A method for quenching and tempering a forged piece of a lower transition section of a coal direct liquefaction reactor
By setting buffer blocks on the forgings in the lower transition section of the direct coal liquefaction reactor and stacking them in a staggered manner, a stable cooling gap and support structure are formed, which solves the problem of deformation caused by uneven cooling during tempering heat treatment of forgings, and improves production efficiency and yield.
Patent Information
- Application Number
- CN202611422580.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
During the tempering heat treatment process, the forgings in the lower transition section of the direct coal liquefaction reactor are prone to heat treatment deformations such as warping and elliptical deformation due to uneven wall thickness and complex shape, which affect production efficiency and yield.
Multiple buffer blocks are set at both ends of the lower transition section forging to form a circumferentially spaced distribution. Two pre-treated forgings are stacked with opposite orientations and circumferentially staggered to form a stable cooling gap and cross support structure for tempering heat treatment.
It effectively suppressed the heat treatment deformation of forgings, improved the utilization rate of quenching equipment, shortened the production cycle, reduced energy consumption, and ensured the mechanical properties of forgings.
Smart Images

Figure CN123152844A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat treatment technology for metallic materials, and more specifically, to a method for tempering heat treatment of forgings in the transition section of a direct coal liquefaction reactor. Background Technology
[0002] The direct coal liquefaction reactor is the core hydrogen-bearing pressure vessel in the direct coal liquefaction process. The lower transition section forging is a crucial component connecting the reactor shell and the end caps, typically manufactured as a single piece using low-alloy heat-resistant steel such as 2.25Cr-1Mo-0.25V. This forging has a lantern-shaped, near-net-shape profile, characterized by its complex shape and significant variations in wall thickness. The quenching and tempering heat treatment (quenching + tempering) is a critical process determining the final mechanical properties of the lower transition section forging, directly impacting the reactor's operational safety and service life.
[0003] Currently, forgings in the lower transition section are prone to heat treatment deformations such as warping and elliptical deformation due to uneven wall thickness and complex shapes, resulting in significant differences in cooling rates at different parts during quenching. In actual production, the deformation of forgings after quenching and tempering is usually large, requiring a significant amount of time for subsequent shaping, which affects production efficiency and yield.
[0004] Therefore, for the tempering heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor, how to effectively reduce heat treatment deformation while ensuring the mechanical properties of the forgings is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] The problem addressed by this invention is: how to effectively reduce heat treatment deformation while ensuring the mechanical properties of forgings in the transition section of a direct coal liquefaction reactor.
[0006] To address the above problems, this invention provides a method for heat treatment of forgings in the transition section of a direct coal liquefaction reactor, comprising: Step S1: Set multiple buffer blocks at one end of the axial ends of the lower transition section forging to obtain a pre-treated lower transition forging; wherein, the multiple buffer blocks are distributed at intervals along the circumferential direction of the lower transition section forging. Step S2: Assemble the two pre-treated lower transition forgings into a stacked state to obtain a combined forging; wherein, in the combined forging, the upper pre-treated lower transition forging and the lower pre-treated lower transition forging face opposite directions, and the two are offset by a preset angle in the circumferential direction, so that the buffer block on the upper pre-treated lower transition forging abuts and supports the lower lower transition forging, and the buffer block on the lower pre-treated lower transition forging abuts and supports the upper lower transition forging, and a cooling gap is formed between the upper and lower lower transition forgings; Step S3: Perform quenching and tempering heat treatment on the combined forging.
[0007] Optionally, in step S1, two buffer blocks are provided at one end of the axial ends of the lower transition section forging, and the two buffer blocks are evenly spaced along the circumferential direction of the lower transition section forging.
[0008] Optionally, in step S2, the preset angle is 90 degrees.
[0009] Optionally, the inner diameter of the lower transition section forging is 4720mm to 4800mm, the outer diameter is 5480mm to 5560mm, and the height is 810mm to 850mm.
[0010] Optionally, the buffer block is a sector-shaped block, with the center of the sector-shaped block located on the axis of the lower transition section forging; the radial width of the buffer block is 360mm to 400mm, the axial height is 360mm to 400mm, and the outer arc length is 1100mm to 1180mm.
[0011] Optionally, in step S3, the quenching and tempering heat treatment includes: heating the combined forging to the austenitizing temperature, holding it at that temperature, and then quenching and tempering at high temperature; wherein the austenitizing temperature is 920°C to 950°C.
[0012] Optionally, the high-temperature tempering temperature is 650°C to 700°C.
