Fluorine-free complex fluxing and slag system regulating method for LF refining furnace
By optimizing the composition of LF refining slag and using composite modifiers, combined with a segmented heating and stirring process, the problems of high melting point and fluorine contamination in LF refining slag were solved, achieving low-cost, high-efficiency slag melting point reduction and improved steel purity.
Patent Information
- Application Number
- CN202611203788.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-24
AI Technical Summary
The slag in the existing LF refining furnace has a high melting point, slow slag formation, and serious fluorine pollution, resulting in excessive inclusions and unstable performance in the steel. In addition, the traditional fluorine-free process has poor compatibility and limited melting point reduction effect.
By employing a fluorine-free composite fluxing and slag system control method, and optimizing the quaternary slag system ratio of CaO-Al₂O₃-SiO₂-MgO, a composite modifier of nano-alumina powder, borates, and titanates is used, combined with a segmented heating and intermittent stirring process, low-temperature rapid melting of slag is achieved.
It lowers the slag melting point by 60℃~90℃, shortens the slag formation time by more than 30%, reduces fluorine pollution, extends the service life of the ladle, improves the purity of molten steel and production stability, and reduces production costs.
Smart Images

Figure CN123152829A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of secondary refining metallurgical technology of iron and steel, and in particular relates to a fluorine-free composite fluxing and slag system control method for LF refining furnace. Background Technology
[0002] The LF refining furnace is a core secondary refining equipment in steelmaking, capable of desulfurization, removal of non-metallic inclusions, fine-tuning of steel composition and temperature, and homogenization of steel composition. It is widely used in the production of various high-quality steel products. As the core medium in the LF refining process, the melting point, fluidity, and phase structure of the slag directly determine the refining efficiency and the purity of the molten steel.
[0003] Currently, the LF refining furnace in steelmaking generally adopts the CaO-Al2O3-SiO2 ternary basic slag system. This slag system has good chemical stability and strong desulfurization ability, but it has the defect of a high melting point, with a conventional melting temperature of 1580℃~1620℃. In the early stage of refining, the slag formation rate is slow, and it remains in a semi-molten solid state for a long time. The slag has poor fluidity and cannot quickly cover the surface of the molten steel. This not only leads to a large temperature drop in the molten steel and a longer refining cycle, but also seriously restricts the slag's ability to adsorb oxides and sulfide inclusions in the molten steel, which can easily cause quality problems such as excessive inclusions and unstable performance in the steel.
[0004] To address the issue of high slag melting point, traditional industrial processes commonly employ the addition of fluorite (CaF2) to lower it. While fluorite effectively disrupts the silicate network structure of slag and reduces the slag melting temperature, it presents several drawbacks: First, the high-temperature decomposition of fluorite generates fluoride gases, causing air pollution and failing to meet the environmental protection requirements of green metallurgy. Second, fluoride ions severely corrode the magnesia-carbon bricks lining of the ladle, significantly reducing its service life and increasing production and maintenance costs. Third, excessive fluorite can lead to excessively low slag viscosity, resulting in slag entrapment and secondary oxidation of molten steel, ultimately reducing the purity of the molten steel.
[0005] Existing technologies for reducing the melting point of LF refining furnace slag suffer from poor adaptability, limited melting point reduction effect, and uneven slag formation. These technologies can only achieve a small reduction in melting point, failing to meet the demands of high-efficiency refining production. Furthermore, most of these methods rely on single-component control and do not combine slag microstructure modification with synergistic optimization of the smelting process, resulting in poor overall metallurgical performance. Therefore, developing a fluorine-free, efficient, low-cost, and widely adaptable method for reducing the melting point of LF refining furnace slag is a current research focus for those skilled in the art. Summary of the Invention
[0006] To address the above-mentioned technical deficiencies, this invention provides a method for fluorine-free composite fluxing and slag system control in LF refining furnaces, solving the technical problems of high melting point, slow slag formation, fluorine pollution, and severe furnace lining erosion in traditional processes. By optimizing slag system components, modifying composite fluxing, and coordinating segmented smelting processes, the invention achieves low-temperature rapid melting of slag, improves refining efficiency and steel quality, and simultaneously realizes green fluorine-free production.
