A sealant for road crack repair

A solvent-free sealant was prepared by combining components A and B, which solved the problem of existing sealants being easily combustible at high temperatures and achieved a road crack repair effect with high flame retardancy and strong mechanical properties.

CN123152425APending Publication Date: 2026-11-24REED XINXIANG ROAD INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611535687.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing road crack repair sealants are flammable under high temperatures and lack flame retardancy, posing a risk of fire spread.

Method used

The sealant is prepared by combining components A and B. Component A is a flame retardant additive generated by the reaction of PEPA with tetra(2-chloroethyl) ethylidene diphosphate and a reducing agent of 4-hydroxybenzaldehyde. Component B is a silanol generated by the reaction of γ-aminopropyltriethoxysilane with 4,4'-diphenylmethane diisocyanate. The sealant is prepared by simple cross-linking and curing.

Benefits of technology

The prepared sealant has a high solids mass fraction, requires no crosslinking aids or catalysts, has suitable viscosity and mechanical strength, and also has high flame retardancy and strong mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a sealant for repairing road cracks, belonging to the field of sealants. This invention addresses the technical problem of poor flame retardancy in existing sealants used for road crack repair. The sealant for road crack repair comprises component A and component B; component A is a reaction reducing agent of PEPA, tetrakis(2-chloroethyl)ethylene diphosphate, and 4-hydroxybenzaldehyde; component B is a reaction product of hydrolyzed silanol and 4,4'-diphenylmethane diisocyanate. The sealant contains only components A and B. By adjusting the raw material composition and relative molecular mass of the two components, it achieves suitable viscosity and mechanical strength at room temperature without the need for crosslinking aids and catalysts. Components A and B of the sealant can be combined through a simple crosslinking and curing reaction to obtain a high-quality sealant with high flame retardancy and strong mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sealant technology, and more specifically to a sealant for repairing road cracks.

[0002] Background technology.

[0003] With the continuous advancement of infrastructure construction and the nationwide coverage of road construction, the demand for road construction has diversified, and the complexity of construction has increased accordingly. Water seepage is a common problem in road construction. Seepage often occurs at construction joints and lining cracks, severely affecting the stability and safety of the road structure. Grouting and filling with sealant materials is an effective solution. Grouting materials need to be easy to control, have high bonding strength, and strong permeability to achieve good results in practical engineering applications.

[0004] For example, patent application CN105199666A discloses a sealant for repairing road cracks. The sealant comprises base asphalt, fine rubber powder, fossil powder, SBS modified asphalt, styrene-butadiene rubber powder, activator, tackifier, and diesel fuel. This sealant possesses advantages such as sealing properties, high-strength adhesion, and good low-temperature adhesion, and can be widely used for crack filling and repair of asphalt pavements such as asphalt, concrete highways, and airport runways.

[0005] Patent application CN1376756A discloses a road crack sealant. The road crack sealant comprises petroleum asphalt, SBS, tackifying resin, asphalt anti-stripping agent, rubber antioxidant, and toluene. This road crack sealant exhibits excellent aging resistance and will not soften or deform under high-temperature conditions.

[0006] However, on asphalt roads adjacent to vehicles, ordinary non-flame-retardant road crack repair sealants, being polymer materials, are prone to intense combustion under high temperatures. If the prepared road crack repair sealant possesses a certain degree of flame retardancy, the spread of fire can be prevented from the source.

[0007] To address this technical deficiency, a solution is proposed. Summary of the Invention

[0008] The purpose of this invention is to provide a sealant for repairing road cracks, which solves the technical problem that ordinary road crack repair sealants in the prior art have poor flame retardancy.

[0009] The objective of this invention can be achieved through the following technical solutions: A sealant for repairing road cracks, comprising component A and component B; Component A is a reaction reduction product of PEPA, tetra(2-chloroethyl) ethylidene diphosphate and 4-hydroxybenzaldehyde; Component B is a reaction product of hydrolyzed silanol and 4,4'-diphenylmethane diisocyanate.

