A type of Cr 3+ Activated oxyfluoride near-infrared phosphors, their preparation methods and applications

CN123152467APending Publication Date: 2026-11-24INST OF RESOURCES UTILIZATION & RARE EARTH DEV GUANGDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611122987.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

尽管学界已对过渡金属离子(Cr3+、Cr4+、Fe3+、Ni2+、Mn4+)与稀土离子(Pr3+、Nd3+、Eu2+、Tm3+、Yb3+)掺杂的无机荧光材料进行了系统性探索,但多数体系仍存在本质缺陷:稀土离子因4f-4f跃迁的本征锐线发射特性,与宽谱检测需求相悖;Eu2+掺杂体系虽可实现近红外发射,但受晶体场强度与电子云效应制约,难以将发射波长有效调控至>900 nm的近红外二区;Cr4+、Fe3+、Ni2+等体系则普遍面临光致发光量子效率(PLQY)偏低或激发光谱与蓝光芯片失配的问题

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152467A_ABST
    Figure CN123152467A_ABST
Patent Text Reader

Abstract

This invention discloses a Cr 3+ The activated oxyfluoride near-infrared phosphor material has the following chemical composition: Mg4Ge 0.5‑ x Si 0.5 F2O5:xCr 3+ Where x is the amount of Cr substitution, and 0 < x < 0.5. The near-infrared phosphor material has excitation peaks between 360-500 nm and 575-690 nm, with the strongest emission peak at 721 nm. It can be used as a near-infrared light conversion material for near-ultraviolet and blue LED chips, in phosphor-converted light-emitting diode devices, for plant growth lighting, and also in solvent identification, where the solvent is anhydrous ethanol and deionized water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of inorganic luminescent materials technology, specifically to a Cr... 3+ Activated oxyfluoride near-infrared phosphors, their preparation methods, and applications. Background Technology

[0002] Near-infrared (NIR) light sources, with their unique penetrability, low bio-damage, and spectral fingerprinting characteristics, have demonstrated irreplaceable application value in fields such as night vision imaging, plant light regulation, biosensing, non-destructive testing, and in-situ component analysis, becoming a research hotspot in optoelectronic technology. Based on the principles of vibrational spectroscopy, the fundamental frequency vibrational absorption characteristics of hydrogen-containing functional groups such as CH, OH, and NH in the 700-1100 nm near-infrared region of molecules provide a theoretical basis for substance identification and component analysis. Crucially, this band serves as the primary window for bio-optical imaging; due to the low absorption characteristics of biomolecules such as water and hemoglobin, it enables optical detection of deep tissues and non-invasive sensing of metabolites such as blood glucose. Therefore, developing near-infrared light sources that combine broadband emission characteristics with high luminous efficiency is essential for overcoming the physical limits of traditional detection technologies. However, existing technologies have inherent limitations: traditional tungsten halogen lamps and supercontinuum lasers, while offering broad spectral coverage, are bulky, inefficient, and require complex thermal management, severely restricting system integration; near-infrared light-emitting diodes (LEDs), though compact, suffer from narrow-band emission characteristics with a typical full width at half maximum (FWHM) of <50 nm, making them unsuitable for multi-component detection and broadband imaging applications. Therefore, developing near-infrared light source technology that combines efficient excitation and broadband emission has become a critical bottleneck that urgently needs to be overcome in this field.

