High-frequency high-speed adhesive film for FPC and preparation method thereof
By blending modified HDPE resin with functional additives, a high-frequency, high-speed adhesive film with low dielectric loss and high bonding strength was prepared, which solved the problems of insufficient dielectric properties and poor heat resistance of existing technologies, and realized the substitution and industrial application of domestic high-frequency adhesive films.
Patent Information
- Application Number
- CN202611321491.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing ordinary adhesive films have high dielectric constants and high dielectric losses in high-frequency and high-speed communication, resulting in severe signal transmission attenuation. They also lack resistance to high-temperature solder impact and cannot meet the production process and performance requirements of high-frequency FPCs and high-speed optical modules, leading to the reliance on imports for domestically produced high-end high-frequency adhesive films.
High-frequency, high-speed adhesive films were prepared by blending modified HDPE resin with functional additives. The dielectric constant DK was 2.5-2.8 and the dielectric loss DF was 0.0008-0.0013. The films were prepared by using a combination of twin-screw extruders and single-screw extruders with multiple casting and calendering processes. The films have excellent low dielectric and low loss characteristics, can withstand the thermal shock of soldering at 300℃, and have weak adhesion characteristics to achieve composite bonding between copper foil and epoxy resin substrate.
It achieves low dielectric loss, low signal transmission attenuation, resistance to high-temperature solder thermal shock, high bonding strength, and is compatible with FPC flexible circuit board production processes. It can replace imported high-end adhesive films, reducing procurement costs and supply dependence risks in the industrial chain.
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-frequency and high-speed adhesive film technology, specifically to a high-frequency and high-speed adhesive film for FPC and its preparation method. Background Technology
[0002] With the rapid development of artificial intelligence technology, high-frequency and high-speed communication has become an indispensable core engineering technology in the modern communication field, and communication bandwidth is gradually evolving and upgrading to 400G, 800G and even 1.6T levels. High-speed optical modules are the core carrier devices of high-frequency and high-speed communication systems, while FPC flexible circuit boards and high-frequency PCB substrates are the key basic materials for optical module manufacturing. The bonding and lamination between substrate layers requires the use of special high-frequency and high-speed adhesive films.
[0004] Most domestically available ordinary adhesive films use conventional resin systems, which generally suffer from problems such as high dielectric constant, high dielectric loss, and severe attenuation of high-frequency signal transmission. At the same time, they have insufficient resistance to high-temperature solder impact and low peel strength to copper foil, making them difficult to adapt to the production process and performance requirements of high-frequency FPCs and high-speed optical modules. They cannot replace imported high-end adhesive films. To solve the current situation of dependence on imports for high-end high-frequency adhesive films, this invention provides a high-frequency and high-speed adhesive film for FPCs and its preparation method. Summary of the Invention
[0005] The purpose of this invention is to provide a high-frequency, high-speed adhesive film for FPC and its preparation method, so as to solve the problems mentioned in the background art.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a high-frequency, high-speed adhesive film for FPC, comprising a high-frequency, high-speed adhesive film body, wherein the high-frequency, high-speed adhesive film body is made by blending modified HDPE resin and functional additives, and by weight, the modified HDPE resin is composed of the following raw materials: 100 parts of high-density polyethylene (HDPE), 4-8 parts of hydroxyethyl acrylate, 2-6 parts of acrylic acid, and 0.2-0.5 parts of dicumyl peroxide;
[0007] Based on 100 parts of modified HDPE resin, the functional additive is composed of the following raw materials: 10-50 parts of diphenylmethane-type bismaleimide, 10-50 parts of diallyl bisphenol A, 2-3 parts of 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, and 0.5-2 parts of benzoyl peroxide.
[0008] Optionally, the thickness of the finished adhesive film is 30-35 μm, and the dielectric constant DK of the adhesive film is 2.5-2.8 and the dielectric loss DF is 0.0008-0.0013 at a frequency of 10 GHz.
[0009] Optionally, after being baked and cured at a constant temperature of 180°C for 60 minutes, the adhesive film can withstand a solder thermal shock of 300°C for 10 seconds, and the 90° peel strength between the adhesive film and the copper foil is 1.2-1.5 kg / cm.
[0010] A method for preparing a high-frequency, high-speed adhesive film for FPC, specifically comprising the following steps:
[0011] S1. Preparation of modified HDPE resin: High-density polyethylene, hydroxyethyl acrylate, acrylic acid and dicumyl peroxide are mixed evenly according to the formula ratio, and put into a twin-screw extruder for melt reaction, extrusion and granulation to obtain modified HDPE resin granules.