[0013] Optionally, in step S1, the buffer block is set by welding.
[0014] Optionally, the buffer block is made of the same material as the lower transition section forging.
[0015] Optionally, the material of the lower transition section forging is 2.25Cr-1Mo-0.25V steel.
[0016] Compared with related technologies, this invention sets multiple buffer blocks spaced circumferentially at one end of the lower transition section forging, and stacks two pre-treated lower transition forgings with opposite orientations and circumferential misalignment, allowing the upper and lower forgings to abut and support each other through their respective buffer blocks, thereby forming a stable cooling gap between them. This cooling gap allows the quenching medium to flow fully through the space between the upper and lower forgings during the tempering heat treatment process, ensuring uniform cooling of the inner surface of the forging facing the gap side, avoiding thermal stress concentration and non-uniform deformation caused by uneven cooling in traditional single-piece independent processing. Simultaneously, the cross-support structure formed by the buffer blocks mutually constrains the upper and lower forgings throughout the heat treatment heating, holding, and cooling processes, effectively suppressing deformation trends such as ellipticity changes and end-face warping caused by the forging's own weight or phase transformation stress, enhancing the overall shape stability of the forging. Furthermore, stacking two forgings in the same furnace changes the traditional "one furnace, one piece" independent processing mode, significantly improving the utilization rate of large quenching equipment and heat treatment furnaces, shortening the overall cycle of mass production, and reducing energy consumption per unit product. Therefore, for the tempering heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor, the method of this invention can effectively reduce heat treatment deformation while ensuring that the forgings obtain the required mechanical properties, and at the same time achieve intensive production, improve efficiency and reduce costs. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the structure of the lower transition section forging in an embodiment of the present invention; Figure 2 This is a schematic diagram of the pre-treated transition forging in an embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of the combined forging in an embodiment of the present invention.
[0018] Explanation of reference numerals in the attached figures: 1. Buffer block. Detailed Implementation
[0019] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Although some embodiments of the present invention are shown in the drawings, it should be understood that the present invention can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the accompanying drawings and embodiments of the present invention are for illustrative purposes only and are not intended to limit the scope of protection of the present invention.
[0020] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0021] The term "comprising" and its variations as used herein are open-ended, meaning "including but not limited to"; the term "based on" means "at least partially based on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one additional embodiment"; the term "some embodiments" means "at least some embodiments"; and the term "optionally" means "optional embodiments". Definitions of other terms will be given in the following description. It should be noted that the concepts of "first," "second," etc., mentioned in this invention are used to distinguish different objects, not to describe a specific order or hierarchy. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0022] It should be noted that, as Figure 1 As shown, in this invention, the inner and outer diameters of the lower transition section forging both refer to the dimensions corresponding to its riser end.
[0023] This invention provides a method for heat treatment of forgings in the transition section of a direct coal liquefaction reactor, comprising: Step S1: Set multiple buffer blocks 1 at one end of the axial ends of the lower transition section forging to obtain a pre-treated lower transition forging, such as... Figure 2 As shown; wherein, multiple buffer blocks 1 are distributed at circumferential intervals along the lower transition section forging; as Figure 1 As shown, the axial ends of the lower transition section forging are the sprue end and the riser end, respectively. Figure 2 As shown, exemplarily, the buffer block 1 is disposed at the sprue end of the lower transition section forging; Step S2: Assemble the two pre-treated transition forgings into a stacked state to obtain a combined forging, such as... Figure 3 As shown; where, as Figure 3As shown, in the combined forging, the upper pre-treated lower transition forging and the lower pre-treated lower transition forging face opposite directions (i.e., their sprue ends face each other), and the two are offset by a preset angle in the circumferential direction, so that the buffer block 1 on the upper pre-treated lower transition forging abuts and supports the lower transition forging, and the buffer block 1 on the lower pre-treated lower transition forging abuts and supports the upper lower transition forging, and a cooling gap is formed between the upper and lower lower transition forgings; Step S3: Perform quenching and tempering heat treatment on the combined forging.