[0003] Phosphor-converting light-emitting diodes (Pc-LEDs) are considered an ideal path to achieving high-performance near-infrared light sources due to their tunable fluorescence spectra and process compatibility. As the core component of Pc-LEDs, the spectral characteristics of the near-infrared emitting phosphor directly determine the overall performance of the device. Therefore, developing phosphors that can be efficiently excited by blue LED chips and possess broadband near-infrared emission characteristics has significant scientific and application value. Although the academic community has already studied transition metal ions (Cr... 3+ Cr 4 + Fe 3+ Ni 2+ Mn 4+ ) and rare earth ions (Pr 3+ 、Nd 3+ Eu 2+ Tm 3+ Yb 3+Systematic exploration has been conducted on doped inorganic fluorescent materials, but most systems still suffer from fundamental defects: the intrinsic sharp-line emission characteristics of rare-earth ions due to the 4f-4f transition contradict the requirements for broad-spectrum detection; Eu 2+ Although doped systems can achieve near-infrared emission, the emission wavelength is difficult to effectively tune to the near-infrared II region >900 nm due to limitations imposed by crystal field strength and electron cloud effects; Cr 4+ Fe 3+ Ni 2+ Systems like these generally face problems such as low photoluminescence quantum efficiency (PLQY) or mismatch between the excitation spectrum and the blue light chip. In contrast, Cr... 3+ Ions exhibit unique advantages: their broadband absorption generated by dd transitions perfectly matches the emission spectrum of blue LED chips, and in a weak octahedral crystal field, spin-allowed... 4 T2→ 4 The A2 transition can generate broadband near-infrared emission covering 650-1200 nm. Further, through crystal field engineering and lattice site manipulation strategies, emission wavelength tuning from the NIR-I to NIR-II bands can be achieved. Therefore, Cr 3+ Doped broadband near-infrared phosphors combine efficient excitation-emission matching with spectral tunability, making them ideal candidate materials for overcoming the bottlenecks of existing near-infrared light source technologies. Summary of the Invention

[0004] The purpose of this invention is to provide a Cr 3+ The activated oxyfluoride near-infrared phosphor, its preparation method, and its application have solved the problem.

[0005] This invention is achieved through the following technical solutions:

[0006] A type of Cr 3+ The activated oxyfluoride near-infrared phosphor material is characterized by having the chemical composition formula: Mg4Ge 0.5-x Si 0.5 F2O5:xCr 3+ , where x is the amount of Cr substitution, and 0 < x < 0.5, preferably 0.001 ≤ x ≤ 0.07.

[0007] The Cr 3+ The preparation method of activated oxyfluoride near-infrared phosphor material includes the following steps: weighing raw materials containing magnesium, germanium, silicon, fluorine and chromium according to their chemical composition, wherein the stoichiometric ratio of magnesium, germanium, silicon, fluorine and chromium is 4:0.5-x:0.5:2:x, where x is the amount of Cr substitution, and 0 < x < 0.5, grinding and mixing thoroughly, placing in a reaction vessel, sintering at 1050-1150℃ in an air atmosphere, cooling to room temperature, and grinding to obtain the target phosphor.

[0008] Preferably, the sintering step is as follows: heating to 1100°C at a rate of 3-5°C / min in air atmosphere, holding at the temperature for 6 hours, cooling to room temperature, and grinding to obtain the target phosphor.

[0009] Preferably, the magnesium-containing raw material is selected from one or more of magnesium oxide, magnesium fluoride, and magnesium carbonate.

[0010] Preferably, the germanium-containing raw material is germanium dioxide.

[0011] Preferably, the silicon-containing raw material is selected from silicon dioxide.

[0012] Preferably, the fluorine-containing raw material is selected from magnesium fluoride.

[0013] Preferably, the chromium-containing raw material is selected from chromium oxide.

[0014] This invention Cr 3+ The activated oxyfluoride near-infrared phosphor material has high purity and exhibits excitation peaks between 360-500 nm and 575-690 nm, with the strongest emission peak at 721 nm. Therefore, this invention also protects the Cr... 3+ The application of activated oxyfluoride near-infrared phosphor materials as near-infrared light conversion materials excited by near-ultraviolet and blue LED chips. It is used in phosphor-converted light-emitting diode devices for plant growth lighting.

[0015] This invention also protects the Cr 3+ The application of activated oxyfluoride near-infrared phosphor materials in solvent identification, specifically, the solvents being anhydrous ethanol and deionized water. When the phosphor of this invention is mixed with anhydrous ethanol and deionized water respectively, its luminescence intensity exhibits different changes under 449 nm excitation. When the phosphor is mixed with anhydrous ethanol, its luminescence intensity is significantly enhanced under 449 nm excitation. When the phosphor is mixed with deionized water, its luminescence intensity is significantly weakened under 449 nm excitation. Therefore, it can be used in the identification of solvents anhydrous ethanol and deionized water. Specifically, the mass-to-volume ratio of the phosphor to anhydrous ethanol or water is 0.5-1.5 g / ml.

