A stepwise thermal-induced hydrogen bond reconstitution temporary plugging agent and a preparation method thereof
By employing a step-by-step thermally induced hydrogen bond reconstruction-chain relaxation cycle enhancement process, the mechanical properties of the hydrogel are improved, enabling it to stably seal irregular pores under high temperature and pressure and completely degrade at reservoir temperature. This solves the problem of existing temporary plugging agents failing to seal under high temperature and pressure, achieving efficient sealing and environmentally friendly degradation.
Patent Information
- Application Number
- CN202611080988.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-24
AI Technical Summary
Existing temporary plugging agents cannot simultaneously meet the requirements of high strength, flexible self-adaptation, and controllable degradation under high temperature and high pressure. In particular, they are not effective in sealing irregular pores and gaps. Furthermore, traditional hydrogel materials are prone to swelling and have low strength under high temperature and high pressure, leading to plugging failure.
A step-by-step thermally induced hydrogen bond reconstruction-chain relaxation cycle enhancement process is adopted. The hydrogel is subjected to multiple heating and drying and low-temperature cooling treatments to increase the number of polymer chain segment rearrangements and hydrogen bonds, thereby enhancing mechanical properties. It can be adapted to the sealing of regular and irregular pores and gaps, is stable and does not fall off under high temperature and high pressure, and completely degrades at reservoir temperature.
It has achieved a temporary plugging agent with high pressure resistance, large deformation, stable embedding, and controllable degradation. It is suitable for sealing irregular pores and fractures, is stable and does not fall off under high temperature and high pressure, and its degradation products are compatible with fracturing fluid, causing no secondary damage to the reservoir, thus meeting the needs of efficient fracturing and stimulation of unconventional oil and gas reservoirs.
Smart Images

Figure CN123152452A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil and gas extraction technology, specifically to a step-by-step thermally induced hydrogen bond reconstruction temporary plugging agent and its preparation method. Background Technology
[0002] The development of unconventional oil and gas reservoirs has become a major development direction. Unconventional oil and gas reservoirs are characterized by low porosity and low permeability, making exploration and development difficult. At present, long horizontal sections combined with segmented multi-cluster volumetric stimulation have become an efficient development model for unconventional reservoirs.
[0003] Temporary plugging and redirection technology involves injecting a plugging agent into the wellbore. This agent travels with the fluid to a permeable perforation and sets, forcing the fluid at the bottom of the well to redistribute and flow into low-permeability fractures. This controls the direction of fracture propagation, causing fractures to extend in new directions, improving the efficiency of multi-cluster stimulation, increasing fracture complexity, and ultimately achieving reservoir stimulation. Currently, commonly used temporary plugging agents in fracturing include plugging balls and plugging knots.
[0004] Unconventional reservoir stimulation involves large amounts of sand addition, resulting in irregularly shaped pores after erosion. Rigid spherical temporary plugging materials can only seal regular circular pores, and they are prone to falling off the perforation site after the construction pressure drops, exhibiting poor setting stability under dynamic scouring. Rope-type temporary plugging materials have good flexibility and are easy to bend and deform, but their high-temperature pressure resistance is limited, failing to achieve effective sealing under high temperature and pressure, leading to low sealing efficiency. Meanwhile, traditional hydrogel temporary plugging agents suffer from problems such as excessive water absorption and swelling, sudden drop in strength, and complex processes for enhancing mechanical properties, making it difficult to meet the requirements for efficient temporary plugging of irregular pores under high temperature and pressure.
[0005] Currently, domestic temporary plugging balls are mainly made of plastic, rubber, nylon, and wax. Plastic, rubber, and nylon balls are difficult to dissolve, and when deformed, they can become stuck in the borehole, blocking the borehole passage and affecting subsequent flowback and oil and gas production. While wax balls can dissolve at certain temperatures, their low compressive strength results in unstable plugging, especially under high formation fracturing pressure, making them unable to withstand pressure and achieve effective temporary plugging and diversion. Therefore, to ensure the effectiveness of temporary plugging and diversion fracturing operations, there is an urgent need for a high-strength borehole plugging ball made of a soluble material.
[0006] For example, Chinese patent application publication number CN113773823A discloses a biodegradable temporary plugging ball suitable for downhole fracturing operations. This temporary plugging ball combines polyglycolic acid and flexible biodegradable resin, supplemented with functional fillers, and has both high mechanical strength and certain flexibility. It also effectively improves heat resistance stability. The resulting temporary plugging ball can still maintain a relatively stable sealing and pressure-bearing function under high temperature conditions, and has good biodegradability.