[0010] Furthermore, the preparation method of component A includes the following steps: A1, PEPA, NaH and acetonitrile are mixed, and tetra(2-chloroethyl) ethylidene diphosphate is added. The mixture is heated and stirred at 50-60℃, and then refluxed at 80-85℃ for 6-8 hours. After cooling, the mixture is filtered and the solid is collected. The solid is washed and dried to constant weight, which is the prepared flame retardant additive. PEPA undergoes a nucleophilic substitution reaction with tetra(2-chloroethyl)ethylidene diphosphate to yield a flame retardant additive.

[0011] A2. Under inert gas protection, 4-hydroxybenzaldehyde solution is added dropwise to sodium hydride to form a reaction system; the reaction system is reacted at 65-75℃ for 40-48h, and the intermediate product is obtained by recrystallization with ethyl acetate; a mixed solvent is added to the intermediate product, and then sodium borohydride is added, and the mixture is stirred at room temperature until the sodium borohydride is completely dissolved, and the component A is prepared by recrystallization with ethanol.

[0012] Excess halogens in the flame retardant additive can undergo nucleophilic substitution with 4-hydroxybenzaldehyde, and the aldehyde group of the intermediate product is then reduced to an alcohol hydroxyl group, which is the prepared component A.

[0013] Further, in step A1, the ratio of PEPA, NaH, acetonitrile and tetra(2-chloroethyl) ethylene diphosphate is 1.8-3.6g:0.3-0.5g:50-60mL:5-10g.

[0014] Further, in step A2, the ratio of sodium hydride to 4-hydroxybenzaldehyde solution is 20-30g:7-14g, and the ratio of intermediate product, mixed solvent, and sodium borohydride is 10-20g:60-80mL:25-35g; the ratio of intermediate product to mixed solvent is 10-20g:60-80mL.

[0015] Furthermore, the preparation method of component B includes the following steps: γ-aminopropyltriethoxysilane is mixed with deionized water and hydrolyzed to obtain γ-aminopropyltriethoxysilanol; silanol is mixed with liquid 4,4'-diphenylmethane diisocyanate and reacted to form component B.

[0016] Methoxysilanes can be hydrolyzed to generate silanols, which can then undergo nucleophilic addition reactions with isocyanate groups to form component B with a Si-OC structure.

[0017] Furthermore, the ratio of γ-aminopropyltriethoxysilane to deionized water is 11-22g:2-3mL, and the ratio of silanol to liquid 4,4'-diphenylmethane diisocyanate is 12-24g:25-50g.

[0018] Furthermore, the mass ratio of component A to component B is 1:2-3.

[0019] The present invention has the following beneficial effects: 1. The road crack repair adhesive prepared by this invention is a solvent-free sealant with a high solids content. The sealant consists of only components A and B. By adjusting the raw material composition and relative molecular mass of the two components, it achieves suitable viscosity and mechanical strength at room temperature without the need for crosslinking aids and catalysts. In this invention, the NCO / OH molar ratio of the two components is greater than or equal to 1. The excess -NCO groups can chemically react with the crosslinking aids, further improving the cohesive strength of the adhesive layer.

[0020] 2. Component A contains cage-like phosphate esters, phosphate esters, alkyl side chains, benzene rings, and hydroxyl structures. Component A not only possesses flame retardancy and is reactive with isocyanates, but also has a high molecular weight. Component B has multiple benzene rings and alkyl side chains. Components A and B, through simple crosslinking and curing reactions, can yield a high-quality sealant with high flame retardancy and strong mechanical properties. Detailed Implementation

[0021] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0022] Example 1 This embodiment provides a component A for a sealant used in road crack repair, comprising the following steps: A1. Take a 250 mL three-necked flask, add 1.8 g of PEPA and 0.3 g of NaH, then add 50 mL of acetonitrile solution and 5 g of tetra(2-chloroethyl)ethylidene diphosphate. Heat and stir at 50 °C for 10 min, then reflux at 80 °C for 6 h. Cool, filter, and collect the solid. Wash the solid successively with deionized water and anhydrous ethanol, then dry it in a constant temperature drying oven to constant weight, which is the prepared flame retardant additive.