[0007] To achieve the above-mentioned technical objectives, the present invention is implemented through the following technical solution: A method for controlling the slag system and fluorine-free composite fluxing agent in an LF refining furnace includes: S1. Initial material preparation and slag ratio control: Based on the type of steel grade refined by LF, prepare fluorine-free low-melting-point refining base slag, and control the mass ratio of CaO to Al2O3 in the base slag to be 1.1 to 1.5, and the mass fraction of SiO2 ≤ 8%; S2. Addition of composite flux modifier: Nano-alumina powder is used to regulate the formation of the eutectic phases of calcium dodecanoate and calcium aluminate in the slag, and forms a multi-component low-melting-point composite phase with borate and titanate, thereby reducing the liquidus temperature of the system from a microstructural perspective. During the initial stage of slag formation in LF refining, a composite flux modifier is added to the ladle. This composite flux modifier is composed of nano-alumina powder, borate, and titanate. S3. Segmented heating and slag treatment: A segmented electric heating process is adopted in combination with bottom blowing argon gas stirring. First, low temperature pretreatment is carried out, and then high temperature melting is carried out to promote the complete melting of slag. S4. Slag System Steady-State Control: After the slag is completely melted, maintain the slag melting point at 1490℃~1530℃.
[0008] Preferably, the basic slag comprises, by mass percentage: 45%~48% CaO, 32%~38% Al2O3, 5%~8% SiO2, 4%~7% MgO, with the balance being unavoidable impurities.
[0009] Preferably, the amount of the composite flux modifier added is 2.0% to 4.5% of the total mass of the base slag.
[0010] Preferably, the mass ratio of the nano-alumina powder, borate, and titanate is 3:2:1.
[0011] Preferably, the nano-alumina powder has a particle size of 200nm~500nm, the borate is anhydrous borax, and the titanate is calcium metatitanate.
[0012] Preferably, the segmented heating and slag treatment includes: The first stage involves an electrical power of 800kW~1000kW, a heating time of 3min~5min, and controlling the temperature of the steel slag system to 1450℃~1470℃. The second stage involves increasing the power supply to 1200kW-1400kW and maintaining a constant temperature for 4-6 minutes.
[0013] Preferably, during the segmented heating and slag treatment process, bottom blowing argon gas is used for stirring throughout the process, and the argon gas flow rate is controlled at 8L / (min·t steel) to 12L / (min·t steel).
[0014] Preferably, the composite flux modifier is added in batches, with 60% to 70% of the total amount added initially, and the remaining amount added after the first stage of heating is completed.
[0015] Preferably, the bottom-blown argon gas is produced in an intermittent stirring mode, with a stirring-to-pause time ratio of (1~2):1.
[0016] Preferably, the preparation of the base slag adopts a premixing and preheating process, in which the raw materials are mixed evenly and then preheated to 300℃~400℃ and kept at that temperature for 1h~3h.
[0017] The advantages and technical effects of this invention are: This invention adopts a fluorine-free formulation system, completely abandoning the traditional fluorite fluxing process, eliminating fluoride pollution and furnace lining fluoride corrosion problems, reducing the furnace lining erosion rate by 15%~20%, extending the service life of the ladle, reducing production costs, and meeting green metallurgical production standards.
[0018] This invention optimizes the quaternary slag system ratio of CaO-Al2O3-SiO2-MgO, precisely controls the calcium-aluminum ratio, and combines it with a special composite fluxing modifier to precisely disrupt the high-temperature dense network structure of the slag, significantly reducing the slag liquidus temperature and stably lowering the slag melting point to 1490℃~1530℃, which is 60℃~90℃ lower than the traditional slag system. The slag formation time is shortened by more than 30%, effectively solving the problems of slow slag formation and large temperature drop of molten steel in the early stage of refining.
[0019] The composite modifier in this invention has multiple functions, including fluxing, grain refinement, and slag property optimization. It not only lowers the melting point of slag, but also optimizes slag viscosity and surface activity, enhances the slag's ability to adsorb alumina and sulfide inclusions, significantly improves the purity of molten steel, and reduces the defect rate of steel.