[0007] For example, Chinese patent CN114395385B discloses a biodegradable polymer composite gel temporary plugging ball that not only has excellent expansion and water-blocking performance, but also excellent degradation performance.
[0008] For example, Chinese patent CN112795373B discloses a soluble plugging agent, a plugging ball, and a preparation method thereof suitable for fracturing at different temperatures. Compared with traditional biodegradable materials, this biodegradable plugging ball improves the material's temperature resistance and mechanical strength by adjusting its molecular structure and adding nanomaterials, overcoming the problems of traditional biodegradable materials not being able to dissolve at low temperatures and having a narrow temperature range. Furthermore, the invention has a simple synthesis process, widely available raw materials, and low cost.
[0009] For example, Chinese patent application CN112280545A discloses a non-metallic biodegradable adaptive temporary plugging ball. This plugging ball consists of a rigid biodegradable core and a flexible biodegradable shell covering the core. The rigid biodegradable core has good compressive strength, while the biodegradable shell covering the core has good flexibility. Under pressure, it can undergo a certain degree of adaptive elastic deformation relative to the perforation hole (especially irregularly shaped perforations), producing a deformation that adapts to the shape of the perforation hole, thus forming a good seal. This allows for rapid and effective plugging in the early stages of pressurization, improving the success rate of plugging and reducing the loss of fracturing fluid.
[0010] It can be seen that the materials with dissolving properties are mainly composite resin materials. However, these materials generally have poor mechanical properties, especially when used to prepare temporary plugging balls. Their pressure-bearing capacity is limited, and they are easily deformed and passed through under high pressure, thus failing to achieve effective sealing.
[0011] Existing technologies primarily focus on material compounding and temperature-resistant modification, failing to employ a step-by-step thermally induced hydrogen bond reconstruction mechanism to achieve directional mechanical enhancement. This makes it difficult to simultaneously meet the engineering requirements of high strength under pressure, flexible self-adaptation, and controllable degradation. In summary, existing technologies still lack a temporary plugging technology that integrates mechanical reinforcement, adaptability to irregular pores, high-temperature stability, and environmental degradation.
[0012] In view of this, improvements should be made to the existing technology. Summary of the Invention
[0013] To address existing technical problems, this invention proposes a step-by-step thermally induced hydrogen bond reconstruction temporary plugging agent and its preparation method. Employing a step-by-step thermally induced hydrogen bond reconstruction-chain relaxation cycle enhancement process, the mechanical properties are significantly enhanced through polymer chain segment rearrangement, increased hydrogen bond quantity, and network densification. This results in a temporary plugging agent possessing characteristics such as high pressure resistance, large deformation, stable embedding, and controllable degradation. It can be adapted for sealing both regular and irregular pores and fractures, maintains stable setting under high temperature and pressure without detachment, and its degradation products are compatible with the fracturing fluid system, causing no secondary damage to the reservoir. This meets the requirements for efficient fracturing stimulation of unconventional oil and gas reservoirs.
[0014] According to one aspect of the present invention, a method for preparing a temporary plugging agent with stepwise thermally induced hydrogen bond reconstruction is provided, which includes cyclic treatment of a hydrogel by alternating multiple heating and drying to deswell and low-temperature cooling chain relaxation to obtain the temporary plugging agent.
[0015] According to one embodiment of the present invention, the number of cycles is 3.
[0016] According to one embodiment of the present invention, the temperatures for the three heating and drying processes to remove swelling are increased sequentially, with temperature ranges of 25~35℃, 35~45℃, and 45~55℃, respectively.
[0017] According to one embodiment of the present invention, the temperature range for relaxation of the three-stage cryogenic cooling chain is 0~25°C.
[0018] According to one embodiment of the present invention, the heat preservation time after heating and drying to remove swelling is 2 to 12 hours.
[0019] According to one embodiment of the present invention, the reaction time after the low-temperature cooling chain relaxation is 2-4 hours.
[0020] According to another aspect of the present invention, a stepwise thermally induced hydrogen bond remodeling temporary plugging agent is proposed, which is prepared by any of the above technical solutions.
[0021] According to one embodiment of the present invention, the pressure resistance of the temporary plugging agent is ≥35 MPa.
