Two-component aircraft coating adhesion promoter and method for its production
The use of a two-component aircraft coating adhesion promoter solves the problem that existing technologies cannot fully meet standards, achieving a significant improvement in adhesion and corrosion resistance while meeting environmental protection requirements.
Patent Information
- Application Number
- CN202611331093.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
Existing adhesion promoters do not fully comply with AIMS04-04-053 and BMS10-128 standards and have pollution problems.
A two-component aircraft coating adhesion promoter is used, comprising a siloxane coupling agent with metal corrosion inhibitor groups and a hydrolysis promoter, which are used as component A and component B, respectively, to achieve pretreatment of aircraft paint and enhance the adhesion and corrosion resistance between metal and paint.
It achieves enhanced adhesion and corrosion resistance in aircraft surface treatment, fully complies with AIMS04-04-053 and BMS10-128 standards, and does not contain the toxic substance chromium.
Smart Images

Figure CN123152379A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating pretreatment technology, and in particular to a two-component aircraft coating adhesion promoter and its preparation method. Background Technology
[0002] Alodine treatment is currently the most widely used chemical conversion coating process for aluminum alloys in the aerospace industry. Chromate conversion treatment technology, represented by Alodine 1200S, can form a brownish-yellow conversion film on the aluminum alloy surface. This film not only has extremely strong corrosion resistance but also ensures good adhesion for subsequent coatings. After decades of engineering verification, Alodine treatment has become the standard pretreatment method for skin coating systems in civil aircraft manufacturing and maintenance.
[0003] However, Alodine conversion solutions contain trivalent and hexavalent chromium ions. Hexavalent chromium compounds are classified as Group 1 carcinogens by the International Agency for Research on Cancer, posing a serious threat to the health of operators and the environment. In the field of aerospace manufacturing and maintenance, finding a chromium-free surface pretreatment technology to replace traditional chromate conversion treatment has become an urgent issue that the industry needs to address.
[0004] In recent years, novel chromium-free adhesion promoters, represented by sol-gel technology, have attracted widespread attention. This technology constructs a pretreatment layer on aluminum alloy surfaces through the formation of an organic-inorganic hybrid film, providing both enhanced adhesion and corrosion protection, without containing toxic or harmful chromium compounds. Currently, existing surface adhesion promoters for civil aircraft painting and repair require compliance with Airbus's technical standard AIMS04-04-053 for Airbus aircraft and Boeing's BMS10-128 standard. Currently available products only meet the Boeing BMS10-128 standard, and actual tests show that none meet the AIMS04-04-053 standard's requirement of preventing hydrogen embrittlement corrosion of high-strength cadmium-plated steel.
[0005] Therefore, existing technologies still need to be improved and developed. Summary of the Invention
[0006] In view of the shortcomings of the prior art, the purpose of this invention is to provide a two-component aircraft coating adhesion promoter and its preparation method, aiming to solve the problem that existing adhesion promoters cannot fully comply with AIMS04-04-053 and BMS10-128 standards and cause serious pollution.
[0007] The technical solution of the present invention is as follows: A two-component aircraft coating adhesion promoter, comprising, by weight parts: 1-5 parts of siloxane coupling agent with metal corrosion inhibitor groups; 45-60 parts of hydrolysis accelerator.
[0008] The two-component aircraft coating adhesion promoter, wherein the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80wt%-90wt% of methylimidazoline-epoxysiloxane coupling agent adduct and 10wt%-20wt% of 4-[3-(trimethoxysilyl)propyl]morpholine; wherein the molecular formula of the methylimidazoline-epoxysiloxane coupling agent adduct is […]. .
[0009] The two-component aircraft coating adhesion promoter, wherein the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 20 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
[0010] The two-component aircraft coating adhesion promoter, wherein the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 90 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 10 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
[0011] The two-component aircraft coating adhesion promoter, wherein the hydrolysis promoter comprises, by mass percentage: 15wt%-25wt% organic solvent, with the balance being water; Preferably, the organic solvent is selected from one or more of isopropanol, ethanol, and n-propanol.
[0012] The two-component aircraft coating adhesion promoter comprises, by weight, 1 part of a siloxane coupling agent with a metal corrosion inhibitor group and 49 parts of a hydrolysis accelerator.