[0020] This invention employs a synergistic process of segmented heating and intermittent stirring to achieve uniform diffusion of modifiers and synchronous melting of slag. The slag system exhibits uniform and stable properties, with no local overmelting or undermelting. The process demonstrates strong stability and adaptability, making it suitable for refining various steel grades and possessing high value for industrial application. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 A flowchart of a preferred embodiment of the present invention is shown. Detailed Implementation
[0023] To make the above-mentioned objectives, control system design, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0024] A method for controlling the slag system and fluorine-free composite fluxing agent in an LF refining furnace includes: S1. Initial material preparation and slag system ratio control: Based on the LF refining steel grade, a fluorine-free low-melting-point refining base slag is prepared. The base slag composition by mass percentage includes: CaO 45%~52%, Al2O3 32%~38%, SiO2 5%~8%, MgO 4%~7%, with the balance being unavoidable impurities. The CaO / Al2O3 mass ratio is controlled at 1.1~1.5, and the content of high-melting-point SiO2 is limited to optimize the basic melting performance of the slag system from the source.
[0025] S2. Addition of composite flux modifier: In the initial stage of LF refining and slag formation, a composite flux modifier accounting for 2.0% to 4.5% of the total mass of the base slag is added. The modifier is composed of nano alumina powder, anhydrous borax, and calcium metatitanate in a mass ratio of 3:2:1. Through the modification of trace components, the microstructure of the slag is reconstructed.
[0026] S3. Segmented heating and slag treatment: Two-stage electric heating combined with intermittent bottom blowing argon stirring is adopted. The slag is initially melted at low temperature and then smelted at high temperature in a steady state. This ensures that the modifier is evenly dispersed, achieves complete melting of slag and homogenization of phases, and avoids the problems of incomplete slag treatment and uneven slag performance.
[0027] S4. Slag System Steady-State Control: After melting, the melting point and composition of the slag are detected, and the amount of modifier is finely adjusted to maintain the low-temperature steady state of the slag system and ensure the stable operation of subsequent refining processes.
[0028] The basic slag in this invention adopts a pre-grinding, preheating and pretreatment process to refine the raw material particle size, remove impurity gases and improve the melting uniformity of the slag system; the composite modifier is added in batches to effectively avoid high temperature failure and maximize the effect of fluxing modification; the intermittent bottom blowing stirring mode takes into account both the mixing effect and the stability of molten steel quality.
[0029] Example 1: LF refining of plain carbon steel to reduce melting point, the specific steps are as follows: S1. Basic Slag Proportioning and Pretreatment: Prepare the basic slag, which by mass percentage is CaO 48%, Al2O3 35%, SiO2 6.5%, MgO 5.5%, with the remainder being impurities, and the CaO / Al2O3 mass ratio is 1.37; crush and sieve each raw material to 100 mesh, mix them evenly, and then pretreat them by keeping them at 350℃ for 2 hours.
[0030] S2. Modifier addition: After the basic slag is put into the furnace, the composite flux modifier is added at the initial stage of power-on. The amount added is 3.0% of the total mass of the basic slag. The mass ratio of the modifier nano alumina powder, anhydrous borax and calcium metatitanate is 3:2:1. 70% is added initially, and the remaining 30% is added after the first stage of heating.
[0031] S3. Segmented slag melting: The first stage is powered by 900kW, heated for 4 minutes, and the system temperature rises to 1460℃; the second stage is powered by 1300kW, and is heated at a constant temperature for 5 minutes; argon gas is blown from the bottom throughout the process, with a flow rate of 10L / (min·t steel), stirring for 1 minute and stopping and circulating for 30 seconds.
[0032] S4. Steady-state control: After the smelting is completed, the slag melting point is 1510℃, the slag forming time is shortened by 32% compared with the traditional process, the slag has good fluidity, the total oxygen content of the molten steel is reduced by 18%, and the furnace lining erosion rate is significantly reduced.