[0022] Due to the adoption of the above technical solutions, this invention has the following advantages compared with the prior art: It adopts a step-type thermally induced hydrogen bond reconstruction-chain relaxation cycle enhancement process, which significantly enhances mechanical properties through polymer chain segment rearrangement, increase in the number of hydrogen bonds and network densification. This makes the temporary plugging agent have the characteristics of high pressure resistance, large deformation, stable embedding and controllable degradation. It can be adapted to the plugging of regular and irregular pores and fractures, and it is stable and does not fall off under high temperature and high pressure. The degradation products are compatible with the fracturing fluid system and do not cause secondary damage to the reservoir, thus meeting the needs of efficient fracturing and stimulation of unconventional oil and gas reservoirs. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some implementation examples of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 A cyclic mechanism diagram of a method for preparing a stepwise thermally induced hydrogen bond remodeling temporary plugging agent according to an embodiment of the present invention is shown; Figure 2 The diagram shows a comparison of the microstructures during the preparation process of a step-by-step thermally induced hydrogen bond remodeling temporary plugging agent according to an embodiment of the present invention. Detailed Implementation
[0025] The following detailed description of the embodiments is intended to exemplify the principles of the present invention, but should not be construed as limiting the scope of the invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0026] These embodiments are provided to make this disclosure thorough and complete, and to fully express the scope of the invention to those skilled in the art. It should be noted that, unless otherwise specifically stated, the relative arrangement of components and steps, material composition, numerical expressions, and values set forth in these embodiments should be interpreted as merely exemplary and not as limiting.
[0027] It should be noted that, in the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0028] All terms used in this invention have the same meaning as understood by one of ordinary skill in the art to which this disclosure pertains, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries should be interpreted as having meanings consistent with their meanings in the context of the relevant art, and not as idealized or highly formalized, unless expressly defined herein.
[0029] Techniques, methods, and equipment known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and equipment should be considered part of the specification.
[0030] The existing technology has the following core problems: (1) Rigid circular temporary plugging balls are poorly adaptable to irregular holes and gaps, are easy to fall off due to dynamic scouring, and have insufficient sealing stability; (2) Conventional hydrogel temporary plugging agents absorb too much water and swell, have low mechanical strength and poor performance uniformity, and have limited pressure bearing capacity under high temperature and high pressure conditions, resulting in sealing failure; (3) Traditional hydrogel reinforcement process is complicated, costly, and has limited reinforcement effect.
[0031] This invention provides a method for preparing a temporary plugging agent with stepwise thermally induced hydrogen bond reconstruction, which includes cyclic treatment of hydrogel with alternating heating and drying to deswell and low-temperature cooling to relax, in order to obtain the desired temporary plugging agent.
[0032] In the preparation method of the temporary plugging agent based on the step-type thermally induced hydrogen bond reconstruction according to this application, a step-type thermally induced hydrogen bond reconstruction-chain relaxation cycle enhancement process is adopted. Through polymer chain segment rearrangement, increase in the number of hydrogen bonds and network densification, the mechanical properties are significantly enhanced, giving the temporary plugging agent the characteristics of high pressure resistance, large deformation, stable embedding and controllable degradation. It can be adapted to the plugging of regular and irregular pores and fractures, and it is stable and does not fall off under high temperature and high pressure. The degradation products are compatible with the fracturing fluid system and do not cause secondary damage to the reservoir, thus meeting the needs of efficient fracturing stimulation of unconventional oil and gas reservoirs.
[0033] Figure 1 A step-like thermally induced hydrogen bond reconstruction-chain relaxation cycle mechanism diagram is shown, which represents the changes in hydrogen bonds and interchain spacing from the initial state to the deswelling state and the chain relaxation state. Figure 2 A comparison of the microstructure of the flexible adaptive temporary plugging agent before and after hydrogen bond remodeling heat treatment is shown. (Reference) Figure 1 and Figure 2 This invention drives the gel to deswell and densify through heating, reducing the inter-chain spacing and significantly increasing the number of intermolecular hydrogen bonds. The cooling stage provides sufficient relaxation time for the chain segments, achieving uniform arrangement and structural homogenization. Through hydrogen bond reconstruction and physical cross-linking optimization, the mechanical properties are greatly enhanced, improving pressure resistance, structural stability and temperature resistance. It can effectively seal perforations of different diameters and is a temporary plugging agent that can continue to seal even when the bottom hole pressure decreases, thereby improving the perforation cluster opening rate.
[0034] In some specific embodiments, the cyclic treatment is performed three times. The first cycle initially establishes the shrinkage orientation memory and removes a large amount of free water; the second cycle repairs and strengthens the network, further consolidating the chain segment orientation; the third cycle thoroughly consolidates the anisotropic structure, making the polymer chain orientation more uniform and fully releasing internal stress. The three-cycle treatment enables hydrogen bond reconstruction and mechanical enhancement. By controlling the step-by-step heating range, holding time, and cooling relaxation time, the inter-chain spacing and the number of hydrogen bonds can be adjusted to achieve on-demand enhancement of mechanical strength.