[0023] A2. Add 7g of flame retardant to a 250mL three-necked flask equipped with a mechanical stirrer, reflux condenser, and nitrogen protection. Then add 20g of sodium hydride to the flask, followed by dropwise addition of a 4-hydroxybenzaldehyde solution (obtained by dissolving 1.2g of 4-hydroxybenzaldehyde in 10mL of THF solvent). The addition should be completed within 1 hour to form a reaction system. React the system at 65℃ for 40 hours. After the reaction is complete, recrystallize from ethyl acetate to obtain an intermediate product. Mix THF and 25wt% formaldehyde aqueous solution at a volume ratio of 1:1 to form a mixed solvent. Add 10g of the intermediate product to 60mL of the mixed solvent, then add 25g of sodium borohydride. Stir at room temperature until the sodium borohydride is completely dissolved, and then recrystallize from 90% (v / v) ethanol to prepare component A.

[0024] Example 2 This embodiment provides a component A for a sealant used in road crack repair, comprising the following steps: A1. Take a 250 mL three-necked flask, add 2.7 g of PEPA and 0.4 g of NaH, then add 55 mL of acetonitrile solution and 8 g of tetra(2-chloroethyl)ethylidene diphosphate. Heat and stir at 55 °C for 12 min, then reflux at 82 °C for 7 h. Cool, filter, and collect the solid. Wash the solid successively with deionized water and anhydrous ethanol, then dry it in a constant temperature drying oven to constant weight, which is the prepared flame retardant additive.

[0025] A2. Add 12g of flame retardant to a 250mL three-necked flask equipped with a mechanical stirrer, reflux condenser, and nitrogen protection. Then add 25g of sodium hydride to the flask, followed by dropwise addition of a 4-hydroxybenzaldehyde solution (obtained by dissolving 1.8g of 4-hydroxybenzaldehyde in 15mL of THF solvent). The addition is completed within 1.5 hours, forming a reaction system. The reaction system is reacted at 70℃ for 44 hours. After the reaction is complete, recrystallize from ethyl acetate to obtain an intermediate product. Mix THF and 20wt% de1 formaldehyde aqueous solution at a volume ratio of 1:1 to form a mixed solvent. Add 15g of the intermediate product to 70mL of the mixed solvent, then add 30g of sodium borohydride. Stir at room temperature until the sodium borohydride is completely dissolved, and then recrystallize from 90% (v / v) ethanol to prepare component A.

[0026] Example 3 This embodiment provides a component A for a sealant used in road crack repair, comprising the following steps: A1. Take a 250 mL three-necked flask, add 3.6 g of PEPA and 0.5 g of NaH, then add 60 mL of acetonitrile solution and 10 g of tetra(2-chloroethyl)ethylidene diphosphate. Heat and stir at 60 °C for 15 min, then reflux at 85 °C for 6-8 h. Cool, filter, and collect the solid. Wash the solid successively with deionized water and anhydrous ethanol, then dry it in a constant temperature drying oven to constant weight to obtain the prepared flame retardant additive.

[0027] A2. Add 14g of flame retardant to a 250mL three-necked flask. The three-necked flask is equipped with a mechanical stirrer, a reflux condenser and a nitrogen protection device. Then add 30g of sodium hydride to the three-necked flask and add 4-hydroxybenzaldehyde solution (2.4g of 4-hydroxybenzaldehyde dissolved in 20mL of THF solvent) dropwise. The addition is completed within 2h to form a reaction system. The reaction system is reacted at 75℃ for 48h. After the reaction is completed, the intermediate product is obtained by recrystallization with ethyl acetate. THF and 30wt% formaldehyde[1] aqueous solution are mixed at a volume ratio of 1:1 to form a mixed solvent. 20g of the intermediate product is added to 80mL of the mixed solvent, and then 35g of sodium borohydride is added to it. The mixture is stirred at room temperature until the sodium borohydride is completely dissolved. Then, it is recrystallized with 90% volume fraction ethanol to prepare component A.

