A method of wet processing of beryllium glass to suppress aluminum-enhanced leaching

By constructing a carbonate/bicarbonate buffer system through CO₂ pressure leaching technology, the problems of low beryllium leaching rate and severe impurity dissolution in the wet processing of beryllium glass were solved, achieving efficient beryllium leaching and separation of iron and aluminum impurities, reducing production costs and environmental pressure.

CN123152879APending Publication Date: 2026-11-24CHINA ENFI ENG CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611446789.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies in the wet processing of beryllium glass suffer from low beryllium leaching rates, severe impurity dissolution, high production costs, and significant environmental pressures. There is a lack of systematic research on the applicability and selective separation mechanism of CO₂ pressurization technology in the field of beryllium glass.

Method used

A CO₂ pressure leaching technology was used to construct a carbonate/bicarbonate buffer system. By forming a soluble complex with beryllium ions through HCO₃⁻, combined with a high temperature and high pressure environment, efficient leaching of beryllium and selective separation of iron and aluminum impurities were achieved.

Benefits of technology

Increase beryllium leaching rate to 97%, reduce aluminum leaching rate to below 30%, reduce chemical reagent consumption in subsequent impurity removal processes, simplify process flow, reduce production costs, reduce wastewater discharge, and achieve resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152879A_ABST
    Figure CN123152879A_ABST
Patent Text Reader

Abstract

This invention provides a hydrometallurgical method for leaching beryllium glass with aluminum-inhibiting and enhanced properties, belonging to the field of hydrometallurgical technology. The method includes mixing the beryllium glass to be treated, a strong acid leaching aid, and water, and placing the mixture in an autoclave for slurry treatment; heating the autoclave and introducing CO2 gas to achieve a preset leaching temperature and pressure for leaching reaction; after the leaching reaction, cooling the autoclave, depressurizing, and separating the solid and liquid phases to obtain a beryllium-rich leachate and iron-aluminum slag. This invention maintains a high dissolved CO2 concentration in the liquid phase through pressurization, resulting in a more stable local acid-base environment and reducing drastic local pH fluctuations at the solid-liquid interface caused by rapid mineral dissolution. Simultaneously, the CO2 dissolved in the liquid phase forms a carbonic acid system, which may react with the leached Be. 2+ Formation of weak coordination or weak complexation reduces the amount of free Be in the solution. 2+ The activity promotes the dissolution of beryllium glass, increases the beryllium leaching rate, and achieves the technical effect of beryllium leaching rate ≥97% and aluminum leaching rate ≤30%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrometallurgical technology, and more specifically, to a hydrometallurgical treatment method for aluminum-inhibiting and strengthening leaching of beryllium glass. Background Technology

[0002] Beryllium glass, as an important secondary resource for beryllium extraction, is primarily treated using atmospheric pressure acid / alkali leaching via wet processing. Existing technologies typically improve beryllium leaching rates by increasing leaching agent concentration, raising temperature, extending reaction time, or adding oxidants. However, these methods have several drawbacks: Firstly, under atmospheric pressure, the beryllium leaching reaction is hampered by the solid product layer, resulting in slow kinetics and generally low leaching rates. Secondly, simply increasing the leaching agent concentration exacerbates the simultaneous dissolution of impurities such as iron (Fe) and aluminum (Al), leading to the consumption of large amounts of chemical reagents in subsequent impurity removal processes and increasing the risk of valuable metal co-precipitation losses, significantly increasing production costs and process complexity. Furthermore, excessive use of acid / alkali increases wastewater treatment load and creates significant environmental pressure.

[0003] In recent years, CO2 pressure leaching technology has been gradually applied in the field of mineral processing. Its core lies in utilizing the carbonate / bicarbonate buffer system formed after CO2 dissolves in water, and selectively dissolving or separating metal ions by adjusting the pH of the slurry. For example, in the processing of uranium- and vanadium-containing mineral resources, CO2 pressure leaching has been proven to effectively construct complex leaching systems or achieve the selective removal of calcium and magnesium impurities.