[0033] Example 2: Low-alloy steel LF refining process to reduce melting point This embodiment is used for verification of the refining process of low alloy steel. Under the process framework of Example 1, the proportion of CaO is appropriately increased according to the basicity requirements of low alloy steel.
[0034] S1. Basic slag ratio and pretreatment: Prepare the basic slag, by mass percentage: CaO: 48%, Al2O3: 36%, SiO2: 5.8%, MgO: 6.2%, with the remainder being impurities. The CaO / Al2O3 mass ratio is 1.39. The raw materials are sieved to 120 mesh and pretreated at 400℃ for 2 hours.
[0035] S2. Modifier addition: The amount of composite flux modifier added is 3.8% of the total mass of the base slag. The modifier is a mixture of nano alumina powder, anhydrous borax, and calcium metatitanate in a mass ratio of 3:2:1. It is added in batches, with 70% added initially and the remaining 30% added after the first stage of heating.
[0036] S3. Segmented slag melting: The first stage is powered by 950 kW, heated for 5 min, and the system temperature is 1470℃; the second stage is powered by 1350 kW, and is heated at a constant temperature for 6 min; the bottom-blown argon flow rate is 11 L / (min·t steel), and the intermittent stirring mode is adopted.
[0037] S4. Steady-state control: The slag melting point was measured to be 1495℃, the slag-forming efficiency was increased by 35%, the total amount of inclusions in the molten steel was reduced by 22%, and the refining cycle was shortened by 8 min.
[0038] Comparative Example 1: Traditional Fluorite Fluxing Process Using conventional CaO-Al2O3-SiO2 base slag, with 3% fluorite added as flux, and conventional electric melting process, the final slag melting point is 1560℃. The slag formation time is long, and there are fluoride waste gas emissions during the refining process. The ladle furnace lining is severely eroded, and the incidence of slag defects in molten steel is high.
[0039] As can be seen from the comparison of the embodiments and comparative examples, the method of the present invention has a lower slag melting point, faster slag formation speed, no fluorine pollution, less furnace lining loss, and significantly improved steel purity and production stability compared with the traditional process. The overall metallurgical effect is far superior to the traditional process.
[0040] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
[0041] Example 3: LF refining process for pipeline steel to reduce melting point S1. Basic Slag Proportioning and Pretreatment: Prepare the basic slag, by mass percentage: CaO 46%, Al2O3 37%, SiO2 7.5%, MgO 6%, with the balance being unavoidable impurities. Control the CaO / Al2O3 mass ratio to be 1.24. Crush and sieve all raw materials to below 100 mesh, mix them evenly, and then premix and preheat at 320℃ for 2.5 hours.
[0042] S2. Modifier Addition: After the base slag is fed into the furnace, a composite flux modifier is added at the initial stage of power-on, with an addition amount of 4.5% of the total mass of the base slag. The modifier is a compound of nano-alumina powder (particle size 300nm), anhydrous borax, and calcium metatitanate in a mass ratio of 3:2:1. It is added in batches, with 65% of the total amount added initially, and the remaining 35% added after the first stage of heating is completed.
[0043] S3. Segmented slag melting: First stage: 850kW power, heating for 5 minutes, system temperature reaches 1455℃; Second stage: power increased to 1250kW, constant temperature melting for 6 minutes. Argon gas is used for bottom blowing throughout the process, with an argon flow rate of 9 L / (min·t steel), using an intermittent stirring mode, and a stirring-to-pause time ratio of 1.5:1 (i.e., 1.5 minutes of stirring followed by 1 minute of pause).
[0044] S4. Slag System Steady-State Control: After smelting, the slag melting point was measured to be 1520℃. Compared with the traditional fluorite fluxing process, the slag formation time was shortened by 35%; the slag had good fluidity and quickly covered the surface of the molten steel; the total oxygen content of the molten steel was reduced by 20%, and the sulfur content was reduced to below 0.003%; the furnace lining erosion rate was reduced by 18% compared with the traditional process, and the service life of the ladle was extended.