[0012] S2. Preparation of film composite granules: The modified HDPE resin obtained in step S1 is mixed evenly with diphenylmethane type bismaleimide, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butylperoxide and benzoyl peroxide, and then fed into a single screw extruder for melt extrusion, water cooling and pelletizing to obtain film composite plastic granules.
[0013] S3. The adhesive film composite particles prepared in step S2 are fed into a casting machine to be cast into an initial film, and then pressed into a high-frequency high-speed adhesive film of a set thickness through a multi-pass calendering process.
[0014] Optionally, in step S1, the screw length-to-diameter ratio of the twin-screw extruder is 33:1, the screw speed is set to 25 r / min, and the processing temperatures of each section of the extruder are 140℃, 170℃, 190℃, 190℃, 190℃, 190℃, and 185℃ respectively.
[0015] Optionally, in step S2, the screw length-to-diameter ratio of the single-screw extruder is 30:1, and the temperatures of each extrusion granulation section are 150℃, 145℃, 145℃, 140℃, and 140℃ respectively.
[0016] Optionally, the adhesive film obtained in step S3 has weak adhesive properties, which can realize the composite bonding of copper foil and epoxy resin substrate.
[0017] Optionally, in step S2, the water-cooled pelletized composite particles are air-dried to remove water, and the moisture content of the particles is controlled to be less than 0.05% to avoid residual moisture affecting the dielectric and adhesive properties of the film.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] 1. This invention uses high-density polyethylene graft modification to obtain modified HDPE resin, and then combines it with diphenylmethane-type bismaleimide, diallyl bisphenol A and a composite initiator to construct a film system. The resulting film has excellent low dielectric and low loss characteristics. At a frequency of 10 GHz, the dielectric constant DK is 2.5-2.8 and the dielectric loss DF is as low as 0.0008-0.0013, which can significantly reduce the attenuation of high-frequency signal transmission and meet the high-frequency and high-speed signal transmission requirements of 400G-800G high-speed optical modules.
[0020] 2. The high-frequency, high-speed adhesive film prepared by this invention can withstand the thermal shock of soldering at 300°C for 10 seconds after being baked and cured at a constant temperature of 180°C for 60 minutes. It has excellent thermal stability and is suitable for the process requirements of hot pressing, reflow soldering and other processes in the production of FPC flexible circuit boards. It is not prone to defects such as delamination, blistering and peeling. The 90° peel strength between the adhesive film and the copper foil can reach 1.2-1.5 kg / cm. It has high bonding strength and good interfacial bonding stability. At the same time, the surface of the adhesive film has weak adhesive properties, which can directly realize the composite bonding of copper foil and epoxy resin substrate without additional primer treatment. It has strong processing adaptability.
[0021] 3. This invention defines the process parameters for the modified resin, film particles, and the entire film-forming process. It adopts a twin-screw modified granulation, a single-screw extrusion pelletizing, and multiple calendering molding with casting. The process route is simple and controllable, and the production parameters are stable, making it suitable for industrial-scale mass production. At the same time, an air-drying and dehydration treatment is added after granulation to strictly control the moisture content of the particles, avoid residual moisture from degrading the dielectric and adhesive properties of the film, and improve the batch stability of the product. In addition, the developed high-frequency and high-speed film can completely replace imported similar products, realize the localization of high-end high-frequency film materials, and effectively reduce the procurement costs and supply dependence risks of the industrial chain. Detailed Implementation
[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Example 1
[0024] A high-frequency, high-speed adhesive film for FPC includes a high-frequency, high-speed adhesive film body. The high-frequency, high-speed adhesive film body is made by blending modified HDPE resin and functional additives. By weight, the modified HDPE resin is composed of the following raw materials: 100 parts of high-density polyethylene (HDPE), 4 parts of hydroxyethyl acrylate, 2 parts of acrylic acid, and 0.2 parts of dicumyl peroxide. Based on 100 parts of modified HDPE resin, the functional additives are composed of the following raw materials: 10 parts of diphenylmethane-type bismaleimide, 10 parts of diallyl bisphenol A, 2 parts of 2,5-dimethyl-2,5-di-tert-butylperoxide, and 0.5 parts of benzoyl peroxide.
[0025] A method for preparing a high-frequency, high-speed adhesive film for FPC, specifically including the following steps:
[0026] S1. Preparation of modified HDPE resin: High-density polyethylene, hydroxyethyl acrylate, acrylic acid and dicumyl peroxide are mixed evenly according to the formula ratio, and put into a twin-screw extruder for melt reaction, extrusion and granulation to obtain modified HDPE resin granules. The screw length-to-diameter ratio of the twin-screw extruder is 33:1, the screw speed is set to 25 r / min, and the processing temperatures of each section of the extruder are 140℃, 170℃, 190℃, 190℃, 190℃, 190℃ and 185℃ respectively.