[0028] Example 4 This embodiment provides a sealant for repairing road cracks, including the following steps: S1. Add 11g of γ-aminopropyltriethoxysilane to a beaker, then add 2mL of deionized water dropwise and mix well to obtain γ-aminopropyltriethoxysilane. Heat 25g of 4,4'-diphenylmethane diisocyanate to 55℃ until it is completely melted. Mix 12g of silane and liquid 4,4'-diphenylmethane diisocyanate, stir at 100r / min at room temperature and react for 30min to finally form component B.

[0029] S2. Add components A and B prepared in Example 1 to a beaker at a mass ratio of 1:2, mix well, and allow to cure naturally at room temperature for 10 minutes to obtain the sealant for road crack repair.

[0030] Example 5 This embodiment provides a sealant for repairing road cracks, including the following steps: S1. Add 16g of γ-aminopropyltriethoxysilane to a beaker, then add 3mL of deionized water dropwise and mix well to obtain γ-aminopropyltriethoxysilane. Heat 35g of 4,4'-diphenylmethane diisocyanate to 60℃ until it is completely melted. Mix 18g of silane and liquid 4,4'-diphenylmethane diisocyanate, stir at 150r / min at room temperature and react for 45min to finally form component B.

[0031] S2. Add components A and B prepared in Example 2 to a beaker at a mass ratio of 1:2.5, mix well, and allow to cure naturally at room temperature for 5 minutes to obtain the sealant for road crack repair.

[0032] Example 6 This embodiment provides a sealant for repairing road cracks, including the following steps: S1. Add 22g of γ-aminopropyltriethoxysilane to a beaker, then add 3mL of deionized water dropwise and mix well to obtain γ-aminopropyltriethoxysilane. Heat 50g of 4,4'-diphenylmethane diisocyanate to 65℃ until it is completely melted. Mix 24g of silane and liquid 4,4'-diphenylmethane diisocyanate, stir at 200r / min at room temperature and react for 60min to finally form component B.

[0033] S2. Add components A and B prepared in Example 3 to a beaker at a mass ratio of 1:3, mix well, and allow to cure naturally at room temperature for 10 minutes to obtain the sealant for road crack repair.

[0034] Comparative Example 1 The difference between this comparative example and Example 6 is that step A1 is omitted, and the prepared flame retardant is replaced with an equal mass of 4-hydroxybenzaldehyde.

[0035] Comparative Example 2 The difference between this comparative example and Example 6 is that step A1 is omitted, and the prepared flame retardant additive is replaced with an equal mass of tetra(2-chloroethyl) ethylidene diphosphate.

[0036] Comparative Example 3 The difference between this comparative example and Example 6 is that the components A and B prepared in Example 3 are mixed at a mass ratio of 1:1 to obtain the sealant for road crack repair.

[0037] Performance testing: 1. Place 20 mL of the sealant for road crack repair prepared in Examples 4-6 and Comparative Examples 1-3 into a 50 mL beaker, heat in a constant temperature water bath at 50°C, and stir to ensure the sealant solution reaches a uniform temperature. Then, measure its viscosity using a rotational viscometer. Perform three measurements each time and calculate the average value.

[0038] 2. According to ASTM D2240, the Shore hardness values ​​of the sealants prepared for road crack repair in Examples 4-6 and Comparative Examples 1-3 were tested sequentially. At least five valid tests were performed on the same sample, and the median of the final test results was taken.

[0039] 3. In accordance with GB / T528-2009, the sealants for road crack repair prepared in Examples 4-6 and Comparative Examples 1-3 were cut into dumbbell-shaped specimens using a cutting machine. The total length of the dumbbell specimen was 75 mm, the length of the narrow section was 25 mm, and the test length was 20 mm. At least five valid tests were performed on the same sample, and the median of the final test results was taken.

[0040] 4. Styrene-butadiene rubber was cut into standard strips with a width of 25 mm and a length of 50 mm. The standard strips were then coated and bonded with the sealants prepared in Examples 4-6 and Comparative Examples 1-3 for road crack repair, with a coating thickness of 3 mm, to obtain bonded samples. After the bonded samples were left to stand for 48 hours, their peel strength was tested.