[0035] Three cycles can significantly shorten the preparation cycle, reduce energy consumption, and ensure high performance stability and reproducibility between batches.
[0036] In some specific embodiments, the temperatures for the three heating and drying processes to remove swelling are increased sequentially, with temperature ranges of 25~35℃, 35~45℃, and 45~55℃, respectively.
[0037] The initial low-temperature treatment removes only the weakly bound water on the surface and induces the initial orientation of shallow chain segments, constructing an initial shrinkage skeleton. This effectively avoids internal stress concentration and macroscopic cracks caused by direct impact from high temperatures. The intermediate temperature drives the synergistic shrinkage of the deep network and consolidates the cross-linking density, ensuring uniform densification of the structure from the surface inwards. Finally, a higher temperature promotes the complete removal of residual crystalline regions and strongly bound water, completing the final shaping of the high-strength, dense structure. The step-by-step heating significantly reduces the thermal damage and irreversible entanglement of the polymer chains caused by a single high-temperature treatment. It also ensures a high degree of matching between the chain segment relaxation rate and the deswelling process, fully releasing internal stress and balancing the excellent compressive strength and flexibility of the temporary plugging agent, while guaranteeing process controllability and high batch-to-batch reproducibility.
[0038] Based on the above embodiments, the temperature range of the three low-temperature cooling chain relaxation stages is 0~25℃.
[0039] In some specific embodiments, the holding time after heating and drying to remove swelling is 2-12 hours, providing a sufficient and controllable time window for the rearrangement of polymer chain segments and the homogenization of the structure. If the holding time is too short, the temperature field and moisture concentration field inside the gel have not yet reached equilibrium, which easily leads to the formation of a sandwich structure where the surface is over-shrunken while the core is not, resulting in stress concentration and uneven performance. On the other hand, if the holding time is too long, it will cause irreversible chain entanglement and mechanical embrittlement caused by excessive shrinkage, while significantly increasing the energy consumption of preparation, which deviates from the economic principle of industrial production.
[0040] Based on the above embodiments, the reaction time after the low-temperature cooling chain relaxation is 2~12 hours. If the relaxation time is insufficient, the contracted polymer chains have not yet obtained enough kinetic energy and hydration opportunities to rearrange and expand, and a large amount of freezing stress remains inside the network. During the subsequent heating and deswelling process, it is very easy to cause sudden breakage of stress concentration points and microcrack propagation, which seriously weakens the cycle life and structural integrity of the temporary plugging agent. On the other hand, if the relaxation time is too long, the chain segment hydration and rearrangement will tend to saturate and equilibrium. Continuing to extend the time will not further improve the performance, but will increase production energy consumption and cycle costs.
[0041] In some specific embodiments, the method of drying by heating to remove swelling includes a hot water bath.
[0042] This invention also proposes a stepwise thermally induced hydrogen bond reconstruction temporary plugging agent, which is prepared by any of the methods mentioned in the above technical solutions.
[0043] Based on the above embodiments, the pressure resistance of the temporary plugging agent is ≥35 MPa.
[0044] The temporary plugging agent of the present invention exhibits enhanced mechanical strength through hydrogen bond reconstruction. In some embodiments, after step-heat induction treatment, it has a compressive strength ≥40MPa and is stable at high temperatures of 70~140℃ for 1~2h. It loses its mechanical strength at reservoir temperature for 2~6h and completely degrades in 24~120h, leaving no residue and causing no secondary damage. The thermal cycling process is simple, has a short cycle, and can be mass-produced.
[0045] This invention utilizes a stepped heating and cooling cycle to drive gel deswelling, densification, and chain rearrangement, significantly increasing the number of intermolecular hydrogen bonds and optimizing the physical cross-linking network, thereby achieving a substantial enhancement of mechanical strength. Temperature and time can be controlled to achieve on-demand enhancement of mechanical strength; under formation conditions, it initially loses strength and then completely degrades, with the product being compatible and harmless. It is suitable for temporary plugging and redirection in long horizontal sections of conventional and unconventional oil and gas reservoirs at 70-140℃, capable of sealing regular / irregular perforations and fractures formed after fracturing and sand erosion. It is compatible with various water-based fracturing fluid systems, overcoming the technical bottleneck of traditional plugging agents in synergistically addressing pressure resistance, flexibility, and degradation. With hydrogen bond reconstruction and adaptive flexibility as its core advantages, it significantly improves perforation cluster opening rate, temporary plugging efficiency, and construction safety, reducing operation time and reservoir damage risk. It can be widely applied to the efficient development of unconventional oil and gas such as shale oil, shale gas, and tight sandstone gas, possessing good field promotion value and industrial application prospects, and is of great significance for improving the production enhancement and transformation effects of oil and gas fields.