[0045] Example 4: LF refining process for silicon steel to reduce melting point S1. Basic Slag Proportioning and Pretreatment: Prepare the basic slag, by mass percentage: CaO 48%, Al2O3 34%, SiO2 5%, MgO 7%, with the balance being unavoidable impurities. Control the CaO / Al2O3 mass ratio to be 1.41. Crush and sieve all raw materials to 120 mesh, mix them evenly, and then premix and preheat at 380℃ for 1.5 hours.
[0046] S2. Modifier addition: The amount of composite flux modifier added is 2.0% of the total mass of the base slag. The modifier ratio is the same as in Example 3 (the particle size of the nano-alumina powder is 200nm). It is added in batches, with 65% of the total amount added initially, and the remaining part added after the first stage of heating is completed.
[0047] S3. Segmented slag melting: First stage: 1000kW power, heating for 3 minutes, system temperature reaches 1470℃; Second stage: power increased to 1400kW, constant temperature melting for 4 minutes. Argon gas is used for bottom blowing stirring throughout the process, with an argon gas flow rate controlled at 12 L / (min·t steel), using intermittent stirring mode.
[0048] S4. Slag System Steady-State Control: After smelting, the slag melting point was measured at 1505℃. Compared with traditional processes, the slag formation time was shortened by 30%; the slag's ability to adsorb Al2O3 inclusions was significantly enhanced, and the rating of Class B inclusions (alumina) in the steel decreased from 2.0 to 0.5; the refining cycle was shortened by 6 minutes, and the power consumption per ton of steel was reduced by approximately 8 kWh; there were no fluoride emissions, resulting in significant environmental benefits.
[0049] Example 5: LF refining process for reducing melting point of heavy rail steel S1. Basic Slag Proportioning and Pretreatment: Prepare the basic slag, which by mass percentage is CaO 48%, Al2O3 33%, SiO2 8%, MgO 4.5%, with the remainder being unavoidable impurities. Control the CaO / Al2O3 mass ratio to be 1.45. The raw materials are crushed and sieved to 100 mesh, mixed evenly, and then premixed and preheated at 300℃ for 3 hours.
[0050] S2. Modifier addition: The amount of composite flux modifier added is 3.5% of the total mass of the base slag. The modifier ratio is the same as in Example 3 (the particle size of the nano-alumina powder is 500nm). A batch addition method is adopted, with 60% of the total addition added initially, and the remaining 40% added after the first stage of heating is completed.
[0051] S3, Segmented slag melting: First stage: Power supply 800kW, heating for 4.5min, system temperature rises to 1450℃; Second stage: Increase the power supply to 1200kW and melt at a constant temperature for 5.5 minutes. Use bottom-blowing argon gas for stirring throughout the process, controlling the argon flow rate at 8L / (min.t steel), and adopt an intermittent stirring mode with a stirring-to-pause time ratio of 2:1.
[0052] S4. Slag System Steady-State Control: After smelting, the slag melting point was found to be 1530℃. The slag formation time was shortened by 31% compared to the traditional fluorite process; the purity of the molten steel was significantly improved, the total oxygen content was reduced by 17%, and the number of large non-metallic inclusions was reduced by 40%; the furnace lining erosion rate was reduced by 15%, and the consumption of refractory materials per ton of steel decreased; the internal defect rate of the finished heavy rails was reduced by 25%, and the stability of mechanical properties was improved.
[0053] Comparative Example 2: Control test of single-component modifier (borate only). Except for the type of modifier, all other process conditions and parameters in this comparative example are consistent with those in Example 1, so as to examine the synergistic effect of each component in the composite modifier individually.
[0054] S1. Basic slag ratio and pretreatment: Same as in Example 1 (CaO 48%, Al2O3 35%, SiO2 6.5%, MgO 5.5%, CaO / Al2O3=1.37), pretreatment at 350℃ for 2 hours.
[0055] S2. Modifier addition: Only anhydrous borax is added as a modifier, with an addition amount of 3.0% of the total mass of the base slag, and it is added in one go.
[0056] S3, Segmented slag smelting: Same as Example 1 (first stage 900kW / 4min to 1460℃, second stage 1300kW / 5min, argon flow rate 10L / (min·t steel), intermittent stirring).