[0027] S2. Preparation of film composite granules: The modified HDPE resin obtained in step S1 is mixed evenly with diphenylmethane-type bismaleimide, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butylperoxide, and benzoyl peroxide. The mixture is then fed into a single-screw extruder for melt extrusion and water-cooled pelletizing to obtain film composite plastic granules. The screw length-to-diameter ratio of the single-screw extruder is 30:1. The extrusion granulation temperatures are 150℃, 145℃, 145℃, 140℃, and 140℃ respectively. After water-cooled pelletizing, the film composite granules are air-dried to remove water, and the moisture content of the granules is controlled to be below 0.05% to avoid residual moisture affecting the dielectric and adhesive properties of the film.
[0028] S3. The adhesive film composite particles prepared in step S2 are fed into a casting machine to be cast into an initial film, and then pressed into a high-frequency high-speed adhesive film of a set thickness through a multi-pass calendering process. The surface of the adhesive film has weak adhesion characteristics, which can realize the composite bonding of copper foil and epoxy resin substrate.
[0029] The finished film has a thickness of 30-35μm. At a frequency of 10GHz, the dielectric constant DK is 2.5-2.8 and the dielectric loss DF is 0.0008-0.0013.
[0030] Example 2
[0031] A high-frequency, high-speed adhesive film for FPC includes a high-frequency, high-speed adhesive film body. The high-frequency, high-speed adhesive film body is made by blending modified HDPE resin and functional additives. By weight, the modified HDPE resin is composed of the following raw materials: 100 parts of high-density polyethylene (HDPE), 6 parts of hydroxyethyl acrylate, 4 parts of acrylic acid, and 0.35 parts of dicumyl peroxide. Based on 100 parts of modified HDPE resin, the functional additives are composed of the following raw materials: 30 parts of diphenylmethane-type bismaleimide, 30 parts of diallyl bisphenol A, 2.5 parts of 2,5-dimethyl-2,5-di-tert-butylperoxide, and 1.5 parts of benzoyl peroxide.
[0032] A method for preparing a high-frequency, high-speed adhesive film for FPC, specifically including the following steps:
[0033] S1. Preparation of modified HDPE resin: High-density polyethylene, hydroxyethyl acrylate, acrylic acid and dicumyl peroxide are mixed evenly according to the formula ratio, and put into a twin-screw extruder for melt reaction, extrusion and granulation to obtain modified HDPE resin granules. The screw length-to-diameter ratio of the twin-screw extruder is 33:1, the screw speed is set to 25 r / min, and the processing temperatures of each section of the extruder are 140℃, 170℃, 190℃, 190℃, 190℃, 190℃ and 185℃ respectively.
[0034] S2. Preparation of film composite granules: The modified HDPE resin obtained in step S1 is mixed evenly with diphenylmethane-type bismaleimide, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butylperoxide, and benzoyl peroxide. The mixture is then fed into a single-screw extruder for melt extrusion and water-cooled pelletizing to obtain film composite plastic granules. The screw length-to-diameter ratio of the single-screw extruder is 30:1. The extrusion granulation temperatures are 150℃, 145℃, 145℃, 140℃, and 140℃ respectively. After water-cooled pelletizing, the film composite granules are air-dried to remove water, and the moisture content of the granules is controlled to be below 0.05% to avoid residual moisture affecting the dielectric and adhesive properties of the film.
[0035] S3. The adhesive film composite particles prepared in step S2 are fed into a casting machine to be cast into an initial film, and then pressed into a high-frequency high-speed adhesive film of a set thickness through a multi-pass calendering process. The surface of the adhesive film has weak adhesion characteristics, which can realize the composite bonding of copper foil and epoxy resin substrate.
[0036] The finished film has a thickness of 30-35μm. At a frequency of 10GHz, the dielectric constant DK is 2.5-2.8 and the dielectric loss DF is 0.0008-0.0013.
[0037] Example 3
[0038] A high-frequency, high-speed adhesive film for FPC includes a high-frequency, high-speed adhesive film body. The high-frequency, high-speed adhesive film body is made by blending modified HDPE resin and functional additives. By weight, the modified HDPE resin is composed of the following raw materials: 100 parts of high-density polyethylene (HDPE), 8 parts of hydroxyethyl acrylate, 6 parts of acrylic acid, and 0.5 parts of dicumyl peroxide. Based on 100 parts of modified HDPE resin, the functional additives are composed of the following raw materials: 50 parts of diphenylmethane-type bismaleimide, 50 parts of diallyl bisphenol A, 3 parts of 2,5-dimethyl-2,5-di-tert-butylperoxide, and 2 parts of benzoyl peroxide.
