDAO UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611584139.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing underwater diatom self-healing coatings have low diatom survival rates in extreme hydration environments, and delayed release leads to accelerated corrosion. Furthermore, the lack of targeted control affects repair efficiency and long-term durability.

Method used

By employing a combination of magnesium phosphate cement matrix, alkaline-resistant crescent-shaped diatoms encapsulated with alginate microspheres, intelligent responsive additives, sodium citrate buffers, and inert mineral fillers, the on-demand release and protection of diatoms can be achieved by adjusting the local reaction environment and rheological state.

Benefits of technology

It improves the survival rate of diatoms in extreme hydration environments, ensures the repair effect of cracked areas, has early hardening ability and resistance to chloride ion penetration, and enhances the adhesion strength and repair efficiency of underwater repair layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152318A_ABST
    Figure CN123152318A_ABST
Patent Text Reader

Abstract

This application provides an underwater diatom self-healing coating and its preparation method. The coating comprises the following components in parts by weight: 40-60 parts of magnesium phosphate cement matrix, 3-8 parts of alkaline-resistant crescent-shaped rhomboid algae encapsulated with alginate microspheres, 1-5 parts of smart responsive additive, 15-30 parts of sodium citrate buffer, 0.5-2 parts of anti-washout agent, and 5-10 parts of inert mineral filler. The smart responsive additive is a pH-sensitive polymer. The coating has early hardening ability, underwater repair ability, and resistance to chloride ion penetration. The preparation method involves pre-mixing the magnesium phosphate cement matrix, sodium citrate buffer, smart responsive additive, anti-washout agent, and inert mineral filler, adding them to a mixing liquid, mechanically stirring, then vacuum degassing the slurry, and finally adding the alkaline-resistant crescent-shaped rhomboid algae encapsulated with alginate microspheres using a low-speed paddle stirring method, thus achieving a gentle composite of diatom microspheres and cement matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of marine engineering materials technology, and in particular to an underwater diatom self-healing coating and its preparation method. Background Technology

[0002] Coastal / underwater concrete structures that have been used for a long time may develop cracks due to the marine environment or wet-dry cycles. Bio-healing materials, with their self-repairing, long-lasting corrosion resistance, and underwater compatibility, can be used to repair these cracks. Bio-healing materials are mainly classified according to the type of living organism they contain: bacterial self-healing materials (such as Bacillus), fungal self-healing materials (such as Neurospora crassa), and algal self-healing materials (such as diatoms).

[0003] Existing underwater diatom self-healing coatings (such as systems based on magnesium phosphate cement and alginate microspheres) can achieve the protection and release of diatoms, but the release process depends on the external environment (such as water / light) and lacks specificity. Diatoms may be released prematurely before concrete cracks appear or in a stable environment, leading to wasted activity and low repair efficiency. Furthermore, in complex marine environments, delayed release after crack formation may exacerbate corrosion. Current technologies have not solved the problem of "on-demand" control of diatom release, limiting the long-term durability and precise repair accuracy of the coatings.

[0004] More critically, introducing live microorganisms or diatoms directly into cementitious substrates presents a severe survival rate problem. *Nitzschia closterium*, a typical marine diatom, has an optimal growth pH range of 7.5–8.5 and an optimal temperature range of 15–20°C; it ceases growth and reproduction above 25°C. When *Nitzschia closterium* is introduced into cementitious substrates, the pH changes drastically from acidic to alkaline during the cement hydration stage, releasing a large amount of heat of hydration. *Nitzschia closterium* encapsulated within the cement substrate is easily killed in large numbers under the combined effects of this pH change and high heat, severely weakening the actual biomineralization remediation effect.

[0005] Therefore, there is an urgent need to develop a new type of diatomaceous earth coating that can effectively ensure the survival of living diatoms in extreme hydration environments and has excellent underwater intelligent triggering performance, in order to meet the growing demand for long-term restoration in marine engineering. Summary of the Invention

[0006] The purpose of this application is to provide an underwater diatom self-healing coating and its preparation method, so as to solve or alleviate the problems existing in the prior art.

[0007] To achieve the above objectives, this application provides the following technical solution: An underwater diatom self-healing coating comprises the following components in parts by weight: 40-60 parts magnesium phosphate cement matrix, 3-8 parts alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, 1-5 parts smart responsive additive, 15-30 parts sodium citrate buffer, 0.5-2 parts anti-washout agent, and 5-10 parts inert mineral filler; wherein the smart responsive additive is a pH-sensitive polymer.

[0008] Magnesium phosphate cement matrix features rapid setting and hardening, high early strength, and good interfacial adhesion, which facilitates the rapid formation of a repair layer with sufficient strength after underwater application. Sodium citrate buffers regulate the local reaction environment and delay the early hydration reaction of magnesium phosphate cement, while inert mineral fillers utilize their own heat capacity and particle dispersion to mitigate local heat accumulation. By using sodium citrate buffers, hydroxypropyl methylcellulose, and anti-washout agents to regulate the setting process and rheological properties of the magnesium phosphate cement matrix, the coating maintains necessary workability, water resistance, and adhesion to damp substrates within the specified application time. Smart-responsive additives exhibit different ionization states under different pH conditions, allowing their dispersion and swelling behavior to change with the local pH environment, thus regulating the local rheological state and mass transport processes within the coating. The smart-responsive additives, when used in conjunction with alkali-resistant crescent-shaped algae encapsulated in alginate microspheres, provide favorable conditions for the migration of moisture and repair-related substances within the crack area, but do not directly limit the targeted release of diatoms. The release of diatom microspheres is achieved by the destruction of the alginate microsphere shell after the repair layer cracks or by communication with the external aquatic environment.