[0013] A method for preparing a two-component aircraft coating adhesion promoter includes the following steps: The methylimidazoline-epoxysiloxane coupling agent adduct was mixed with 4-[3-(trimethoxysilyl)propyl]morpholine to obtain a siloxane coupling agent with a metal corrosion inhibitor group; An organic solvent is mixed with water to obtain a hydrolysis accelerator; The siloxane coupling agent with the metal corrosion inhibitor group and the hydrolysis accelerator are packaged separately as component A and component B to obtain a two-component aircraft coating adhesion accelerator.
[0014] The method for preparing the two-component aircraft coating adhesion promoter includes the following steps: mixing 2-methylimidazoline with γ-glycidoxypropyltrimethoxysilane and heating and stirring to obtain the methylimidazoline-epoxysiloxane coupling agent adduct.
[0015] The preparation method of the two-component aircraft coating adhesion promoter includes a heating and stirring treatment at a temperature of 90℃-100℃, a heating and stirring treatment time of 40min-60min, and a stirring speed of 60 rpm-90 rpm.
[0016] The method for preparing the two-component aircraft coating adhesion promoter, wherein the molar ratio of 2-methylimidazoline to γ-glycidoxypropyltrimethoxysilane is 1:1.
[0017] Beneficial effects: This invention provides a two-component aircraft coating adhesion promoter and its preparation method. The two-component aircraft coating adhesion promoter, by mass parts, includes: 1-5 parts of a siloxane coupling agent with a metal corrosion inhibitor group; and 45-60 parts of a hydrolysis promoter. This invention utilizes a siloxane coupling agent with metal corrosion inhibitor groups as component A. This siloxane coupling agent possesses metal corrosion inhibitor groups that prevent hydrogen embrittlement corrosion of high-strength cadmium-plated steel, and siloxane groups that enhance adhesion. The siloxane groups can hydrolyze into silanols, exhibiting a coupling effect and enhancing paint adhesion to the metal surface. The hydrolysis accelerator, as component B, promotes the hydrolysis of siloxanes into silanols. The siloxane coupling agent with metal corrosion inhibitor groups and the hydrolysis accelerator are packaged separately for storage. When used, they are mixed and activated according to a specified ratio before spraying. This process is used for pre-treatment before aircraft painting, increasing adhesion between metal and paint and enhancing the corrosion resistance of aircraft metal. It is chromium-free and fully complies with AIMS04-04-053 and BMS10-128 standards. Attached Figure Description
[0018] Figure 1 A schematic diagram of the synthetic pathway for methylimidazoline-epoxysiloxane coupling agent adducts; Figure 2 A diagram illustrating the classification of adhesion test results; Figure 3 This is a schematic diagram of filamentous corrosion. Detailed Implementation
[0019] This invention provides a two-component aircraft coating adhesion promoter and its preparation method. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0020] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and should not be interpreted in an idealized or overly formal sense unless specifically defined as herein.
[0021] Before painting aircraft skin and other structural components, proper surface pretreatment must be performed to ensure good adhesion between the coating system and the metal substrate and to impart sufficient corrosion resistance to the substrate.
[0022] Faced with increasingly stringent environmental regulations, the commonly used alodine treatment is no longer adequate, placing unprecedented pressure on the aerospace industry to transform. The EU's REACH regulation has explicitly included hexavalent chromium in its list of substances of very high concern and requires authorized use. Simultaneously, the European Chemicals Agency has further published a proposal to restrict the use of hexavalent chromium, planning to implement strict controls on chromic anhydride, chromic acid, dichromic acid, and their salts throughout the EU. As a result, traditional aerospace surface treatment processes such as chromate-containing chemical conversion treatments and chromic acid anodizing are facing gradual elimination or strict restrictions. Major aerospace industrial nations such as the United States have also successively introduced regulations restricting the use of hexavalent chromium.
[0023] Currently, although new chromium-free adhesion promoters represented by sol-gel technology meet environmental protection requirements, they only meet the Boeing BMS10-128 standard. Actual tests show that they do not meet the technical requirements of AIMS04-04-053 standard for not causing hydrogen embrittlement corrosion on high-strength cadmium-plated steel.
[0024] Therefore, developing a high-efficiency and environmentally friendly metal adhesion promoter for aircraft surfaces that fully complies with AIMS04-04-053 and BMS10-128 standards is of great engineering application value and practical significance for promoting the green transformation of aerospace surface treatment technology and meeting increasingly stringent environmental compliance requirements.