[0039] A method for preparing a high-frequency, high-speed adhesive film for FPC, specifically including the following steps:
[0040] S1. Preparation of modified HDPE resin: High-density polyethylene, hydroxyethyl acrylate, acrylic acid and dicumyl peroxide are mixed evenly according to the formula ratio, and put into a twin-screw extruder for melt reaction, extrusion and granulation to obtain modified HDPE resin granules. The screw length-to-diameter ratio of the twin-screw extruder is 33:1, the screw speed is set to 25 r / min, and the processing temperatures of each section of the extruder are 140℃, 170℃, 190℃, 190℃, 190℃, 190℃ and 185℃ respectively.
[0041] S2. Preparation of film composite granules: The modified HDPE resin obtained in step S1 is mixed evenly with diphenylmethane-type bismaleimide, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butylperoxide, and benzoyl peroxide. The mixture is then fed into a single-screw extruder for melt extrusion and water-cooled pelletizing to obtain film composite plastic granules. The screw length-to-diameter ratio of the single-screw extruder is 30:1. The extrusion granulation temperatures are 150℃, 145℃, 145℃, 140℃, and 140℃ respectively. After water-cooled pelletizing, the film composite granules are air-dried to remove water, and the moisture content of the granules is controlled to be below 0.05% to avoid residual moisture affecting the dielectric and adhesive properties of the film.
[0042] S3. The adhesive film composite particles prepared in step S2 are fed into a casting machine to be cast into an initial film, and then pressed into a high-frequency high-speed adhesive film of a set thickness through a multi-pass calendering process. The surface of the adhesive film has weak adhesion characteristics, which can realize the composite bonding of copper foil and epoxy resin substrate.
[0043] The finished film has a thickness of 30-35μm. At a frequency of 10GHz, the dielectric constant DK is 2.5-2.8 and the dielectric loss DF is 0.0008-0.0013.
[0044] As can be seen from the above three embodiments, Embodiment 2 is the optimal embodiment under the overall formulation system. The proportions of each raw material are balanced, and the overall performance of the adhesive film dielectric properties, bonding strength, solder thermal shock resistance and processing adaptability is the best. It is suitable for industrial mass production and bonding applications of high-frequency FPC and high-speed optical module substrates.
[0045] Example 4
[0046] A method for preparing a high-frequency, high-speed adhesive film for FPC includes the following raw material ratios and preparation process:
[0047] Weigh out 100 parts of high-density polyethylene (HDPE), 4 parts of hydroxyethyl acrylate, and 0.2 parts of dicumyl peroxide by weight. Mix them evenly and then add them to a twin-screw extruder for melt reaction and granulation. Set the temperature of each section of the twin-screw extruder to 140℃, 170℃, 175℃, 190℃, 190℃, and 170℃ respectively to obtain modified HDPE resin.
[0048] Take 100 parts of the above modified HDPE resin, 20 parts of diphenylmethane bismaleimide, and 20 parts of diallyl bisphenol A, mix them evenly, and then extrude them at 140°C to form an initial film. Then, through multiple calendering processes, a high-frequency high-speed adhesive film with a thickness of 35μm is produced.
[0049] The adhesive film prepared in this embodiment has weak adhesion, which can directly achieve the bonding and composite of copper foil and epoxy resin substrate. After the adhesive film is cured by constant temperature baking at 180°C for 60 minutes, it can withstand the solder thermal shock of 300°C for 10 seconds.
[0050] Performance testing: At a frequency of 10MHz, the dielectric constant DK of the adhesive film is 2.8-3.3, the dielectric loss DF is 0.003-0.006, and the 90° peel strength between the adhesive film and the copper foil is 1.2-1.5 kg / cm.
[0051] The adhesive film in this embodiment is suitable for 400 Mbps bandwidth FPC production.
[0052] Example 5
[0053] A method for preparing a high-frequency, high-speed adhesive film for FPC includes the following raw material ratios and process steps:
[0054] High-density polyethylene (HDPE) with a melt index of 40 was selected. 100 parts HDPE, 3 parts hydroxyethyl acrylate, and 0.3 parts dicumyl peroxide were taken by weight, mixed evenly, and fed into a twin-screw extruder for melt reaction to obtain modified HDPE resin.