[0009] Furthermore, the alkali-resistant crescent-shaped algae encapsulated in the alginate microspheres is prepared by the following method: Alkali-tolerant rhomboid algae were dispersed in simulated seawater to obtain a diatom dispersion; sodium alginate solution was prepared. Using the diatom dispersion as the inner phase and the sodium alginate solution as the outer phase, droplets of the outer phase covering the inner phase are formed by a coaxial dropping device and dropped into a calcium lactate crosslinking solution at 5-15℃ for 1-5 minutes to form core-shell microspheres with an inner phase containing alkali-resistant crescent-shaped algae as the core layer and calcium alginate gel as the shell layer. The core-shell microspheres are washed and filtered to obtain alkali-resistant crescent-shaped algae encapsulated in alginate microspheres, which are then individually sealed and stored at 2-8℃ for later use.

[0010] The dry weight ratio of sodium alginate to the alkali-tolerant crescent-shaped algae is 2:1 to 4:1.

[0011] Furthermore, the alkaline-tolerant *Nyctaginata* was gently stirred at 50–150 r / min for 5–15 min at 5–15 °C to disperse in simulated seawater. The mass fraction of *Nyctaginata* in the diatom dispersion was 0.5 wt%–2 wt%, and the mass fraction of the sodium alginate solution was 1.5 wt%–3 wt%. The cross-linked core-shell microspheres were immediately washed 2-3 times with the isotonic seawater buffer solution and collected by filtration through a sieve to obtain alkali-resistant rhomboid algae encapsulated in wet alginate microspheres for later use.

[0012] Furthermore, the simulated seawater was prepared from six salts—sodium chloride, magnesium chloride hexahydrate, sodium sulfate, calcium chloride, potassium chloride, and sodium bicarbonate—and water. The proportions of sodium chloride, magnesium chloride hexahydrate, sodium sulfate, calcium chloride, potassium chloride, and sodium bicarbonate in the total mass of the salts were 58.72%, 26.57%, 9.79%, 2.78%, 1.66%, and 0.48%, respectively. The total salt concentration of the simulated seawater was 35 g / L.

[0013] Furthermore, the intelligent response additive is polyacrylic acid micro powder containing a retarder, and its preparation steps are as follows: dispersing polyacrylic acid in simulated seawater, adding a retarder, and stirring evenly to obtain a spray-dried liquid, wherein the mass ratio of polyacrylic acid, simulated seawater and retarder is 1:(10-20):(0.03-0.10); the retarder is selected from one or more of boric acid, borax, citric acid and citrate. The spray-dried liquid is spray-dried to obtain polyacrylic acid micro powder containing a retarder; the median particle size D50 of the polyacrylic acid micro powder containing the retarder is 10-50 μm.

[0014] Furthermore, the inert mineral filler is composed of quartz sand and fine sand; the mass ratio of quartz sand to fine sand is (2-4):1.

[0015] Furthermore, the magnesium phosphate cement matrix is ​​prepared by the following method: Low-activity magnesium oxide, potassium dihydrogen phosphate, hydroxypropyl starch, hydroxypropyl methylcellulose and sodium citrate with activity values ​​of 40-60s were dried and sieved respectively. The low-activity magnesium oxide and potassium dihydrogen phosphate are added to a dry powder mixing device and dry-mixed at 15-30°C for 1-3 minutes. Add the hydroxypropyl starch, hydroxypropyl methylcellulose and sodium citrate, and continue dry mixing for 2-5 minutes to obtain a uniform magnesium phosphate cement dry powder matrix; The mass percentages of potassium dihydrogen phosphate, hydroxypropyl starch, hydroxypropyl methylcellulose, and sodium citrate are 20%–30%, 5%–10%, 2%–4%, and 10%–15% of the mass of the low-activity magnesium oxide, respectively.

[0016] Furthermore, the sodium citrate buffer is prepared by the following steps: Citric acid was added to deionized water and stirred to form an aqueous citric acid solution. Sodium carbonate was added in batches to the aqueous citric acid solution at 20–40°C with stirring. After the carbon dioxide bubbles basically stopped escaping, stirring was continued for 20–60 minutes to obtain a sodium citrate reaction solution. The molar ratio of citric acid to sodium carbonate was 1:(1.45–1.55), and the final pH of the reaction was 7.5–9.0. The sodium citrate reaction solution was filtered to remove insoluble matter and concentrated under reduced pressure at a temperature not exceeding 65°C to achieve a concentration of 285–570 g / L based on anhydrous sodium citrate. Ethanol is added to the concentrated sodium citrate solution to induce crystallization. The volume ratio of the concentrated sodium citrate solution to ethanol is 1:(3-5). The solution is stirred or allowed to stand at 20-30°C for 1-4 hours to crystallize. The precipitated crystals were filtered, washed 1-2 times with low-temperature ethanol, and vacuum dried to constant weight at 40-60°C to obtain white sodium citrate powder, which is the sodium citrate buffer.

[0017] This application also proposes a method for preparing the aforementioned underwater diatom self-healing coating, characterized by comprising the following steps: S1. Under conditions of 15-25℃, the magnesium phosphate cement matrix, sodium citrate buffer, smart response additive, anti-washing agent and inert mineral filler are mixed to obtain a premix. S2. Add mixing liquid to the premix and mechanically stir to obtain a uniform magnesium phosphate cement paste; S3. Vacuum degassing is performed on the magnesium phosphate cement slurry, and the temperature of the degassed magnesium phosphate cement slurry is controlled at no higher than 25°C. S4. Add alkali-resistant crescent-shaped algae encapsulated with alginate microspheres to the defoamed magnesium phosphate cement slurry, and mix evenly using a low-speed paddle stirring method to obtain the underwater diatom self-healing coating.

[0018] Furthermore, in step S2, the mechanical stirring speed is 300-600 r / min, and the stirring time is 1-3 min; in step S3, the vacuum degassing time is 1-3 min; in step S4, when adding alkali-resistant crescent-shaped algae encapsulated with alginate microspheres, the temperature of the magnesium phosphate cement slurry is 15-25℃, the speed of the low-speed paddle stirrer is 50-150 r / min, and the stirring time is 1-3 min.