[0016] Compared with the prior art, the beneficial effects of the present invention are:

[0017] (1) The present invention Cr 3+ Activated oxyfluoride near-infrared phosphor materials can be sintered in a single step at temperatures as low as 1050-1150℃, requiring only 6 hours to form a phase. They have the advantages of readily available raw materials, simple manufacturing process, short synthesis time, low energy consumption, and ease of industrialization.

[0018] (2) The present invention Cr3+ The activated oxyfluoride near-infrared phosphor material has high purity and has excitation peaks between 360-500 nm and 575-690 nm, with the strongest emission peak at 721 nm. It can be used as a near-infrared light conversion material for near-ultraviolet and blue LED chips, and can be applied in phosphor-converted light-emitting diode devices for plant growth lighting.

[0019] (3) When the phosphor of the present invention is mixed with anhydrous ethanol and deionized water respectively, its luminescence intensity shows different variation patterns, which can be used in the field of solvent (such as anhydrous ethanol and deionized water) identification. Attached Figure Description

[0020] Figure 1 The Cr prepared in Example 1 3+ The X-ray powder diffraction pattern of the activated oxyfluoride near-infrared phosphor material shows that the obtained sample is a pure phase.

[0021] Figure 2 The Cr prepared in Example 2 3+ The excitation spectrum of the activated oxyfluoride near-infrared phosphor material, as shown in the figure, indicates that the obtained sample has excitation peaks between 360-500 nm and 575-690 nm.

[0022] Figure 3 The Cr prepared in Example 3 3+ The emission spectra of the activated oxyfluoride near-infrared phosphor material and the mixture of 0.5 g phosphor prepared in Example 3 and 0.5 ml anhydrous ethanol are shown in the figure. As can be seen from the figure, the strongest emission peak of both is located at 721 nm, and their peak shape and position are basically the same. It is worth noting that after the phosphor prepared in Example 3 is mixed with anhydrous ethanol, its luminescence intensity is significantly enhanced compared with the original phosphor, reaching 150% of the original intensity.

[0023] Figure 4 The Cr prepared in Example 3 3+ The emission spectra of the activated oxyfluoride near-infrared phosphor material and the mixture of 0.5 g of phosphor prepared in Example 3 and 0.5 ml of deionized water are shown in the figure. As can be seen from the figure, the strongest emission peak of both is located at 721 nm, and their peak shape and position are basically the same. It is worth noting that after the phosphor prepared in Example 3 is mixed with deionized water, the enhancement of its luminescence intensity is significantly weakened compared with the original phosphor, and it is reduced to 70% of the original intensity. Detailed Implementation

[0024] The following is a further description of the invention, but not a limitation thereof.

[0025] Example 1:

[0026] Weigh out 1.2091 g of magnesium oxide (MgO), 0.6230 g of magnesium fluoride (MgF2), 0.5221 g of germanium dioxide (GeO2), 0.3004 g of silicon dioxide (SiO2), and 0.0008 g of chromium trioxide (Cr2O3). Grind the above raw materials evenly in an agate mortar, place the mixture in a corundum crucible, and heat it from room temperature to 1050 ℃ in air at a heating rate of 3 ℃ / min. After reaching the preset temperature, maintain the temperature for 6 h. After the process is complete, allow it to cool naturally and grind it evenly to obtain Mg4Ge 0.499 Si 0.5 F2O5:0.001Cr 3+ Near-infrared phosphor, its XRD pattern is shown in [reference needed]. Figure 1 .

[0027] Example 2:

[0028] Weigh out 1.2091 g of magnesium oxide (MgO), 0.6230 g of magnesium fluoride (MgF2), 0.4918 g of germanium dioxide (GeO2), 0.3004 g of silicon dioxide (SiO2), and 0.0228 g of chromium trioxide (Cr2O3). Grind the above raw materials evenly in an agate mortar, place the mixture in a corundum crucible, and heat it from room temperature to 1100 ℃ in air at a rate of 3 ℃ / min. After reaching the preset temperature, maintain the temperature for 6 h. After the process is complete, allow it to cool naturally and grind it evenly to obtain Mg4Ge 0.47 Si 0.5 F2O5:0.03Cr 3+ Near-infrared phosphor, its excitation spectrum is shown in [reference]. Figure 2 .