[0004] However, the aforementioned CO2 pressurization technologies are all designed for primary minerals or intermediate products from specific smelting processes, whose phase composition and reactivity differ fundamentally from beryllium glass. Beryllium glass is a dense pyrometallurgical product obtained through a high-temperature melting-water quenching process, and its Si-O-Be network structure is highly stable. The CO2 pressurization system, however, can only provide a weakly acidic environment with a pH of 3.5–6.0, which cannot effectively disrupt its phase structure and release beryllium. The applicability and selective separation mechanism of CO2 pressurization technology in the field of beryllium glass lack systematic research, representing a technological gap.

[0005] Therefore, there is an urgent need for a wet processing method for beryllium glass that can utilize the pressurization characteristics of CO2 to achieve efficient leaching of beryllium and in-situ suppression of Fe / Al impurities. Summary of the Invention

[0006] In view of the above problems, the object of the present invention is to provide a wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass, so as to solve at least one problem existing in the prior art.

[0007] Firstly, this invention provides a wet processing method for beryllium glass leaching with aluminum-inhibiting enhancement, comprising the following steps: Step 1, mixing the beryllium glass to be treated, a strong acid leaching aid, and water, and placing the mixture in an autoclave for slurry treatment; Step 2, heating the autoclave and introducing CO2 gas to achieve a preset leaching temperature and pressure, and carrying out a leaching reaction; Step 3, after the leaching reaction is completed, cooling the autoclave, depressurizing it to atmospheric pressure, and performing solid-liquid separation on the reaction slurry to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue. It should be noted that sulfuric acid leaches easily leached amorphous silicate minerals from the beryllium glass, while continuous CO2 pressurization maintains a high dissolved CO2 concentration in the liquid phase, making the local acid-base environment more stable and reducing the drastic local pH fluctuations at the solid-liquid interface caused by rapid mineral dissolution. Simultaneously, CO2 dissolves in the liquid phase to form a carbonic acid system, which may react with the leached Be... 2+ Formation of weak coordination or weak complexation reduces the amount of free Be in the solution. 2+ The activity of beryllium glass is increased, thereby promoting its further dissolution and improving the beryllium leaching rate. At the same time, the high-temperature environment allows iron and aluminum to exist stably in the slag phase in the form of oxides / hydroxides, achieving selective separation.

[0008] Further, a preferred technical solution is that, in step two, CO2 gas is first introduced into the autoclave to replace the air inside, and the temperature is raised to a first set temperature, then the exhaust valve is closed; wherein, the first set temperature is 95-100℃; CO2 gas continues to be introduced into the autoclave, the pressure inside the autoclave is adjusted to 0.5~2.0 MPa, the temperature is raised to 150~180℃, and the leaching reaction is carried out under constant temperature and pressure for 1~4 hours. It should be noted that, during the air replacement stage, the pressure reducing valve of the autoclave remains open, and the autoclave body is connected to the atmosphere; if the slurry temperature is ≤100℃ and the water evaporation rate is slow, the pressure reducing valve can be kept open for a long time to continuously introduce CO2 to replace the air. Once the temperature rises to 100℃ or above, the slurry will boil violently, and a large amount of water vapor will leak out with the replacement gas, causing water loss and liquid-solid ratio imbalance in the system. Therefore, the pressure reducing valve must be closed and sealed before the temperature reaches 100℃ to prevent a large amount of water vapor from escaping and damaging the leaching material system. Thus, the first set upper limit of temperature is 100℃.

[0009] Furthermore, a preferred technical solution is that, in step one, the strong acid leaching aid is sulfuric acid and / or hydrochloric acid.

[0010] Furthermore, a preferred technical solution is that, in step one, the acid-to-ore ratio is controlled to be 1100~1200 kg / t, and the liquid-to-solid ratio is (15~20):1.

[0011] Furthermore, a preferred technical solution is that, in step one, the stirring rate of the slurry treatment is 600~800 rpm.

[0012] Furthermore, a preferred technical solution is that, in step two, the pH at the leaching endpoint of the leaching reaction is 1.2 to 1.8.

[0013] Furthermore, a preferred technical solution is that, in step two, the CO2 gas is industrial waste gas.

[0014] Furthermore, a preferred technical solution is that the high-pressure reactor is a continuous high-pressure reactor or an intermittent high-pressure reactor.