[0055] Take 100 parts by weight of the above modified HDPE resin, 10 parts of diphenylmethane-type bismaleimide, 10 parts of diallyl bisphenol A, and 3 parts of 2,5-dimethyl-2,5-di-tert-butylperoxide, mix them evenly, and put them into a film extruder to extrude and form an initial film with a thickness of 0.3 mm. Then, press it into a high-frequency high-speed adhesive film with a thickness of 30 μm through multiple calendering processes. Except for the proportions and calendering thickness, the other preparation processes, air drying and dehydration and thermal shock resistance conditions are the same as those in Example 4.
[0056] Performance testing: At a frequency of 1MHz, the dielectric constant DK of the adhesive film is 2.7, the dielectric loss DF is 0.0025, and the 90° peel strength between the adhesive film and the copper foil is 1.2kg / cm.
[0057] The adhesive film in this embodiment is suitable for the production of 800 MHz FPC circuits.
[0058] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A high-frequency high-speed adhesive film for FPC, characterized by: The product includes a high-frequency, high-speed adhesive film body, which is made by blending modified HDPE resin with functional additives. By weight, the modified HDPE resin is composed of the following raw materials: 100 parts of high-density polyethylene (HDPE), 4-8 parts of hydroxyethyl acrylate, 2-6 parts of acrylic acid, and 0.2-0.5 parts of dicumyl peroxide. Based on 100 parts of modified HDPE resin, the functional additive is composed of the following raw materials: 10-50 parts of diphenylmethane-type bismaleimide, 10-50 parts of diallyl bisphenol A, 2-3 parts of 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, and 0.5-2 parts of benzoyl peroxide.
2. The high-frequency high-speed adhesive film for FPC according to claim 1, characterized by: The finished adhesive film has a thickness of 30-35 μm, and at a frequency of 10 GHz, the dielectric constant DK is 2.5-2.8 and the dielectric loss DF is 0.0008-0.0013.
3. The high-frequency high-speed adhesive film for FPC according to claim 2, characterized by: After being baked and cured at a constant temperature of 180°C for 60 minutes, the adhesive film can withstand the thermal shock of soldering at 300°C for 10 seconds. The 90° peel strength between the adhesive film and the copper foil is 1.2-1.5 kg / cm.
4. A method for preparing a high-frequency high-speed adhesive film for an FPC, characterized by, The method for preparing the high-frequency, high-speed adhesive film for FPC according to any one of claims 1-3 specifically includes the following steps: S1. Preparation of modified HDPE resin: High-density polyethylene, hydroxyethyl acrylate, acrylic acid and dicumyl peroxide are mixed evenly according to the formula ratio, and put into a twin-screw extruder for melt reaction, extrusion and granulation to obtain modified HDPE resin granules. S2. Preparation of film composite granules: The modified HDPE resin obtained in step S1 is mixed evenly with diphenylmethane type bismaleimide, diallyl bisphenol A, 2,5-dimethyl-2,5-di-tert-butylperoxide and benzoyl peroxide, and then fed into a single screw extruder for melt extrusion, water cooling and pelletizing to obtain film composite plastic granules. S3. The adhesive film composite particles prepared in step S2 are fed into a casting machine to be cast into an initial film, and then pressed into a high-frequency high-speed adhesive film of a set thickness through a multi-pass calendering process.
5. The method for preparing high-frequency, high-speed adhesive film for FPC according to claim 4, characterized in that: In step S1, the screw length-to-diameter ratio of the twin-screw extruder is 33:1, the screw speed is set to 25 r / min, and the processing temperatures of each section of the extruder are 140℃, 170℃, 190℃, 190℃, 190℃, 190℃, and 185℃ respectively.
6. The method for preparing a high-frequency, high-speed adhesive film for FPC according to claim 4, characterized in that: In step S2, the screw length-to-diameter ratio of the single-screw extruder is 30:1, and the temperatures of each extrusion granulation section are 150℃, 145℃, 145℃, 140℃, and 140℃ respectively.
7. The method for preparing a high-frequency, high-speed adhesive film for FPC according to claim 4, characterized in that: The adhesive film obtained in step S3 has weak adhesive properties, which can realize the composite bonding of copper foil and epoxy resin substrate.
8. The method for preparing high-frequency, high-speed adhesive film for FPC according to claim 4, characterized in that: In step S2, the water-cooled pelletized composite particles are air-dried to remove moisture, and the moisture content of the particles is controlled to be below 0.05% to avoid residual moisture affecting the dielectric and adhesive properties of the film.