Glue for nylon and polypropylene (PP) multi-layer composite pipeline and preparation method thereof
By combining EVA, EAA, PP-g-MAH and nylon oligomers, the problems of insufficient adhesion, large difference in interfacial modulus, and insufficient hydrolysis resistance in multilayer composite pipes of nylon and polypropylene (PP) are solved, achieving high-strength adhesion and environmental resistance, and making it suitable for the molding process of multilayer pipes.
Patent Information
- Application Number
- CN202611512530.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
In multilayer composite pipes made of nylon and polypropylene (PP), existing adhesives suffer from insufficient adhesion, large differences in interfacial modulus, and inadequate hydrolysis and high-temperature resistance, leading to easy peeling and delamination between layers.
An adhesive is prepared by combining ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), grafted modified polypropylene (PP-g-MAH), and nylon oligomers through chemical bonding and physical entanglement, thereby enhancing the bonding strength and environmental resistance.
It improves the bonding strength between PA and PP layers, enhances hydrolysis resistance and high temperature resistance, improves processing fluidity, and is suitable for the molding process of multi-layer pipelines.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, specifically to an adhesive for nylon and polypropylene (PP) multilayer composite pipes and its preparation method. Background Technology
[0002] Nylon (PA) and polypropylene (PP) are two commonly used materials in multilayer composite pipes: the PA layer has excellent chemical resistance, hydrolysis resistance, and barrier properties, while the PP layer has low cost, lightweight, and impact resistance. However, PA and PP have a large difference in polarity (PA is a polar material, while PP is a non-polar material), resulting in extremely low interfacial adhesion when directly laminated, which easily leads to interlayer delamination and seriously affects pipe performance.
[0003] In existing technologies, adhesives used for PA / PP bonding mostly use EVA or EAA as a single matrix, but this has the following problems: EVA has decent adhesion to PP, but insufficient adhesion to polar PA. EAA has strong adhesion to PA, but poor wettability to PP and insufficient processing fluidity. The large difference in interfacial modulus between unmodified PP and PA can easily lead to stress concentration and bonding failure. Traditional adhesives lack hydrolysis resistance and high temperature resistance, and are prone to delamination under long-term use in humid and hot environments. To address this, we propose an adhesive for multilayer composite pipes made of nylon and polypropylene (PP) and its preparation method. Summary of the Invention
[0004] The purpose of this invention is to provide an adhesive for multilayer composite pipes made of nylon and polypropylene (PP) and its preparation method, in order to solve the problems mentioned in the background art, such as: EVA has acceptable adhesion to PP, but insufficient adhesion to polar PA; EAA has strong adhesion to PA, but poor wetting properties to PP and insufficient processing fluidity; large difference in interfacial modulus between unmodified PP and PA, which easily leads to stress concentration and adhesion failure; and traditional adhesives have insufficient hydrolysis resistance and high temperature resistance, making them prone to delamination under long-term use in humid and hot environments.
[0005] To achieve the above objectives, the present invention provides the following technical solution: an adhesive for nylon and polypropylene (PP) multilayer composite pipes, comprising the following components by weight: ethylene-vinyl acetate copolymer (EVA): 30-50 parts, wherein the vinyl acetate (VA) content is ≥28 wt%; Ethylene-acrylic acid copolymer (EAA): 20-40 parts, wherein the acrylic acid (AA) content is ≥28 wt%; Graft-modified polypropylene (PP-g-MAH): 10-30 parts, grafting rate ≥0.8wt%; Nylon oligomer: 5-15 parts, number average molecular weight 500-5000 g / mol; wt% refers to the total mass of each copolymer itself.
[0006] Furthermore, the EVA has a VA content of 28-40 wt% and a melt flow rate of 2-20 g / 10 min.
[0007] Furthermore, the AA content of the EAA is 28-35 wt%, and the melt flow rate is 1-15 g / 10 min.
[0008] Furthermore, the matrix polypropylene of the PP-g-MAH is homopolymer PP or copolymer PP, and the melt flow rate is 0.5-10 g / 10 min.