[0025] Based on this, the present invention provides a two-component aircraft coating adhesion promoter, comprising, by weight parts: 1-5 parts of siloxane coupling agent with metal corrosion inhibitor groups; 45-60 parts of hydrolysis accelerator.
[0026] In this embodiment, the siloxane coupling agent with metal corrosion inhibitor groups is used as component A. This siloxane coupling agent possesses metal corrosion inhibitor groups that prevent hydrogen embrittlement corrosion of high-strength cadmium-plated steel and siloxane groups that enhance adhesion. The siloxane groups can hydrolyze into silanols, exhibiting a coupling effect and enhancing the adhesion of paint to the metal surface. The hydrolysis accelerator, as component B, promotes the hydrolysis of siloxanes into silanols. The siloxane coupling agent with metal corrosion inhibitor groups and the hydrolysis accelerator are packaged separately for storage. When used, they are mixed and activated according to a specified ratio before spraying. This process is used for pre-treatment before aircraft painting, increasing the adhesion between the metal and paint and enhancing the corrosion resistance of the aircraft metal. It is chromium-free and fully complies with AIMS04-04-053 and BMS10-128 standards.
[0027] Specifically, before painting the aircraft's metal surface, the metal surface is first deoxidized, cleaned, and dried. Then, the two-component aircraft paint adhesion promoter is mixed evenly according to the specified mass ratio. After 30-60 minutes, it is brushed or sprayed onto the metal surface. After drying, the surface is checked for dryness before proceeding to the next painting process. The mixed two-component aircraft paint adhesion promoter can be used within 24 hours of mixing. Pre-treating the aircraft's metal surface with the two-component aircraft paint adhesion promoter increases the adhesion between the metal and the paint, and also enhances the corrosion resistance of the aircraft metal.
[0028] In some embodiments, the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80wt%-90wt% of a methylimidazoline-epoxysiloxane coupling agent adduct and 10wt%-20wt% of 4-[3-(trimethoxysilyl)propyl]morpholine; wherein the molecular formula of the methylimidazoline-epoxysiloxane coupling agent adduct is […]. .
[0029] Specifically, the methylimidazoline-epoxysiloxane coupling agent adduct is obtained by reacting 2-methylimidazoline and γ-glycidoxypropyltrimethoxysilane, and it has imidazoline groups to prevent hydrogen embrittlement corrosion of high-strength cadmium-plated steel and siloxane groups to enhance adhesion.
[0030] Furthermore, the mechanism of hydrogen embrittlement corrosion is due to the presence of pores on the surface of cadmium-plated carbon steel. Under the action of corrosive media and water, the following corrosion reactions occur: Primary anodic reaction: Cd → Cd 2+ +2e - Hydrolysis then occurs to generate H + Cd2+ +H₂O→Cd(OH)₂+2H₂O + Cathode reaction: 2H + +2e - →H2↑ This results in brittleness due to the hydrogen gas entering the steel, leading to a decrease in strength. The methylimidazoline-epoxysiloxane coupling agent adduct molecule... nitrogen atom of the group and Cd 2+ Coordination occurs, inhibiting Cd 2+ The reaction with water molecules inhibits hydrogen generation, thereby suppressing hydrogen embrittlement in high-strength carbon steel. Furthermore, the imidazoline group can simultaneously coordinate with the surfaces of steel, aluminum, magnesium, titanium alloys, and copper to form a film, protecting the metal from corrosive liquids, and exhibits a synergistic effect with the corrosion-inhibiting effect of 4-[3-(trimethoxysilyl)propyl]morpholine. Moreover, the methylimidazoline-epoxysiloxane coupling agent adduct molecule... Under the influence of water molecules, methanol can be removed to become The silanol structure allows for condensation at one end with the -OH group on a metal surface and at the other end with the -OH group on the surface of inorganic pigments in coatings, enhancing the anchoring of the coating-interface and improving adhesion to metal surfaces. It can also condense within the -OH group of the silanol itself to form a network structure. Simultaneously... The hydroxyl group at the other end of the molecule can react with the groups in the coating to form a stable bridge for anchoring the metal surface to resin or pigment condensation, thereby enhancing the adhesion of the coating to the metal surface.