[0019] This application also proposes the application of an underwater diatom self-healing coating, as described above, in the repair of concrete in offshore engineering projects.

[0020] The technical solution of this application has the following beneficial effects: This application uses calcium alginate core-shell microspheres to encapsulate alkali-resistant rhomboid algae, creating a physical barrier between the diatom cells and the magnesium phosphate cement matrix. This reduces the direct impact of ion concentration changes, local pH fluctuations, and mechanical shearing during the matrix hydration process on the diatom cells, ensuring their activity. When microcracks appear in the repair layer and part of the calcium alginate microsphere shell is damaged, the diatoms and their siliceous shells can enter or remain in the crack area, providing a carrier for the physical filling of the cracks and the subsequent deposition of repair materials, thereby improving the crack sealing effect of the repair layer. Under the underwater construction performance test conditions of this application, the initial setting time of the coating is 13–18 min, with the initial setting time of Example 2 being 15 min. Under the corresponding test conditions and specified age, the adhesion strength of the underwater repair layer can reach a maximum of 3.5 MPa, and the chloride ion diffusion coefficient can reach a minimum of 1.2 × 10⁻⁶. -12 The m² / s indicates that the coating possesses early hardening capability, underwater repair capability, and resistance to chloride ion penetration.

[0021] The preparation method of this application involves pre-mixing magnesium phosphate cement matrix, sodium citrate buffer, smart responsive additive, anti-washing agent, and inert mineral filler, then adding them to a mixing liquid for mechanical stirring. The slurry is then vacuum degassed while the temperature is controlled to not exceed 25°C. Finally, alkali-resistant crescent-shaped algae encapsulated in alginate microspheres are added using a low-speed paddle stirring method, achieving a gentle composite of diatom microspheres and the cement matrix. This process pre-completes steps that could adversely affect diatom activity, such as high-shear mixing and vacuum degassed, and avoids direct damage to the diatom microspheres from high temperatures, ultrasonic cavitation, vacuum environments, and high shear forces through temperature control and low-speed stirring. This helps reduce the risk of premature microsphere rupture and decreased diatom activity, thus providing a process guarantee for the survival and subsequent self-healing function of the alkali-resistant crescent-shaped algae in the magnesium phosphate cement matrix. Attached Figure Description

[0022] Figure 1 The image shows the SEM microstructure of the hardened coating in Example 2 of this invention.

[0023] Figure 2 This is a super-depth-of-field microscope image of alginic acid microspheres encapsulating alkali-resistant rhomboid algae in Example 2 of the present invention. Detailed Implementation

[0024] The present application will now be described in detail with reference to the accompanying drawings and embodiments. Various examples are provided by way of explanation and not by way of limitation. In fact, those skilled in the art will recognize that modifications and variations can be made to the present application without departing from the scope or spirit thereof. For example, a feature shown or described as part of one embodiment may be used in another embodiment to produce yet another embodiment. Therefore, it is desirable that the present application encompass such modifications and variations that fall within the scope of the appended claims and their equivalents.

[0025] The main raw materials used in the following embodiments are as follows: Low-activity magnesium oxide is lightly calcined magnesium oxide with an activity value of 50s; the alkali-tolerant *Nyctaginus crescentis* used in this application is an algae species that has undergone alkali-tolerant domestication, exhibiting stronger adaptability to alkaline environments compared to ordinary *Nyctaginus crescentis*, and maintaining a certain level of activity even under alkaline conditions of pH 9.0–10.0; the intelligent response additive is polyacrylic acid micropowder containing a retarder, wherein the retarder is sodium tetraborate decahydrate; the anti-washout agent is xanthan gum; hydroxypropyl methylcellulose is construction-grade HPMC; sodium alginate is a commercially available product with a purity of not less than 98%; all reagents not specifically mentioned are chemically pure reagents. The quartz sand particle size is 0.5–1 mm, and the fine sand particle size is 0.1–1 mm.

[0026] Example 1 An underwater diatom self-healing coating comprises the following components in parts by weight: 40 parts magnesium phosphate cement matrix, 3 parts alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, 1 part intelligent response additive, 15 parts sodium citrate buffer, 0.5 parts anti-washout agent, and 5 parts inert mineral filler, wherein the inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 2:1; the alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres is measured by the mass of the wet microspheres collected through a sieve and drained until no droplets fall within 5 minutes.

[0027] The preparation method of magnesium phosphate cement matrix is ​​as follows: Low-activity magnesium oxide, potassium dihydrogen phosphate, hydroxypropyl starch, hydroxypropyl methylcellulose and sodium citrate with an activity value of 50s were dried and sieved respectively. By weight, 100 parts of low-activity magnesium oxide and 30 parts of potassium dihydrogen phosphate were added to a dry powder mixing device at 20-25°C and dry-mixed for 2 minutes. Then, 5 parts of hydroxypropyl starch, 2 parts of hydroxypropyl methylcellulose and 10 parts of sodium citrate were added and dry-mixed for another 3 minutes to obtain a uniform magnesium phosphate cement dry powder matrix. The obtained magnesium phosphate cement dry powder matrix was sealed and stored for later use.

[0028] The preparation method of the intelligent response additive is as follows: Polyacrylic acid was dispersed in simulated seawater, and sodium tetraborate decahydrate was added as a retarder; wherein the mass ratio of polyacrylic acid, simulated seawater and sodium tetraborate decahydrate was 1:15:0.05, and the mixture was stirred at 25°C for 30 min to obtain a uniform spray-dried liquid. The obtained liquid material was spray-dried, and by adjusting the feed rate and atomization conditions, the median particle size D50 of the obtained polyacrylic acid micro powder was made to be about 30 μm, thus obtaining a smart response additive.