[0009] Furthermore, the nylon oligomer is a carboxyl-terminated nylon 6 oligomer or an amino-terminated nylon 66 oligomer.
[0010] The method for preparing the adhesive for the nylon and polypropylene (PP) multilayer composite pipe includes the following steps: (1) Add EVA, EAA and PP-g-MAH to a high-speed mixer in proportion and mix at 60-80℃ for 5-15 minutes; (2) Add nylon oligomer and continue mixing for 3-8 minutes; (3) Add the mixture to a twin-screw extruder, melt-blend and extrude at 160-220℃, granulate and dry to obtain the bonding resin.
[0011] Furthermore, the screw speed of the twin-screw extruder is 200-400 rpm, and the length-to-diameter ratio is ≥32:1. Furthermore, prior to the melt blending extrusion in step (3), a pretreatment step of the raw materials is also included: Ethylene-acrylic acid copolymer (EAA) and nylon oligomer are pre-reacted in an internal mixer at a temperature of 140-170°C, a rotor speed of 40-80 rpm, and a processing time of 3-10 min. This process causes partial neutralization of the terminal amino groups of the nylon oligomer with the carboxyl groups of EAA, resulting in the formation of an ionic cluster structure.
[0012] This invention provides an adhesive for nylon and polypropylene (PP) multilayer composite pipes and its preparation method, which has the following beneficial effects: This invention achieves strong adhesion to the PA layer through chemical bonding between EAA and PA, covalent bonding between PP-g-MAH and PA, and interfacial compatibilization of nylon oligomers; at the same time, the PP backbone of EVA and PP-g-MAH is physically entangled with the PP layer, thereby improving the peel strength. The hydrophobic backbones of EVA and EAA endow the bonding resin with good hydrolysis resistance; the introduction of PP-g-MAH improves high temperature resistance; and the low melt viscosity of EVA improves processing fluidity, making it suitable for extrusion, coating and other processes. Detailed Implementation
[0013] The embodiments of the present invention will be described in further detail below with reference to examples. These examples are for illustrative purposes only and should not be construed as limiting the scope of the invention.
[0014] Example 1 Adhesive resin formulation (parts by weight): EVA (VA=28%, melt flow rate=5g / 10min): 40 parts; EAA (AA=30%, melt flow rate=8g / 10min): 30 parts; PP-g-MAH (grafting rate 1.0%, melt flow rate=3g / 10min): 20 parts; terminal carboxyl nylon 6 oligomer (Mn=2000g / mol): 10 parts.
[0015] Preparation steps: (1) Add EVA, EAA, and PP-g-MAH to a high-speed mixer and mix at 70°C for 10 minutes; (2) Add nylon 6 oligomer and continue mixing for 5 minutes; (3) Twin-screw extruder (length-to-diameter ratio 36:1) temperature settings: Zone 1 160℃, Zone 2 180℃, Zone 3 200℃, Zone 4 210℃, Zone 5 200℃, die head 190℃; screw speed 300rpm, extrusion granulation, drying (vacuum drying at 60℃ for 4h) to obtain bonding resin, i.e. glue.
[0016] Example 2 Adhesive resin formulation (parts by weight): EVA (VA=35%, melt flow rate=2g / 10min): 30 parts; EAA (AA=28%, melt flow rate=12g / 10min): 40 parts; PP-g-MAH (grafting rate 0.8%, melt flow rate=5g / 10min): 15 parts; amino-terminated nylon 66 oligomer (Mn=1000g / mol): 15 parts.
[0017] The preparation steps are the same as in Example 1, with the twin-screw temperature set to 150-210℃.
[0018] Example 3 Adhesive resin formulation (parts by weight): EVA (VA=40%, melt flow rate=10g / 10min): 50 parts; EAA (AA=32%, melt flow rate=5g / 10min): 20 parts; PP-g-MAH (grafting rate 1.2%, melt flow rate=1g / 10min): 25 parts; terminal carboxyl nylon 6 oligomer (Mn=500g / mol): 5 parts.