[0031] In this embodiment, the molecular formula of 4-[3-(trimethoxysilyl)propyl]morpholine (CAS No.: 31024-54-1) is: The oxygen and nitrogen atoms of the morpholine group have the function of coordinating with metal ions on the metal surface, which can form a film on the metal surface, block the corrosion of the metal by harmful corrosive media, and produce a corrosion inhibition effect. It has a synergistic effect with the methylimidazoline-epoxysiloxane coupling agent adduct, increasing the corrosion resistance time of the metal plate. In addition, the 4-[3-(trimethoxysilyl)propyl]morpholine also has an active siloxane, which can be hydrolyzed into silanol, which has a coupling effect and enhances the adhesion of paint to the metal surface. Furthermore, the morpholine group has surface activity, which enhances the wetting and leveling effect in the system and is conducive to the formation of a continuous and smooth coating film.
[0032] In a preferred embodiment, the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 20 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
[0033] In another preferred embodiment, the siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 90 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 10 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
[0034] In some embodiments, the hydrolysis accelerator comprises, by mass percentage: 15wt%-25wt% organic solvent, with the balance being water; the organic solvent and water are mixed to form a hydrolysis accelerator, which can dissolve and dilute the siloxane coupling agent with metal corrosion inhibitor groups, thereby promoting the hydrolysis of siloxanes into silanols.
[0035] In some embodiments, the organic solvent is selected from one or more of isopropanol, ethanol, and n-propanol.
[0036] In some embodiments, the product comprises, by weight, 1 part of a siloxane coupling agent with a metal corrosion inhibitor group and 49 parts of a hydrolysis accelerator.
[0037] In addition, the present invention also provides a method for preparing a two-component aircraft coating adhesion promoter, comprising the following steps: Step S10: Mix the methylimidazoline-epoxysiloxane coupling agent adduct with 4-[3-(trimethoxysilyl)propyl]morpholine to obtain a siloxane coupling agent with a metal corrosion inhibitor group; Step S20: Mix the organic solvent with water to obtain a hydrolysis accelerator; Step S30: The siloxane coupling agent with metal corrosion inhibitor group and the hydrolysis accelerator are packaged separately as component A and component B to obtain a two-component aircraft coating adhesion accelerator.
[0038] In this embodiment, the methylimidazoline-epoxysiloxane coupling agent adduct is mixed with 4-[3-(trimethoxysilyl)propyl]morpholine to obtain a siloxane coupling agent with metal corrosion inhibitor groups as component A; then, an organic solvent and water are mixed to obtain a hydrolysis accelerator as component B. The two components are normally packaged separately and mixed in proportion before use. They can be used after 30 minutes, and use within 30 minutes to 24 hours after mixing is suitable. The siloxane coupling agent with metal corrosion inhibitor groups possesses metal corrosion inhibitor groups that prevent hydrogen embrittlement corrosion of high-strength cadmium-plated steel and siloxane groups that enhance adhesion. The siloxane groups can hydrolyze into silanols, exhibiting a coupling effect and enhancing the adhesion of paint to the metal surface. The hydrolysis accelerator promotes the hydrolysis of siloxanes into silanols. The two-component aircraft coating adhesion promoter is used for pretreatment of aircraft paint to increase the adhesion between metal and paint and increase the corrosion resistance of aircraft metal. It is chromium-free and fully complies with AIMS04-04-053 and BMS10-128 standards.
[0039] In some embodiments, the reaction equation for preparing the methylimidazoline-epoxysiloxane coupling agent adduct is as follows: Figure 1 As shown; the preparation method of the methylimidazoline-epoxysiloxane coupling agent adduct includes the following steps: mixing 2-methylimidazoline with γ-glycidoxypropyltrimethoxysilane, and heating and stirring to obtain the methylimidazoline-epoxysiloxane coupling agent adduct.
[0040] In some embodiments, the molar ratio of the 2-methylimidazoline to the γ-glycidoxypropyltrimethoxysilane is 1:1.
[0041] In some embodiments, the temperature of the heating and stirring treatment is 90℃-100℃, the time of the heating and stirring treatment is 40min-60min, and the stirring speed of the heating and stirring treatment is 60 rpm-90 rpm.