[0024] In this embodiment of the invention, multiple buffer blocks 1 are arranged at intervals along the circumference at one end of the lower transition section forging. Two pre-treated lower transition forgings are stacked one on top of the other, facing opposite directions and circumferentially offset. The upper and lower forgings are supported by their respective buffer blocks 1, forming a stable cooling gap between them. This cooling gap allows the quenching medium to flow fully through the space between the upper and lower forgings during the tempering heat treatment process, ensuring uniform cooling of the inner surface of the forging facing the gap. This avoids the thermal stress concentration and non-uniform deformation caused by uneven cooling, which is common in traditional single-piece independent processing. Simultaneously, the cross-support structure formed by the buffer blocks 1 mutually constrains the upper and lower forgings throughout the heat treatment heating, holding, and cooling processes, effectively suppressing deformation trends such as ellipticity changes and end-face warping caused by the forging's own weight or phase transformation stress, thus enhancing the overall shape stability of the forging. Furthermore, stacking two forgings in the same furnace changes the traditional "one furnace, one piece" independent processing mode, significantly improving the utilization rate of large quenching equipment and heat treatment furnaces, shortening the overall cycle of mass production, and reducing energy consumption per unit product. Therefore, for the tempering heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor, the method of this invention can effectively reduce heat treatment deformation while ensuring that the forgings obtain the required mechanical properties, and at the same time achieve intensive production, improve efficiency and reduce costs.
[0025] In some embodiments of the present invention, such as Figure 2 and Figure 3As shown, in step S1, two buffer blocks 1 are set at one end of the axial ends of the lower transition section forging, and the two buffer blocks 1 are evenly spaced along the circumference of the lower transition section forging, with a preset angle of 90 degrees. In this embodiment, two buffer blocks 1 are set at one end of the lower transition section forging, and the upper and lower forgings are stacked with a 90-degree offset in the circumferential direction. The two buffer blocks 1 are symmetrically distributed at 180 degrees in the circumferential direction, and with the 90-degree rotational offset, the buffer blocks 1 of the upper and lower forgings form a uniform four-point support structure in the circumferential direction. This four-point support structure is subjected to balanced force, which can evenly transfer the weight of the upper forging to the lower forging, avoiding local stress concentration and tilting deformation caused by eccentric loading. At the same time, the 90-degree offset makes the buffer blocks 1 of the upper and lower forgings completely offset in the circumferential direction, and each falls into the gap of the buffer block 1 of the other forging, forming a stable interlocking structure, which effectively constrains the ellipticity change and end face warping of the forgings throughout the heat treatment process, further improving the deformation control effect. In addition, the two buffer blocks 1 are designed to balance support stability and ease of operation, ensuring a sufficient number of support points while reducing the amount of welding work.
[0026] In some embodiments of the present invention, such as Figure 1 As shown, the inner diameter of the lower transition section forging is 4720mm to 4800mm, the outer diameter is 5480mm to 5560mm, and the height is 810mm to 850mm; Figure 2 As shown, the buffer block 1 is a fan-shaped block, with its center located on the axis of the lower transition section forging. The buffer block 1 has a radial width of 360mm to 400mm, an axial height of 360mm to 400mm, and an outer arc length of 1100mm to 1180mm. In this embodiment, the fan-shaped buffer block 1 avoids welding defects or stress concentration caused by shape mismatch. The radial width of the buffer block 1 is basically equivalent to the wall thickness of the forging, ensuring a sufficiently large supporting area to withstand the weight of the upper forging without crushing or excessive plastic deformation. The axial height of the buffer block 1, 360mm to 400mm, ensures sufficient flow of quenching medium and uniform cooling without weakening the mutual constraint between the upper and lower forgings due to excessive gaps. The circumferential span corresponding to the outer arc length of 1100mm to 1180mm is moderate, providing sufficient supporting contact area and leaving ample cooling medium flow channels between adjacent buffer blocks 1.
[0027] In some embodiments of the present invention, step S3, the quenching and tempering heat treatment includes: heating the combined forging to the austenitizing temperature, holding it at that temperature, and then quenching and high-temperature tempering; wherein the austenitizing temperature is 920°C to 950°C, and the high-temperature tempering temperature is 650°C to 700°C. In this embodiment, the quenching temperature range is within the austenitizing temperature range of 2.25Cr-1Mo-0.25V steel, which allows the carbides in the steel to fully dissolve and the alloying elements to diffuse uniformly into the austenite, laying the foundation for obtaining a uniform microstructure during subsequent quenching, while avoiding excessively high temperatures that could lead to coarsening of the austenite grains. After quenching, high-temperature tempering at 650°C to 700°C allows the quenched microstructure to fully decompose and transform, forming a stable tempered bainite microstructure, while also eliminating the internal stress generated during quenching. This tempering temperature range achieves a good balance between strength and toughness. It avoids insufficient toughness due to excessively low tempering temperatures, and excessive strength loss due to excessively high tempering temperatures. This helps to further refine the size and distribution of carbide particles, thereby improving the hydrogen embrittlement resistance and long-term service stability of forgings.