[0041] 5. In accordance with GB / T2406.2-2009, the sealants for road crack repair prepared in Examples 4-6 and Comparative Examples 1-3 were made into standard-sized specimens and subjected to limiting oxygen index testing. Specific test results are shown in Table 1.

[0042] Table 1. Performance test data of the samples Data Analysis: Comparative analysis of the data in Table 1 shows that the sealants for road crack repair prepared in Examples 4-6 of this invention have moderate viscosity; in Example 6, the mass ratio of component A to component B is 1:3, the -NCO content is high, and the viscosity value of the synthesized sealant is low.

[0043] In Comparative Example 1, component A was replaced with an equal mass of 4-hydroxybenzaldehyde. On the one hand, the sealant prepared in Comparative Example 1 had a lower relative molecular mass and lower mechanical strength; on the other hand, the sealant prepared in Comparative Example 1 lost its flame-retardant component, and its limiting oxygen index value decreased significantly. In Comparative Example 2, the flame-retardant additive was replaced with an equal mass of tetra(2-chloroethyl)ethylidene diphosphate. Both the flame-retardant properties and mechanical properties of the sealant prepared in Comparative Example 2 decreased.

[0044] In Comparative Example 3, when the mass ratio of NCO / OH was 1:1, the number of excess -NCO groups decreased, the crosslinking density decreased, and the mechanical properties of the sealant prepared in Comparative Example 3 were reduced.

[0045] The above description is merely an example and illustration of the structure of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

[0046] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0047] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A sealant for road crack repair, characterized by, Includes component A and component B; Component A is a reaction reduction product of PEPA, tetra(2-chloroethyl) ethylidene diphosphate and 4-hydroxybenzaldehyde; Component B is a reaction product of hydrolyzed silanol and 4,4'-diphenylmethane diisocyanate.

2. The sealant for road crack repair according to claim 1, wherein The preparation method of component A includes the following steps: A1, PEPA, NaH and acetonitrile are mixed, and tetra(2-chloroethyl) ethylidene diphosphate is added. The mixture is heated and stirred at 50-60℃, and then refluxed at 80-85℃ for 6-8 hours. After cooling, the mixture is filtered and the solid is collected. The solid is washed and dried to constant weight, which is the prepared flame retardant additive. A2. Under inert gas protection, 4-hydroxybenzaldehyde solution is added dropwise to sodium hydride to form a reaction system; the reaction system is reacted at 65-75℃ for 40-48h, and the intermediate product is obtained by recrystallization with ethyl acetate; a mixed solvent is added to the intermediate product, and then sodium borohydride is added, and the mixture is stirred at room temperature until the sodium borohydride is completely dissolved, and the component A is prepared by recrystallization with ethanol.

3. The sealant for road crack repair according to claim 2, wherein In step A1, the ratio of PEPA, NaH, acetonitrile and tetra(2-chloroethyl) ethylene diphosphate is 1.8-3.6g:0.3-0.5g:50-60mL:5-10g.

4. The sealant for road crack repair according to claim 2, wherein In step A2, the ratio of sodium hydride to 4-hydroxybenzaldehyde solution is 20-30g:7-14g, and the ratio of intermediate product, mixed solvent and sodium borohydride is 10-20g:60-80mL:25-35g; the ratio of intermediate product to mixed solvent is 10-20g:60-80mL.

5. The sealant for road crack repair according to claim 1, wherein The preparation method of component B includes the following steps: γ-aminopropyltriethoxysilane is mixed with deionized water and hydrolyzed to obtain γ-aminopropyltriethoxysilanol; silanol is mixed with liquid 4,4'-diphenylmethane diisocyanate and reacted to form component B.

6. The sealant for repairing road cracks according to claim 5, characterized in that, The ratio of γ-aminopropyltriethoxysilane to deionized water is 11-22g:2-3mL, and the ratio of silanol to liquid 4,4'-diphenylmethane diisocyanate is 12-24g:25-50g.

7. The sealant for repairing road cracks according to claim 1, characterized in that, The mass ratio of component A to component B is 1:2-3.

Citation Information

Patent Citations

  • Production and construction technologies of road sealant

    CN105199666A

  • Sealing adhesive for crack on road

    CN1376756A