[0042] In a preferred embodiment, the temperature of the heating and stirring treatment is 95°C, the time of the heating and stirring treatment is 45 min, and the stirring speed of the heating and stirring treatment is 80 rpm.
[0043] Specifically, the 2-methylimidazoline (content >99%) and the γ-glycidoxypropyltrimethoxysilane (content >99%) are added in an equimolar ratio to a reactor equipped with a reflux device. The reactor is preheated to 90℃-100℃, the stirring speed is 60-90 rpm, and the time is 45 minutes. After cooling, the methylimidazoline-epoxysiloxane coupling agent adduct is obtained. During the preparation of the methylimidazoline-epoxysiloxane coupling agent adduct, it is necessary to control the dehumidification and drying of the reactor, pipelines, and packaging materials, and the air humidity should be controlled below 70%.
[0044] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention.
[0045] Example 1 This embodiment provides a two-component aircraft coating adhesion promoter, comprising: Component A, a siloxane coupling agent with a metal corrosion inhibitor group, comprises, by mass percentage: 80 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 20 wt% 4-[3-(trimethoxysilyl)propyl]morpholine; Component B, hydrolysis accelerator, by mass percentage, includes: 15wt% isopropanol and the balance being deionized water.
[0046] Before painting, the metal surface must be thoroughly cleaned and dried. Mix the adhesion promoter with component A at a ratio of 1:49 (by weight). After 30 minutes, brush or spray the mixture onto the metal surface and allow it to dry for 1 hour. Once the surface is dry, proceed to the next painting step. The mixed adhesion promoter can be used within 24 hours of mixing.
[0047] Example 2 This embodiment provides a two-component aircraft coating adhesion promoter, comprising: Component A, a siloxane coupling agent with a metal corrosion inhibitor group, comprises, by mass percentage: 90 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 10 wt% 4-[3-(trimethoxysilyl)propyl]morpholine; Component B, hydrolysis accelerator, by mass percentage, includes: 25wt% isopropanol and the balance being deionized water.
[0048] Before painting, the metal surface must be thoroughly cleaned and dried. Mix the adhesion promoter with component A at a ratio of 1:49 (by weight). After 30 minutes, brush or spray the mixture onto the metal surface and allow it to dry for 1 hour. Once the surface is dry, proceed to the next painting step. The mixed adhesion promoter can be used within 24 hours of mixing.
[0049] Comparative Example 1 This comparative example does not use adhesion promoters to treat the metal surface, but directly sprays the aircraft primer and topcoat as specified in AIMS04-04-053 onto 2024 aluminum alloy.
[0050] Comparative Example 2 In this comparative example, component A consists only of the methylimidazoline-epoxysiloxane coupling agent adduct; component B, the hydrolysis accelerator, comprises, by mass percentage: 15 wt% isopropanol and the remainder deionized water.
[0051] Comparative Example 3 In this comparative example, component A contains only 4-[3-(trimethoxysilyl)propyl]morpholine; component B, a hydrolysis accelerator, comprises, by mass percentage: 15 wt% isopropanol and the remainder deionized water.
[0052] Comparative Example 4 In this comparative example, component A was replaced with deionized water; component B, a hydrolysis accelerator, comprised, by mass percentage, 15 wt% isopropanol and the remainder deionized water.
[0053] Comparative Example 1 was applied directly to 2024 aluminum alloy without surface treatment, using the aircraft primer + topcoat as specified in AIMS 04-04-053. Comparative Examples 2, 3, and 1 were mixed according to a 1:49 mass ratio of component A to component B, sprayed onto the 2024 aluminum alloy surface after 30 minutes, and dried for 1 hour before being coated with the aircraft primer + topcoat as specified in AIMS 04-04-053. All coated panels were tested for adhesion after 7 days of drying according to the adhesion test method specified in AIMS 04-04-053. The results are shown in Table 1. Table 1
[0054] It should be noted that the highest adhesion level is 0, and the lowest is 5. The test results are categorized and explained in detail below. Figure 2 As shown; water resistance is tested by soaking in water for 14 days as specified in the standard; solvent resistance is tested by soaking in the specified solvent for 2 hours and drying for 1 hour as specified in the standard.