[0029] The simulated seawater had a total salt concentration of 35 g / L, with sodium chloride, magnesium chloride hexahydrate, sodium sulfate, calcium chloride, potassium chloride, and sodium bicarbonate accounting for 58.72%, 26.57%, 9.79%, 2.78%, 1.66%, and 0.48% of the total salt mass, respectively.

[0030] Alkali-resistant crescent-shaped algae encapsulated in alginate microspheres were prepared using the following steps: Alkali-tolerant rhomboid algae were added to simulated seawater and gently stirred at 100 r / min for 10 min at 10℃ to obtain a diatom dispersion. The mass fraction of alkali-tolerant rhomboid algae in the diatom dispersion was 0.5 wt%. A sodium alginate solution with a mass fraction of 2.0 wt% was prepared separately. Using the diatom dispersion as the inner phase and sodium alginate solution as the outer phase, droplets with the outer phase coating the inner phase are formed by a coaxial dropping device. The resulting droplets are then dropped into a 1.0 wt% calcium lactate crosslinking solution and crosslinked at 10°C for 3 min. The dry weight ratio of sodium alginate to alkaline-tolerant rhomboid algae is 2:1. Core-shell microspheres containing an alkaline-tolerant rhomboid algae liquid inner core and a calcium alginate gel shell are formed. After cross-linking, the sample was immediately washed three times with isotonic seawater buffer solution, and then filtered through a 1mm to 1.4mm sieve to collect and remove the surface free liquid. The sample was then sealed and stored separately in a wet state at 4°C. The isotonic seawater buffer solution was an aqueous solution with the same salt composition and total salt concentration as the simulated seawater, and the pH was controlled at 7.8 to 8.2.

[0031] Sodium citrate buffers are prepared using the following steps: Citric acid was added to deionized water and stirred to form an aqueous citric acid solution. Sodium carbonate was added in batches at 30°C with stirring. The molar ratio of citric acid to sodium carbonate was 1:1.50. After the carbon dioxide bubbles basically stopped escaping, stirring was continued for 30 minutes. The pH of the reaction endpoint was controlled at 7.5-9.0 to obtain a sodium citrate reaction solution. The reaction solution was filtered to remove insoluble matter, and then concentrated under reduced pressure at a temperature not exceeding 60°C to achieve a concentration of approximately 400 g / L based on anhydrous sodium citrate. Ethanol was added to the concentrate at a volume ratio of 1:4. The mixture was allowed to stand at 25°C for 2 hours to crystallize. The white sodium citrate crystals were collected by filtration, washed twice with low-temperature ethanol, and dried under vacuum at 50°C to constant weight to obtain a sodium citrate buffer.

[0032] A method for preparing an underwater diatom self-healing coating includes the following steps: S1. Under 20°C conditions, the magnesium phosphate cement matrix, sodium citrate buffer, smart response additive, anti-washing agent and inert mineral filler are added to a mixing device and dry-mixed until the components are evenly distributed to obtain a premix. S2. Add mixing liquid to the premixed material and mechanically stir at 400 r / min for 2 min to obtain a uniform magnesium phosphate cement slurry; the mixing liquid is deionized water, and the amount of mixing liquid is 30% of the mass of the dry magnesium phosphate cement matrix powder; S3. Vacuum degas the magnesium phosphate cement slurry for 2 minutes, and control the temperature of the degassed magnesium phosphate cement slurry to be no higher than 25℃. S4. Add alkali-resistant crescent-shaped algae encapsulated with alginate microspheres to the defoamed and cooled magnesium phosphate cement slurry to 20-25℃. Mix evenly using a low-speed paddle mixer at 100r / min for 2min to obtain the underwater diatom self-healing coating.

[0033] Example 2 An underwater diatom self-healing coating comprises the following components in parts by weight: 50 parts magnesium phosphate cement matrix, 5 parts alkali-resistant crescent-shaped algae encapsulated with alginate microspheres, 3 parts intelligent response additive, 22 parts sodium citrate buffer, 1 part anti-washout agent, and 7 parts inert mineral filler. The inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 3:1. The alkali-resistant crescent-shaped algae encapsulated with alginate microspheres is weighed in the same way as in Example 1. Alkali-resistant crescent-shaped algae encapsulated in alginate microspheres were prepared using the following steps: The diatom dispersion was prepared according to the steps of Example 1, but the mass fraction of alkali-tolerant Rhizophora crescentis in the diatom dispersion was 1.0 wt%; a sodium alginate solution with a mass fraction of 2.0 wt% was prepared. Crosslinking was performed according to the steps of Example 1, but the dry mass ratio of sodium alginate to alkali-tolerant rhomboid algae was 3:1; core-shell microspheres containing a liquid inner core of alkali-tolerant rhomboid algae and a calcium alginate gel shell were formed; subsequent steps after crosslinking were the same as in Example 1.

[0034] The components and preparation steps of the magnesium phosphate cement matrix, smart response additive, sodium citrate buffer, and anti-washout agent in this embodiment are the same as in Example 1.

[0035] The underwater diatom self-healing coating prepared in this embodiment was applied to the surface of a concrete substrate. After underwater curing, a hardened coating was formed. Samples were taken on the 28th day of underwater curing for SEM microscopic morphology observation. The results are as follows: Figure 1 As shown. Figure 2 This is a super depth-of-field microscope image of alginic acid microspheres encapsulating alkali-resistant rhomboid algae in Example 2 of the present invention. The microspheres encapsulate multiple green alkali-resistant rhomboid algae cells. Figure 1 A long, strip-like structure can be observed. Based on the *Rhizophora crescentis* material used and its morphological characteristics (the siliceous shell of *Rhizophora crescentis* has a narrow, spindle-shaped to linear surface), it is inferred that this structure belongs to *Rhizophora crescentis*. Figure 1 No complete alginate microsphere structure was clearly observed in the field of view. This is mainly because calcium alginate is a hydrophilic gel with high water content and limited mechanical strength. During the 28-day underwater curing period, calcium alginate continued to swell, the shell structure loosened, and some calcium alginate was converted into sodium alginate and dissolved, thus disrupting the integrity of the shell. Simultaneously, hydration products of magnesium phosphate cement deposited and grew on and around the microspheres. Figure 1 A clear spherical boundary cannot be observed. Figure 1 , Figure 2 This indicates that the alginate microspheres act as a temporary protective carrier during mixing and underwater curing, gradually breaking down or dissolving and releasing alkali-resistant crescent-shaped algae, which are then dispersed in the hardened coating. Figure 1 The spatial distribution of alkali-tolerant crescent-shaped algae is uneven, with multiple alkali-tolerant crescent-shaped algae overlapping and aggregating in some areas, which is speculated to be alkali-tolerant crescent-shaped algae released from the same alginate microsphere.