[0028] In some embodiments of the present invention, in step S1, the buffer block 1 is set by welding. In this embodiment, the buffer block 1 is set at the end of the lower transition section forging by welding. Welded connections have the advantages of high connection strength and good reliability, ensuring that the buffer block 1 remains firmly connected throughout the heat treatment process, without loosening, falling off, or shifting, thereby ensuring that the support structure and cooling gap between the upper and lower forgings remain stable and reliable.
[0029] In some embodiments of the present invention, the buffer block 1 is made of the same material as the lower transition section forging. In this embodiment, the buffer block 1 and the lower transition section forging are made of the same material. Using the same material avoids problems such as welding cracks, interface stress concentration, or electrochemical corrosion caused by differences in thermal expansion coefficients, chemical compositions, or phase transformation behaviors when welding dissimilar materials. During the quenching and tempering heat treatment process, the buffer block 1 and the forging undergo the same heating and cooling process, and their expansion and contraction behaviors are completely synchronized, preventing weld interface peeling or deformation of the buffer block 1 due to differences in thermal stress.
[0030] In some embodiments of the present invention, the lower transition section forging is made of 2.25Cr-1Mo-0.25V steel. This steel grade is a typical grade of steel used in hydrogenation reactors, possessing good high-temperature strength, resistance to hydrogen embrittlement, and resistance to temper embrittlement. It is widely used in key pressure-bearing components in high-temperature and high-pressure hydrogen-environment environments such as direct coal liquefaction reactors.
[0031] The present invention will be further described below with reference to specific embodiments.
[0032] Example 1 A1, such as Figure 1As shown, the axial ends of the lower transition section forging are the sprue end and the riser end, respectively. Two buffer blocks are welded to the sprue end of the lower transition section forging to obtain the pretreated lower transition forging, as shown. Figure 2 As shown; wherein, the two buffer blocks are evenly spaced along the circumference of the lower transition section forging; the inner diameter of the lower transition section forging is 4760mm, the outer diameter is 5520mm, and the height is 830mm; the buffer block is a fan-shaped block, and the center of the corresponding circle of the fan-shaped block is located on the axis of the lower transition section forging; the radial width of the buffer block is 380mm, the axial height is 380mm, and the outer arc length is 1140mm; the material of the lower transition section forging and the buffer block is 2.25Cr-1Mo-0.25V steel.
[0033] A2. Assemble the two pre-treated transition forgings into a stacked state to obtain a combined forging, such as... Figure 3 As shown; where, as Figure 3 As shown, in the combined forging, the upper pre-treated lower transition forging and the lower pre-treated lower transition forging face opposite directions (i.e., their sprue ends face each other), and they are offset by a preset angle in the circumferential direction, so that the buffer block on the upper pre-treated lower transition forging abuts and supports the lower transition forging, and the buffer block on the lower pre-treated lower transition forging abuts and supports the upper lower transition forging, forming a cooling gap between the upper and lower lower transition forgings; wherein, the preset angle is 90 degrees.
[0034] A3. The combined forging is subjected to quenching and tempering heat treatment; wherein, the quenching and tempering heat treatment includes: first heating the combined forging to 930°C and holding it for 8 hours, then quenching and cooling it, and then tempering it at a high temperature of 670°C for 10 hours.
[0035] A4. After the quenching and tempering heat treatment is completed, the combined forging is disassembled to obtain the heat-treated lower transition section forging.
[0036] Example 2 The difference from Example 1 is that in step A1, the radial width of the buffer block is 360mm, the axial height is 360mm, and the outer arc length is 1180mm.
[0037] Example 3 The difference from Example 1 is that in step A1, the radial width of the buffer block is 400mm, the axial height is 400mm, and the outer arc length is 1100mm.
[0038] Comparative Example 1 A single lower transition section forging is subjected to quenching and tempering heat treatment to obtain a heat-treated lower transition section forging. The quenching and tempering heat treatment includes: first heating the lower transition section forging to 930℃ and holding it at that temperature for 8 hours, then quenching and cooling it, followed by high-temperature tempering at 670℃ for 10 hours. The lower transition section forging has an inner diameter of 4760mm, an outer diameter of 5520mm, and a height of 830mm. The material of the lower transition section forging is 2.25Cr-1Mo-0.25V steel.