[0055] As shown in Table 1, in Comparative Example 1, the metal surface was untreated, and the coating adhesion, water resistance, and solvent resistance were all rated at level 2. In Comparative Example 2, component A was 100% methylimidazoline-epoxysiloxane coupling agent adduct, and the coating adhesion, water resistance, and solvent resistance were all rated at level 1, indicating that the methylimidazoline-epoxysiloxane coupling agent enhanced the coating adhesion, but still did not reach the standard requirement of level 0. In Comparative Example 3, component A was 100% 4-[3-(trimethoxysilyl)propyl]morpholine, and the coating... The adhesion, water resistance, and solvent resistance of the coating are all rated as Grade 1, indicating that 4-[3-(trimethoxysilyl)propyl]morpholine enhances the adhesion of the coating, but still does not meet the standard requirement of Grade 0. In Example 1, Component A, consisting of 80% methylimidazoline-epoxysiloxane coupling agent and 20% 4-[3-(trimethoxysilyl)propyl]morpholine, produces a coating with adhesion, water resistance, and solvent resistance all rated as Grade 0, which meets the requirements of AIMS04-04-053 standard. This shows that the two components have a synergistic effect in enhancing adhesion, which is better than when used alone.
[0056] Hydrogen embrittlement corrosion tests were conducted on the adhesion promoters of Comparative Example 2, Comparative Example 4, and Example 1. The components were mixed at a mass ratio of Component A:Component B of 1:49 and then subjected to an AIMS 04-04-053 hydrogen embrittlement test. The results are shown in Table 2. Table 2
[0057] As shown in Table 2, Comparative Example 4, which contained deionized water but no corrosion inhibitor, exhibited hydrogen embrittlement fracture because deionized water causes hydrogen embrittlement. In Comparative Example 2, component A was a 100% methylimidazoline-epoxysiloxane coupling agent adduct, which passed the hydrogen embrittlement test required by AIMS04-04-053 standard, and component B was the same. This indicates that the methylimidazoline-epoxysiloxane coupling agent adduct is an effective hydrogen embrittlement corrosion inhibitor. Example 1, which contained the methylimidazoline-epoxysiloxane coupling agent adduct, also passed the hydrogen embrittlement test.
[0058] The adhesion promoters of Comparative Examples 1, 2, 3, and 1 were subjected to coating corrosion resistance tests. Comparative Example 1 was applied directly to 2024 aluminum alloy without surface treatment, using the aircraft primer + topcoat as specified in AIMS 04-04-053. Comparative Examples 2, 3, and 1 were mixed according to the A:B mass ratio of 1:49, sprayed onto the 2024 aluminum alloy surface after 30 minutes, and dried for 1 hour before being coated with the aircraft primer + topcoat as specified in AIMS 04-04-053. All coated panels were dried for 7 days and then subjected to filiform corrosion and salt water immersion corrosion tests as specified in AIMS 04-04-053. The results are shown in Table 3. Table 3
[0059] It should be noted that filamentous corrosion refers to the corrosion length of the metal on both sides of the scribe line under the coating after scribing the coating surface to penetrate into the metal substrate according to the AIMS04-04-053 standard and immersing it in dilute hydrochloric acid for 960 hours. A schematic diagram of filamentous corrosion is shown below. Figure 3 As shown.
[0060] As shown in Table 3, Comparative Example 1, with no surface treatment, failed in both filamentous corrosion (500 hours) and hydrochloric acid immersion corrosion (1000 hours). In Comparative Example 2, component A was 100% methylimidazoline-epoxysiloxane coupling agent adduct, which improved the filamentous corrosion resistance to 800 hours and the hydrochloric acid immersion corrosion resistance to 1300 hours, indicating that the methylimidazoline-epoxysiloxane coupling agent enhances the corrosion resistance of the coating, but still does not meet the standard requirements. In Comparative Example 3, component A was 100% 4-[3-(trimethoxysilyl)propyl]morpholine. The filamentous corrosion resistance was increased to 750 hours and the hydrochloric acid immersion corrosion resistance was increased to 1200 hours, indicating that 4-[3-(trimethoxysilyl)propyl]morpholine enhanced the corrosion resistance of the coating, but still did not meet the standard requirements. In Example 1, the A component, consisting of 80% methylimidazoline-epoxysiloxane coupling agent and 20% 4-[3-(trimethoxysilyl)propyl]morpholine, showed that the coating's filamentous corrosion resistance and salt water immersion corrosion resistance both met the AIMS04-04-053 standard requirements, indicating that the two components have a synergistic effect in inhibiting corrosion, which is better than when used alone.