[0036] The preparation method of the underwater diatom self-healing coating in this embodiment is the same as in Embodiment 1.

[0037] Example 3 An underwater diatom self-healing coating comprises the following components in parts by weight: 60 parts magnesium phosphate cement matrix, 8 parts alkali-resistant crescent-shaped algae encapsulated with alginate microspheres, 5 parts intelligent response additive, 30 parts sodium citrate buffer, 2 parts anti-washout agent, and 10 parts inert mineral filler. The inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 4:1. The alkali-resistant crescent-shaped algae encapsulated with alginate microspheres is weighed in the same manner as in Example 1. Alkali-resistant crescent-shaped algae encapsulated in alginate microspheres were prepared using the following steps: The diatom dispersion was prepared according to the steps of Example 1, but the mass fraction of alkali-tolerant rhomboid algae in the diatom dispersion was 2.0 wt%; a sodium alginate solution with a mass fraction of 2.0 wt% was prepared. Crosslinking was performed according to the steps of Example 1, but the dry mass ratio of sodium alginate to alkali-tolerant rhomboid algae was 4:1; core-shell microspheres containing a liquid inner core of alkali-tolerant rhomboid algae and a calcium alginate gel shell were formed; subsequent steps after crosslinking were the same as in Example 1.

[0038] The components and preparation steps of the magnesium phosphate cement matrix, smart response additive, sodium citrate buffer, and anti-washout agent in this embodiment are the same as in Example 1.

[0039] The preparation method of the underwater diatom self-healing coating in this embodiment is the same as in Embodiment 1.

[0040] Comparative Example 1 The only difference between this comparative example and Example 2 is that the amount of alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres was increased from 5 parts to 15 parts. All other components and preparation conditions were the same as in Example 2. This example was used to investigate the effect of excessive alginate microsphere addition on the coating's application performance, underwater interface performance, and post-treatment self-healing performance.

[0041] The underwater diatom self-healing coating of this embodiment includes the following components in parts by weight: 50 parts magnesium phosphate cement matrix, 15 parts alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, 3 parts smart response additive, 22 parts sodium citrate buffer, 1 part anti-washout agent, and 7 parts inert mineral filler, wherein the inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 3:1.

[0042] Comparative Example 2 The only difference between this comparative example and Example 2 is that ordinary phosphate buffer is used to replace sodium citrate buffer in equal amounts, with an addition amount of 22 parts. All other components and preparation conditions are the same as in Example 2. This example is used to investigate the effects of different buffering systems on the maintenance of diatom activity, underwater interface performance, and subsequent self-healing performance.

[0043] The underwater diatom self-healing coating of this embodiment includes the following components in parts by weight: 50 parts magnesium phosphate cement matrix, 5 parts alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, 3 parts smart response additive, 22 parts ordinary phosphate buffer, 1 part anti-washout agent, and 7 parts inert mineral filler, wherein the inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 3:1.

[0044] Comparative Example 3 Compared with Example 2, this comparative example does not contain hydroxypropyl methylcellulose in the magnesium phosphate cement matrix.

[0045] An underwater diatom self-healing coating comprises the following components in parts by weight: 50 parts magnesium phosphate cement matrix, 5 parts alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, 3 parts intelligent response additive, 22 parts sodium citrate buffer, 1 part anti-washout agent, and 7 parts inert mineral filler, wherein the inert mineral filler is composed of quartz sand and fine sand in a mass ratio of 3:1; the magnesium phosphate cement matrix comprises 100 parts low-activity magnesium oxide, 30 parts potassium dihydrogen phosphate, 5 parts hydroxypropyl starch, and 10 parts sodium citrate.

[0046] Comparative Example 4 This comparative example does not contain inert mineral fillers compared to Example 2.

[0047] Comparative Example 5 The only difference from Example 2 is that it does not contain smart response additives.

[0048] Comparative Example 6 The only difference from Example 2 is that the active alkali-resistant rhomboid algae in the alginate microspheres are replaced with an equal amount of inactivated rhomboid algae.

[0049] Experimental Example To verify the application performance, diatom activity protection effect, reaction environment regulation effect, and underwater repair performance of the underwater diatom self-healing coating of this application, tests were conducted on Examples 1-3 and each comparative example. Test items included initial setting time, underwater adhesion strength, chloride ion transport performance, hydration temperature rise, early pH change, underwater spread, diatom microsphere integrity, diatom culturable survival rate, pH response performance, crack repair performance, morphology and composition of crack repair products, and long-term underwater service performance. Each test group had at least three parallel specimens, and the test results are expressed as mean and standard deviation.

[0050] (1) Integrity test of alginate microspheres: Samples were taken after the alginate microspheres were prepared, after the magnesium phosphate cement slurry was added in step S4 and low-speed stirring was completed, and after the coating was applied and hardened underwater for 1 day. The microspheres were observed using an optical microscope, with at least five fields of view randomly selected. The number of intact microspheres and the total number of microspheres were counted. The average particle size, shell continuity, and presence of cracks, collapses, or significant deformation of the microspheres were also recorded.