[0057] S4. Slag System Steady-State Control: The slag melting point was measured to be 1555℃. The slag formation time was only shortened by 12% compared to the traditional fluorite process, with limited improvement in slag fluidity, a reduction of only 8% in the total oxygen content of the molten steel, and no significant improvement in furnace lining erosion. This indicates that the fluxing effect of a single borate is limited and cannot achieve the synergistic melting reduction effect of the composite modifier of this invention.
[0058] Table 1 shows a comparison of the technical effects:
[0059] The above supplementary embodiments fully demonstrate that the method of the present invention exhibits stable low-temperature melting effect and excellent metallurgical quality improvement capability under different steel grades and different process parameter boundary conditions, and its comprehensive performance is far superior to traditional fluorite process and single-component modification scheme.
Claims
1. A method for controlling the fluorine-free composite flux and slag system in an LF refining furnace, characterized in that, include: S1. Initial material preparation and slag ratio control: Based on the LF refining steel grade, prepare fluorine-free low-melting-point refining base slag, and control the mass ratio of CaO to Al2O3 in the base slag to be 1.1~1.5, and the mass fraction of SiO2 ≤8%; S2. Addition of composite flux modifier: In the initial stage of LF refining with energized slag formation, a composite flux modifier is added to the ladle. The composite flux modifier is composed of nano alumina powder, borates, and titanates. S3. Segmented heating and slag treatment: A segmented electric heating process is adopted in combination with bottom blowing argon gas stirring. First, low temperature pretreatment is carried out, and then high temperature melting is carried out to promote the complete melting of slag. S4. Slag System Steady-State Control: After the slag is completely melted, maintain the slag melting point at 1490℃~1530℃.
2. The method according to claim 1, characterized in that, The basic slag, by mass percentage, comprises: 45%~48% CaO, 32%~38% Al2O3, 5%~8% SiO2, 4%~7% MgO, with the balance being unavoidable impurities.
3. The method for fluorine-free composite fluxing and slag system control in LF refining furnaces according to claim 1, characterized in that, The amount of the composite flux modifier added is 2.0% to 4.5% of the total mass of the base slag.
4. The method for fluorine-free composite fluxing and slag system control in LF refining furnaces according to claim 1, characterized in that, The mass ratio of the nano-alumina powder, borate, and titanate is 3:2:
1.
5. The method for fluorine-free composite fluxing and slag system control for LF refining furnaces according to claim 1, characterized in that, The nano-alumina powder has a particle size of 200 nm to 500 nm, the borate is anhydrous borax, and the titanate is calcium metatitanate.
6. The method for fluorine-free composite fluxing and slag system control in LF refining furnaces according to claim 1, characterized in that, The segmented heating and slag-removing treatment includes: In the first stage, the power supply is 800 kW to 1000 kW, the temperature rises in 3 min to 5 min, and the temperature of the steel slag system is controlled to 1450℃ to 1470℃; In the second stage, the power supply is increased to 1200 kW~1400 kW, and the constant temperature melting is carried out for 4 min~6 min.
7. The method for fluorine-free composite fluxing and slag system control in LF refining furnaces according to claim 1, characterized in that, During the segmented heating and slag treatment process, bottom blowing argon gas is used for stirring throughout the process, and the argon gas flow rate is controlled at 8 L / (min·t steel) to 12 L / (min·t steel).
8. The method for fluorine-free composite fluxing and slag system control for LF refining furnaces according to claim 1, characterized in that: The composite flux modifier is added in batches, with 60% to 70% of the total amount added initially, and the remaining amount added after the first stage of heating is completed.
9. The method for fluorine-free composite fluxing and slag system control in LF refining furnaces according to claim 1, characterized in that, The bottom-blown argon gas is produced using an intermittent stirring mode, with a stirring-to-pause time ratio of (1~2):
1.
10. The method for fluorine-free composite fluxing and slag system control for LF refining furnaces according to claim 1, characterized in that: The preparation of the basic slag adopts a premixing and preheating process. After the raw materials are mixed evenly, they are preheated to 300℃~400℃ and kept at that temperature for 1 h~3 h.