[0061] In summary, the present invention provides a two-component aircraft coating adhesion promoter and its preparation method. The two-component aircraft coating adhesion promoter, by mass parts, comprises: 1-5 parts of a siloxane coupling agent with a metal corrosion inhibitor group; and 45-60 parts of a hydrolysis promoter. This invention utilizes a siloxane coupling agent with metal corrosion inhibitor groups as component A. This siloxane coupling agent possesses metal corrosion inhibitor groups that prevent hydrogen embrittlement corrosion of high-strength cadmium-plated steel, and siloxane groups that enhance adhesion. The siloxane groups can hydrolyze into silanols, exhibiting a coupling effect and enhancing paint adhesion to the metal surface. The hydrolysis accelerator, as component B, promotes the hydrolysis of siloxanes into silanols. The siloxane coupling agent with metal corrosion inhibitor groups and the hydrolysis accelerator are packaged separately for storage. When used, they are mixed and activated according to a specified ratio before spraying. This process is used for pre-treatment before aircraft painting, increasing adhesion between metal and paint and enhancing the corrosion resistance of aircraft metal. It is chromium-free and fully complies with AIMS04-04-053 and BMS10-128 standards.
[0062] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.
Claims
1. A two-component aircraft coating adhesion promoter, characterized in that, By weight, including: 1-5 parts of siloxane coupling agent with metal corrosion inhibitor groups; 45-60 parts of hydrolysis accelerator.
2. The two-component aircraft coating adhesion promoter according to claim 1, characterized in that, The siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80wt%-90wt% of methylimidazoline-epoxysiloxane coupling agent adduct and 10wt%-20wt% of 4-[3-(trimethoxysilyl)propyl]morpholine; wherein, the molecular formula of the methylimidazoline-epoxysiloxane coupling agent adduct is […]. .
3. The two-component aircraft coating adhesion promoter according to claim 2, characterized in that, The siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 80 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 20 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
4. The two-component aircraft coating adhesion promoter according to claim 2, characterized in that, The siloxane coupling agent with metal corrosion inhibitor groups comprises, by mass percentage: 90 wt% methylimidazoline-epoxysiloxane coupling agent adduct and 10 wt% 4-[3-(trimethoxysilyl)propyl]morpholine.
5. The two-component aircraft coating adhesion promoter according to claim 1, characterized in that, The hydrolysis accelerator comprises, by mass percentage: 15wt%-25wt% organic solvent, with the balance being water; Preferably, the organic solvent is selected from one or more of isopropanol, ethanol, and n-propanol.
6. The two-component aircraft coating adhesion promoter according to claim 1, characterized in that, By mass, it includes: 1 part of siloxane coupling agent with metal corrosion inhibitor group and 49 parts of hydrolysis accelerator.
7. A method for preparing a two-component aircraft coating adhesion promoter as described in any one of claims 1-6, characterized in that, Including the following steps: The methylimidazoline-epoxysiloxane coupling agent adduct was mixed with 4-[3-(trimethoxysilyl)propyl]morpholine to obtain a siloxane coupling agent with a metal corrosion inhibitor group; An organic solvent is mixed with water to obtain a hydrolysis accelerator; The siloxane coupling agent with the metal corrosion inhibitor group and the hydrolysis accelerator are packaged separately as component A and component B to obtain a two-component aircraft coating adhesion accelerator.
8. The method for preparing the two-component aircraft coating adhesion promoter according to claim 7, characterized in that, The method for preparing the methylimidazoline-epoxysiloxane coupling agent adduct includes the following steps: mixing 2-methylimidazoline with γ-glycidoxypropyltrimethoxysilane, and heating and stirring the mixture to obtain the methylimidazoline-epoxysiloxane coupling agent adduct.
9. The method for preparing the two-component aircraft coating adhesion promoter according to claim 8, characterized in that, The temperature of the heating and stirring treatment is 90℃-100℃, the time of the heating and stirring treatment is 40min-60min, and the stirring speed of the heating and stirring treatment is 60 rpm-90 rpm.
10. The method for preparing the two-component aircraft coating adhesion promoter according to claim 8, characterized in that, The molar ratio of 2-methylimidazoline to γ-glycidoxypropyltrimethoxysilane is 1:1.