[0051] The formula for calculating the integrity rate of microspheres is: Microsphere integrity rate / % = Number of intact microspheres / Total number of observed microspheres × 100%.

[0052] The results of the integrity test of alginate microspheres are shown in Table 1: Table 1 Results of integrity test for alginate microspheres

[0053] By comparing the microsphere integrity rates at different stages, the protective effect of the low-temperature, low-speed stirring, and post-addition microsphere process on the alginate core-shell microsphere structure of this application can be evaluated. The results show that the integrity rates of the microspheres prepared in Examples 1-3 are all above 96.5%, proving the feasibility of the alginate microsphere preparation method of this application. After 2 minutes of low-speed paddle stirring at 100 r / min in step S4, the integrity rate only slightly decreased, still maintaining a high integrity rate of 92.8%–94.1%, proving that the calcium alginate gel shell has sufficient mechanical strength to resist the mild shearing action during coating preparation. The integrity rate results after 1 day of underwater hardening indicate that the alginate microspheres have good structural stability in the hydration of magnesium phosphate cement and in the underwater environment. The average particle size of the microspheres slightly increases with the increase of diatom content and sodium alginate ratio, indicating that the formulation adjustment affects the microsphere moldability.

[0054] (2) Survival rate test of alkaline-tolerant rhomboid algae at different stages: To verify the retention of the activity of alkali-resistant crescent-shaped algae during the preparation process of this application, the survival rate of raw diatoms, diatoms prepared into alginate microspheres, diatoms after adding coating, and diatoms after 1 day, 7 days, and 28 days of underwater construction and hardening were tested.

[0055] Diatoms were detected using a live / dead cell fluorescence staining method. For raw diatoms and microsphere samples, live / dead cell staining was performed directly. For hardened coated specimens, the specimens were cut to expose the diatom-containing microsphere area, and the number of live and dead cells was observed and counted under a fluorescence microscope or confocal microscope. At least five fields of view were randomly selected from each group for counting. The diatom survival rate was calculated using the following formula: Diatom survival rate / % = Number of live diatom cells / (Number of live diatom cells + Number of dead diatom cells) × 100%.

[0056] The test results are shown in Table 2: Table 2. Survival rate test results of alkaline-tolerant *Nyctaginea crescentis* at different stages

[0057] The above test results were used to evaluate the protective effects of alginate microsphere encapsulation, sodium citrate buffer system, inert mineral filler, and post-microsphere addition process on diatom activity (the data in the first two columns of Comparative Examples 1-5 are consistent with Example 2 because the alkaline-resistant *Rhizoctonia solani* encapsulated with alginate microspheres from Example 2 was used). Comparative Example 6 used inactivated *Rhizoctonia solani* as a negative control to determine the contribution of live diatoms to the later repair process. The results showed that as the coating preparation process progressed, the diatom survival rate gradually decreased, but the decrease was controllable. After coating preparation, all examples showed a diatom survival rate of over 86%. Comparative Examples 2 and 4 showed a significant decrease in survival rate after coating preparation, indicating that if microspheres are dry-mixed with other components simultaneously or conventional high-speed stirring is used, it will cause microsphere rupture and diatom death. During underwater hardening from 1 to 28 days, the survival rate of the alkaline-resistant *Rhizoctonia solani* in Examples 1-3 was over 64%, indicating that the sodium citrate buffer system was effective, and the calcium alginate shell also delayed the OH- oxidative stress. - and Mg 2+ Plasma penetration into cells allows diatoms to survive and adapt inside hardened cement. Example 2 is the preferred embodiment, illustrating that the diatom loading and the proportion of a thicker shell achieve the optimal balance between nutrient supply and mechanical protection.

[0058] Comparative Example 2, by replacing the sodium citrate-type buffer with a regular buffer, failed to effectively utilize ion exchange and synergistic neutralization. This resulted in the instantaneous high alkalinity during the early stages of magnesium phosphate cement hydration, directly damaging the diatom cell walls. The living diatoms suffered severe "alkali poisoning," leading to extremely low survival rates and hindering subsequent effective biomineralization, significantly reducing impermeability. Comparative Example 4, lacking the synergistic effect of inert mineral fillers, prevented the timely absorption of the large amount of latent heat of hydration generated during the magnesium phosphate cement system's hydration process. This caused a rapid increase in local microenvironment temperature above the diatoms' tolerance limit, resulting in severe "thermal-induced denaturation and death" of the living diatoms. The survival rate plummeted, greatly weakening the coating's self-healing activity. Comparative Example 5 demonstrates that the intelligent response additive, through swelling to create a high-viscosity microenvironment, provides some auxiliary protection for diatoms, but is not a decisive factor.

[0059] (3) pH response performance test of smart response additives: To verify the pH response performance of polyacrylic acid micropowder containing retarder, the liquid absorption and swelling performance of the smart responsive additive used in the examples was tested under different pH conditions.

[0060] A solution with the same salt composition as the simulated seawater in this application was used, adjusted to different pH conditions, and the same mass of the smart response additive was added to each solution. The samples were then treated at the same temperature and for the same duration. Subsequently, the samples were separated, and the mass before and after liquid absorption was measured. The liquid absorption swelling rate was calculated using the following formula: Swelling rate / % = (mass after liquid absorption - initial dry mass) / initial dry mass × 100%.

[0061] Meanwhile, the apparent viscosity or flow properties of the slurries obtained in Example 2 and Comparative Example 5 without the smart response additive were compared under different pH conditions to evaluate the ability of the smart response additive to regulate the local rheological state.