[0039] Comparative Example 2 Two lower transition forgings are assembled in a stacked manner to obtain a combined forging; in the combined forging, the upper transition forging and the lower lower transition forging face opposite directions (i.e., their sprue ends face each other); the inner diameter of the lower transition section forging is 4760mm, the outer diameter is 5520mm, and the height is 830mm; the material of the lower transition section forging is 2.25Cr-1Mo-0.25V steel.
[0040] The composite forging is subjected to quenching and tempering heat treatment; wherein, the quenching and tempering heat treatment includes: first heating the composite forging to 930°C and holding it at that temperature for 8 hours, then quenching and cooling it, and then tempering it at a high temperature of 670°C for 10 hours.
[0041] After the quenching and tempering heat treatment is completed, the combined forging is disassembled to obtain the heat-treated lower transition section forging.
[0042] Effect Example Twenty heat-treated lower transition section forgings were prepared using the methods of Examples 1 to 3 and Comparative Examples 1 to 2, respectively. The mechanical properties and deformation of each group of forgings were tested, and the average values were taken. The results are shown in Table 1. As can be seen from Table 1, compared with Comparative Examples 1 to 2, the heat-treated lower transition section forgings prepared by Examples 1 to 3 are basically equivalent in mechanical properties and all meet the industry standard requirements. However, in terms of deformation, Examples 1 to 3 are significantly better than Comparative Examples 1 to 2, and the deformation is significantly reduced.
[0043] Table 1
[0044] It should be noted that AKv in Table 1 is used to characterize impact toughness, representing the energy absorbed by the material when subjected to impact load.
[0045] The deformation measurement method in Table 1 is as follows: Eight directional measurement points are evenly selected in the circumference of the forging in the lower transition section after heat treatment. The diameter deviation of each point from that before quenching and tempering is measured, and the average value of the difference of each measurement point is taken as the deformation.
[0046] While the present invention has been disclosed above, its scope of protection is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention, and all such changes and modifications will fall within the scope of protection of the present invention.
Claims
1. A method for heat treatment of forgings in the transition section of a direct coal liquefaction reactor, characterized in that, include: Step S1: Set multiple buffer blocks (1) at one end of the axial ends of the lower transition section forging to obtain a pre-treated lower transition forging; wherein, the multiple buffer blocks (1) are distributed at intervals along the circumferential direction of the lower transition section forging. Step S2: Assemble the two pre-treated lower transition forgings into a stacked state to obtain a combined forging; wherein, in the combined forging, the upper pre-treated lower transition forging and the lower pre-treated lower transition forging face opposite directions, and the two are offset by a preset angle in the circumferential direction, so that the buffer block (1) on the upper pre-treated lower transition forging abuts and supports the lower transition forging, and the buffer block (1) on the lower pre-treated lower transition forging abuts and supports the lower transition forging, and a cooling gap is formed between the upper and lower lower transition forgings; Step S3: Perform quenching and tempering heat treatment on the combined forging.
2. The method for heat treatment of forgings in the transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, In step S1, two buffer blocks (1) are provided at one end of the axial ends of the lower transition section forging, and the two buffer blocks (1) are evenly spaced along the circumferential direction of the lower transition section forging.
3. The method for tempering and heat treatment of forgings in the transition section of a direct coal liquefaction reactor according to claim 2, characterized in that, In step S2, the preset angle is 90 degrees.
4. The method for tempering and heat treatment of forgings in the transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, The lower transition section forging has an inner diameter of 4720mm to 4800mm, an outer diameter of 5480mm to 5560mm, and a height of 810mm to 850mm.
5. The method for tempering and heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor according to claim 4, characterized in that, The buffer block (1) is a fan-shaped block, and the center of the fan-shaped block is located on the axis of the lower transition section forging; the radial width of the buffer block (1) is 360mm to 400mm, the axial height is 360mm to 400mm, and the outer arc length is 1100mm to 1180mm.
6. The method for tempering and heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, In step S3, the quenching and tempering heat treatment includes: heating the combined forging to the austenitizing temperature, holding it at that temperature, and then quenching and tempering at high temperature; wherein the austenitizing temperature is 920°C to 950°C.
7. The method for tempering and heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor according to claim 6, characterized in that, The temperature for high-temperature tempering is 650℃ to 700℃.
8. The method for heat treatment of forgings in the transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, In step S1, the buffer block (1) is set by welding.
9. The method for tempering heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, The buffer block (1) is made of the same material as the lower transition section forging.
10. The method for tempering and heat treatment of forgings in the lower transition section of a direct coal liquefaction reactor according to claim 1, characterized in that, The material of the lower transition section forging is 2.25Cr-1Mo-0.25V steel.