[0019] The preparation steps are the same as in Example 1.
[0020] Comparative Example 1 It contains only EVA (VA=28%) and PP-g-MAH, and no EAA or nylon oligomers.
[0021] Comparative Example 2 It contains only EAA (AA=30%) and PP-g-MAH, and no EVA or nylon oligomers.
[0022] Performance Testing: The bonding resins prepared in the examples and comparative examples were used for hot-pressing PA66 boards and PP boards, respectively, and their peel strength, hydrolysis resistance, and processing flowability were tested under the same conditions. The results showed that the peel strength of the example sample containing EAA and nylon oligomers was significantly higher than that of the comparative example containing only a single matrix. After high-temperature and high-humidity aging, the example sample still maintained high bonding strength, and its hydrolysis resistance was significantly better than that of the comparative example. At the same time, the example sample had a higher melt flow rate, exhibiting better processing flowability and being more suitable for multilayer pipeline molding processes such as extrusion and coating.
[0023] This invention significantly improves the bonding strength and environmental resistance of PA and PP through the synergistic effect of EVA, EAA, PP-g-MAH and nylon oligomers, and has excellent processing fluidity, thus overcoming the shortcomings of the prior art.
[0024] The embodiments of the present invention are given for illustrative and descriptive purposes only, and are not intended to be exhaustive or to limit the invention to the forms disclosed. Many modifications and variations will be apparent to those skilled in the art. The embodiments were chosen and described in order to better illustrate the principles and practical application of the invention, and to enable those skilled in the art to understand the invention and to design various embodiments with various modifications suitable for a particular purpose.
Claims
1. An adhesive for use in multilayer composite pipes of nylon and polypropylene (PP), characterized in that, It consists of the following components in parts by weight: Ethylene-vinyl acetate copolymer (EVA): 30-50 parts, wherein the vinyl acetate (VA) content is ≥28 wt%; Ethylene-acrylic acid copolymer (EAA): 20-40 parts, wherein the acrylic acid (AA) content is ≥28 wt%; Graft-modified polypropylene (PP-g-MAH): 10-30 parts, grafting rate ≥0.8wt%; Nylon oligomers: 5-15 parts, number average molecular weight 500-5000 g / mol.
2. The adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 1, characterized in that, The EVA has a VA content of 28-40 wt% and a melt flow rate of 2-20 g / 10 min.
3. The adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 1, characterized in that, The AA content of the EAA is 28-35wt%, and the melt flow rate is 1-15g / 10min.
4. The adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 1, characterized in that, The matrix polypropylene of the PP-g-MAH is homopolymer PP or copolymer PP, and the melt flow rate is 0.5-10g / 10min.
5. The adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 1, characterized in that, The nylon oligomer is a carboxyl-terminated nylon 6 oligomer or an amino-terminated nylon 66 oligomer.
6. A method for preparing the adhesive for the nylon and polypropylene (PP) multilayer composite pipe as described in claim 5, characterized in that, Includes the following steps: (1) Add EVA, EAA and PP-g-MAH to a high-speed mixer in proportion and mix at 60-80℃ for 5-15 minutes; (2) Add nylon oligomer and continue mixing for 3-8 minutes; (3) Add the mixture to a twin-screw extruder, melt-blend and extrude at 160-220℃, granulate and dry to obtain the bonding resin.
7. The method for preparing the adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 6, characterized in that, The twin-screw extruder has a screw speed of 200-400 rpm and a length-to-diameter ratio of ≥32:
1.
8. The method for preparing the adhesive for nylon and polypropylene (PP) multilayer composite pipes according to claim 6, characterized in that, Before the melt blending extrusion in step (3), a pretreatment step for the raw materials is also included: the ethylene-acrylic acid copolymer (EAA) and the nylon oligomer are pre-reacted in a mixer at a temperature of 140~170℃, a rotor speed of 40~80rpm, and a treatment time of 3~10min, so that the terminal amino groups of the nylon oligomer and the carboxyl groups of EAA undergo a partial neutralization reaction to generate an ionic cluster structure.