[0062] The test results are shown in Table 3: Table 3. pH response performance test results of smart responsive additives

[0063] Table 3 shows that the swelling ratio of the intelligent responsive additive first increases and then decreases with increasing pH, reaching a peak of 240% at pH 8.5, indicating that the polyacrylic acid micropowder has obvious pH-responsive characteristics. In the alkaline environment during the initial hydration of magnesium phosphate cement, the additive still exhibits a high swelling ratio, while its swelling capacity is strongest under neutral to weakly alkaline conditions, indicating that it can sense and respond to local pH changes in the slurry. The viscosity of the slurry in Comparative Example 5 remained essentially unchanged with pH. Compared to Comparative Example 5, the apparent viscosity of the slurry in Example 2 changed significantly with pH, ​​and was higher than that in Comparative Example 5 under all pH conditions, especially at pH 8.5 where the viscosity increase was the greatest. This demonstrates that the additive effectively regulates the local rheological state of the slurry through swelling, forming a high-viscosity microenvironment around the microspheres, which is beneficial for delaying material transport and providing buffer protection for diatoms.

[0064] (4) To evaluate the underwater application performance and basic performance of the coating after the formation of the repair layer, the initial setting time, underwater spread, underwater adhesion strength, and chloride ion transport performance of the above-mentioned examples and comparative examples were tested. The initial setting time and underwater spread were tested according to the method specified in DL / T 5117-2021 "Test Procedure for Underwater Non-Dispersible Concrete"; the underwater adhesion strength was tested according to the tensile bond strength test method in JC / T 907-2018 "Concrete Interface Treatment Agent", with the tensile bond strength after underwater curing at the corresponding age characterizing the underwater adhesion performance; the chloride ion diffusion coefficient was tested according to the rapid chloride ion migration coefficient method (RCM method) in GB / T 50082-2024 "Standard for Test Methods of Long-Term Performance and Durability of Concrete". Each group had at least three parallel specimens, and the test results are shown in Table 4. Table 4. Test Results of Basic Performance of Underwater Construction and Repair Layer

[0065] Table 4 shows that the coatings in this application possess both suitable underwater construction performance and excellent physical properties of the repair layer. The initial setting time of each embodiment is 13–18 min, meeting the requirements for rapid underwater construction; the underwater spread is 128–152 mm, indicating that the slurry has good fluidity and spreading ability underwater, and can fully fill cracks and irregular surfaces; the 28-day underwater adhesion strength and chloride ion diffusion coefficient indicate that the repair layer is firmly bonded to the substrate and has a dense microstructure. Example 2 exhibits the best overall performance.

[0066] Comparative Example 1 showed excessively high viscosity and poor workability. Furthermore, the high diatom content encapsulated in microspheres led to an overly dense network structure within the system, hindering the repair reaction, prolonging the repair time, and reducing the material's repair strength. Comparative Example 2 indicated that ordinary buffers could not effectively regulate the hydration process of magnesium phosphate cement, resulting in coarse crystallization and a loose structure in the hydration products. Diatoms also died from alkali poisoning and could not participate in subsequent pore filling. Comparative Example 3 showed that the lack of HPMC resulted in excessive viscosity loss in the slurry, decreased underwater anti-dispersion properties, and although the fluidity was good, significant material loss occurred. The absence of a gradient transition layer at the interface led to thermal stress concentration, resulting in microcracks after repair. Comparative Example 4 indicated that the lack of synergistic effects from inert mineral fillers prevented timely absorption of latent heat of hydration, causing localized high temperatures that led to thermal shock death of diatoms and decreased volume stability. Comparative Example 5 showed that intelligent response additives have a positive effect on balancing workability and setting time, and optimizing the microstructure. The results of Comparative Example 6 show that diatom metabolic activity has no negative impact on the macroscopic mechanical properties of the cement matrix within 28 days, and the basic properties of the repair layer are mainly determined by the material itself.

[0067] (5) Crack self-healing performance test: To directly verify the underwater self-healing performance of the coating of this application, artificial cracks were prepared on the surface of each group of hardened specimens, and the initial crack width w0 was recorded. The specimens were then placed in a water environment with the same salt concentration as the aforementioned simulated seawater for continuous curing. Microscopic observations were performed on the same crack location at 1d, 7d, 14d, and 28d, and the remaining crack width w0 was recorded. t Each group should have at least 3 parallel specimens, and each specimen should have at least 3 fixed measuring points. The crack closure rate is calculated using the following formula: Crack closure rate / % = (w0 - w) t ) / w0×100%.

[0068] The test results are shown in Table 5.

[0069] Table 5 Initial crack width and crack closure rate at different stages of specimen development

[0070] Table 5 shows that the coating of this application has excellent self-healing ability for cracks in underwater environments, and the repair effect continues to increase with curing time. The crack closure rate of the three embodiments reached more than 70% after 28 days, with Embodiment 2 being the best embodiment. Crack closure mainly depends on the deposition of minerals such as calcium carbonate induced by the metabolic activity of living diatoms, while the deposition of cement matrix hydration products plays an auxiliary filling role.

[0071] Comparative Example 1 shows that excessive microspheres lead to excessively high slurry viscosity, making it difficult to fully penetrate cracks during construction. Furthermore, localized microsphere enrichment hinders material transport, prolonging the repair time. Comparative Example 2 shows that the extremely low diatom survival rate under ordinary buffering agents results in almost complete loss of biomineralization capacity, and buffer failure leads to a loose structure of hydration products, resulting in poor filling effect. Comparative Example 3 shows that the lack of hydroxypropyl methylcellulose (HPMC) results in no gradient transition layer at the interface, leading to thermal stress concentration and the presence of microcracks within the coating after repair. This significantly reduces the material's impermeability and adhesion strength, and interface defects and microcracks provide pathways for crack propagation, reducing the effective filling efficiency of the repair product. Comparative Example 4 shows that the lack of filler leading to diatom thermal shock death is the main cause, while concentrated hydration heat also accelerates the uneven deposition of local hydration products. Comparative Example 5 shows that intelligent responsive additives play an important role in improving repair efficiency by regulating local rheological states and optimizing material transport.