[0029] Example 3:

[0030] Weigh out 1.2091 g of magnesium oxide (MgO), 0.6230 g of magnesium fluoride (MgF2), 0.4499 g of germanium dioxide (GeO2), 0.3004 g of silicon dioxide (SiO2), and 0.0532 g of chromium trioxide (Cr2O3). Grind the above raw materials evenly in an agate mortar, place the mixture in a corundum crucible, and heat it from room temperature to 1150 ℃ in air at a heating rate of 3 ℃ / min. After reaching the preset temperature, maintain the temperature for 6 h. After the process is complete, allow it to cool naturally and grind it evenly to obtain Mg4Ge 0.43 Si 0.5 F2O5:0.07Cr 3+ Near-infrared phosphor, its emission spectrum is shown in [reference]. Figure 3 .

[0031] Application example:

[0032] (1) 0.5 g of the phosphor prepared in Example 3 was mixed with 0.5 ml of anhydrous ethanol. Under excitation at 449 nm, its luminescence intensity was significantly enhanced, reaching 1.5 times that of the original phosphor. See [link to relevant documentation]. Figure 3 .

[0033] (2) 0.5 g of the phosphor prepared in Example 3 was mixed with 0.5 ml of deionized water. Under excitation at 449 nm, its luminescence intensity was significantly reduced to 70% of the original phosphor. See [reference needed]. Figure 4 .

[0034] It can be seen that when the phosphor of the present invention is mixed with anhydrous ethanol and deionized water respectively, its luminescence intensity exhibits different change patterns, and therefore can be used to identify anhydrous ethanol and deionized water.

Claims

1. A type of Cr 3+ Activated oxyfluoride near-infrared phosphor material, characterized in that, The chemical composition is represented by the formula: Mg4Ge 0.5-x Si 0.5 F2O5:xCr 3+ wherein x is the substitution amount of Cr, and 0 < x < 0.

5.

2. The near-infrared phosphor material according to claim 1, characterized in that, 0.001≤x≤0.07。 3. The method for preparing the near-infrared phosphor material according to claim 1, characterized in that, Includes the following steps: Weigh out the raw materials containing magnesium, germanium, silicon, fluorine and chromium according to their chemical composition, wherein the stoichiometric ratio of magnesium, germanium, silicon, fluorine and chromium is 4:0.5-x:0.5:2:x, where x is the amount of Cr substitution, and 0 < x < 0.

5. Grind and mix thoroughly, place in a reaction vessel, sinter at 1050-1150℃ in air atmosphere, cool to room temperature, and grind to obtain the target phosphor.

4. The preparation method according to claim 3, characterized in that, The sintering step is as follows: the temperature is raised to 1100℃ at a rate of 3-5℃ / min in air atmosphere, kept at the temperature for 6 hours, cooled to room temperature, and then ground to obtain the target phosphor.

5. The preparation method according to claim 3, characterized in that, The raw materials containing magnesium are selected from one or more of magnesium oxide, magnesium fluoride, and magnesium carbonate; the raw materials containing germanium are selected from germanium dioxide.

6. The preparation method according to claim 3, characterized in that, The raw material containing silicon is selected from silicon dioxide; the raw material containing fluorine is selected from magnesium fluoride.

7. The preparation method according to claim 3, characterized in that, The chromium-containing raw material is selected from chromium oxide.

8. The application of the near-infrared phosphor material according to claim 1 as a near-infrared light conversion material excited by near-ultraviolet and blue LED chips.

9. The application according to claim 8, characterized in that, It is used in phosphor-converted light-emitting diode devices for plant growth lighting.

10. The application of the near-infrared phosphor material according to claim 1 in the field of solvent identification, characterized in that, The solvent is anhydrous ethanol and deionized water.