[0046] Through stepwise thermally induced hydrogen bond reconstruction and chain relaxation, the mechanical strength and compressive strength of the hydrogel are significantly improved. In some embodiments, the compressive strength is ≥35MPa, and it does not soften or break within 1 hour at high temperature. It is suitable for regular / irregular pores and gaps, and is stable when embedded and sealed, and resistant to dynamic erosion. It loses strength in 4~8h at reservoir temperature and completely degrades in 48~120h. It is environmentally friendly with no residue and no secondary damage to the reservoir. The process is simple, with stepwise thermal cycling replacing traditional freeze-thaw cycles. It is easy to operate, has a short cycle, and can be mass-produced.
[0047] The present invention will be described below through specific embodiments.
[0048] Example 1 The hydrogel was dried at 25°C for 7 hours to remove swelling, then cooled at 15°C for 3 hours to relax; dried at 35°C for 7 hours to remove swelling, then cooled at 15°C for 3 hours to relax; and dried at 45°C for 7 hours to remove swelling, then cooled at 15°C for 3 hours to relax. This process was repeated three times to obtain a temporary plugging agent.
[0049] Example 2 The hydrogel was dried at 30℃ for 2 hours to remove swelling, then cooled at 0℃ for 6 hours to relax; dried at 40℃ for 2 hours to remove swelling, then cooled at 0℃ for 6 hours to relax; and dried at 50℃ for 2 hours to remove swelling, then cooled at 0℃ for 6 hours to relax. This process was repeated three times to obtain a temporary plugging agent.
[0050] Example 3 The hydrogel was dried at 35℃ for 12 hours to remove swelling, then cooled at 10℃ for 8 hours to relax; dried at 40℃ for 12 hours to remove swelling, then cooled at 10℃ for 8 hours to relax; and dried at 50℃ for 12 hours to remove swelling, then cooled at 10℃ for 8 hours to relax. This process was repeated three times to obtain a temporary plugging agent.
[0051] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of different aspects of the invention exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method for preparing a staged thermal induced hydrogen bond reconstitution temporary plugging agent, characterized in that, The hydrogel is subjected to multiple cycles of treatment, each cycle including a sequential heating-drying deswelling stage and a cooling chain relaxation stage; wherein the temperature of the heating-drying deswelling stage in the multiple cycles of treatment is increased sequentially.
2. The method of claim 1, wherein the step of preparing the step- wise thermal induced hydrogen bond reconfiguration temporary plugging agent is characterized by, The temperature of the heating and drying deswelling stage in the multiple cycles of treatment is in the range of 25~60℃, and the temperature difference between two adjacent heating and drying deswelling stages is 5~15℃.
3. The method of claim 2, wherein the step of mixing is performed at a temperature of 20- 30 °C. The number of cycles is 3 to 5.
4. The method of claim 3, wherein the step of mixing is performed at a temperature of 20- 30 °C. The temperature ranges for the heating and drying deswelling stages described in steps 3 to 5 include 25~35℃, 35~45℃, and 45~60℃.
5. The method of claim 1, wherein the step of preparing the step- wise thermal induced hydrogen bond reconfiguration temporary plugging agent is characterized by, The temperature during the relaxation phase of the cooling chain in the multiple-cycle treatment is 0~25℃.
6. The method of claim 1, wherein the step of preparing the step- wise thermal induced hydrogen bond reconfiguration temporary plugging agent is characterized by, The duration of the heating and drying deswelling stage is 2-12 hours.
7. The method of claim 1, wherein the step of mixing is performed at a temperature of 20- 30 °C. The duration of the cooling chain relaxation phase is 2 to 12 hours.
8. The method for preparing the stepwise thermally induced hydrogen bond remodeling temporary plugging agent according to claim 1, characterized in that, The method of heating and drying to remove swelling includes a hot water bath.
9. A temporary plugging agent for stepwise thermally induced hydrogen bond reconstruction, characterized in that, It is prepared by the method described in any one of claims 1-8.
10. The temporary plugging agent for step-by-step thermally induced hydrogen bond remodeling according to claim 9, characterized in that, The pressure resistance of the temporary plugging agent is ≥35MPa.
Citation Information
Patent Citations
Non-metal degradable self-adaptive temporary plugging ball
CN112280545A
Soluble plugging agents and plugging balls suitable for fracturing at different temperatures and their preparation methods
CN112795373B
Degradable temporary plugging ball suitable for underground fracturing operation and preparation method thereof
CN113773823A
A biodegradable polymer composite gel temporary plugging ball
CN114395385B