[0072] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. An underwater diatomaceous earth self-healing coating, characterized in that: The product comprises the following components in parts by weight: 40-60 parts magnesium phosphate cement matrix, 3-8 parts alkaline-resistant rhomboid algae encapsulated with alginate microspheres, 1-5 parts smart responsive additive, 15-30 parts sodium citrate buffer, 0.5-2 parts anti-washout agent, and 5-10 parts inert mineral filler; wherein the smart responsive additive is a pH-sensitive polymer.

2. The underwater diatom self-healing coating according to claim 1, characterized in that: The alkali-resistant crescent-shaped algae encapsulated in the alginate microspheres was prepared by the following method: Alkali-tolerant rhomboid algae were dispersed in simulated seawater to obtain a diatom dispersion; sodium alginate solution was prepared. Using the diatom dispersion as the inner phase and the sodium alginate solution as the outer phase, droplets of the outer phase encapsulating the inner phase are formed by a coaxial dropping device and dropped into a calcium lactate crosslinking solution at 5-15℃ for 1-5 minutes to form core-shell microspheres with an inner phase containing alkali-resistant crescent-shaped algae as the core layer and calcium alginate gel as the shell layer. The core-shell microspheres are washed and filtered to obtain alkali-resistant crescent-shaped algae encapsulated in alginate microspheres, which are then individually sealed and stored at 2-8℃ for later use. The dry weight ratio of sodium alginate to the alkali-tolerant crescent-shaped algae is 2:1 to 4:

1.

3. The underwater diatom self-healing coating according to claim 2, characterized in that: The alkaline-tolerant rhomboid algae was gently stirred at 50–150 r / min for 5–15 min at 5–15℃ to disperse in simulated seawater. The mass fraction of the alkaline-tolerant rhomboid algae in the diatom dispersion was 0.5 wt%–2 wt%, and the mass fraction of the sodium alginate solution was 1.5 wt%–3 wt%. The cross-linked core-shell microspheres were immediately washed 2-3 times with the isotonic seawater buffer solution and collected by filtration through a sieve to obtain alkali-resistant rhomboid algae encapsulated in wet alginate microspheres for later use.

4. The underwater diatom self-healing coating according to claim 2, characterized in that: The simulated seawater was prepared by mixing water with six salts: sodium chloride, magnesium chloride hexahydrate, sodium sulfate, calcium chloride, potassium chloride, and sodium bicarbonate. The proportions of sodium chloride, magnesium chloride hexahydrate, sodium sulfate, calcium chloride, potassium chloride, and sodium bicarbonate in the total mass of the salts were 58.72%, 26.57%, 9.79%, 2.78%, 1.66%, and 0.48%, respectively. The total salt concentration of the simulated seawater was 35 g / L.

5. The underwater diatom self-healing coating according to claim 1, characterized in that: The intelligent response additive is polyacrylic acid micro powder containing a retarder, and its preparation steps are as follows: dispersing polyacrylic acid in simulated seawater, adding a retarder, and stirring evenly to obtain a spray-dried liquid. The mass ratio of polyacrylic acid, simulated seawater, and retarder is 1:(10-20):(0.03-0.10). The retarder is selected from one or more of boric acid, borax, citric acid, and citrate. The spray-dried liquid is spray-dried to obtain polyacrylic acid micro powder containing a retarder; the median particle size D50 of the polyacrylic acid micro powder containing the retarder is 10-50 μm.

6. The underwater diatom self-healing coating according to claim 1, characterized in that: The anti-washing agent includes xanthan gum; the inert mineral filler is composed of quartz sand and fine sand; the mass ratio of quartz sand to fine sand is (2-4):

1.

7. The underwater diatom self-healing coating according to claim 1, characterized in that: The magnesium phosphate cement matrix is ​​prepared by the following method: Low-activity magnesium oxide, potassium dihydrogen phosphate, hydroxypropyl starch, hydroxypropyl methylcellulose and sodium citrate with activity values ​​of 40-60s were dried and sieved respectively. The low-activity magnesium oxide and potassium dihydrogen phosphate are added to a dry powder mixing device and dry-mixed at 15-30°C for 1-3 minutes. Add the hydroxypropyl starch, hydroxypropyl methylcellulose and sodium citrate, and continue dry mixing for 2-5 minutes to obtain a uniform magnesium phosphate cement dry powder matrix; The mass percentages of potassium dihydrogen phosphate, hydroxypropyl starch, hydroxypropyl methylcellulose, and sodium citrate are 20%–30%, 5%–10%, 2%–4%, and 10%–15% of the mass of the low-activity magnesium oxide, respectively.

8. A method for preparing an underwater diatom self-healing coating as described in any one of claims 1 to 7, characterized in that: Includes the following steps: S1. Under conditions of 15-25℃, the magnesium phosphate cement matrix, sodium citrate buffer, smart response additive, anti-washing agent and inert mineral filler are mixed to obtain a premix. S2. Add mixing liquid to the premix and mechanically stir to obtain a uniform magnesium phosphate cement paste; S3. Vacuum degassing is performed on the magnesium phosphate cement slurry, and the temperature of the degassed magnesium phosphate cement slurry is controlled at no higher than 25°C. S4. Add alkali-resistant crescent-shaped algae encapsulated with alginate microspheres to the defoamed magnesium phosphate cement slurry, and mix evenly using a low-speed paddle stirring method to obtain the underwater diatom self-healing coating.

9. The method for preparing the underwater diatom self-healing coating according to claim 8, characterized in that: In step S2, the mechanical stirring speed is 300-600 r / min, and the stirring time is 1-3 min; in step S3, the vacuum degassing time is 1-3 min; in step S4, when adding alkaline-resistant crescent-shaped algae encapsulated with alginate microspheres, the temperature of the magnesium phosphate cement slurry is 15-25℃, the speed of the low-speed paddle stirrer is 50-150 r / min, and the stirring time is 1-3 min.

10. The application of an underwater diatom self-healing coating as described in any one of claims 1 to 7 in the repair of concrete in offshore engineering projects.