[0015] Furthermore, a preferred technical solution is to include a pretreatment step before step one: ball milling the beryllium glass to be treated so that the proportion of material on the 120-mesh sieve is ≥85%.

[0016] Furthermore, a preferred technical solution is that, after the leaching reaction is completed, the beryllium leaching rate is ≥97% and the aluminum leaching rate is ≤30%.

[0017] The wet processing method for beryllium glass with aluminum-inhibiting and enhanced leaching provided by this invention introduces CO2 pressure leaching technology, constructs a carbonate / bicarbonate buffer system, and utilizes HCO3- - The beryllium leaching method enhances the leaching kinetics of valuable elements by forming soluble complexes with beryllium ions, achieving a beryllium leaching rate of ≥97%. Simultaneously, the weakly acidic environment of this buffer system allows for a significant reduction in aluminum leaching rate (≤30%) and iron leaching rate, substantially reducing impurity introduction at the source. Furthermore, the significantly reduced impurity content in the leachate decreases the consumption of alkali for subsequent neutralization and impurity removal, significantly reducing the difficulty of solid-liquid separation, shortening the process flow, and lowering overall production costs. This invention's aluminum-inhibiting and enhanced leaching method for beryllium glass wet processing requires only one stage of CO2 pressurized leaching to achieve leaching and separation, which is simpler than existing CO2 pressurized technologies that require two or more stages of pressurized stepwise impurity removal. Moreover, the use of pure CO2 pressurization eliminates the need for external acid, alkali, or salt reagents, reducing wastewater discharge by 40%. Furthermore, industrial waste gas CO2 can be used for carbon capture and resource utilization, ultimately achieving the technical effects of efficient leaching of valuable elements and simultaneous suppression of iron and aluminum impurities in the beryllium glass wet processing.

[0018] To achieve the foregoing and related objectives, one or more aspects of the invention include the features that will be described in detail below. The following description details certain exemplary aspects of the invention. However, these aspects indicate only a few of the various ways in which the principles of the invention can be used. Furthermore, the invention is intended to include all such aspects and their equivalents. Attached Figure Description

[0019] Other objects and results of the invention will become more apparent and readily understood with reference to the following description taken in conjunction with the accompanying drawings. In the drawings: Figure 1 This is a schematic flowchart of a wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to an embodiment of the present invention. Detailed Implementation

[0020] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation methods and typical parameters of the present invention, and are not intended to limit the parameter range described in the present invention. Reasonable variations derived therefrom are still within the protection scope of the claims of the present invention.

[0021] It should be noted that the endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0022] Unless otherwise defined, all terms, symbols, and other scientific terms used herein are intended to have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In some instances, terms having a conventional meaning are defined herein for clarification or ease of reference, and such definitions should not be construed as indicating a significant difference from conventional understanding in the art. The technical methods described or referenced herein are generally well understood by those skilled in the art and employed by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents, and instruments shall be performed according to the manufacturer's instructions and parameters.

[0023] References to "one embodiment" or "some embodiments" as described in this specification mean that one or more embodiments of this application include a specific feature, structure, or characteristic described in connection with that embodiment. Therefore, the phrases "in one embodiment," "in some embodiments," "in other embodiments," "in still other embodiments," etc., appearing in different parts of this specification do not necessarily refer to the same embodiment, but rather mean "one or more, but not all, embodiments," unless otherwise specifically emphasized. The terms "comprising," "including," "having," and variations thereof mean "including but not limited to," unless otherwise specifically emphasized.

[0024] Existing CO2 pressure leaching methods typically rely on bicarbonate complexation for solubilization, function solely as pH adjusters or precipitants, or simply utilize pressure to enhance mass transfer; none address materials like beryllium glass used in pyrometallurgical processes. This invention provides a wet processing method for beryllium glass with aluminum-inhibiting leaching, overcoming the misconception that the Si-O-Be network structure of beryllium glass cannot be disrupted by CO2 pressure leaching. This invention employs a synergistic approach of CO2 pressure leaching and a small amount of strong acid, achieving both efficient beryllium leaching and in-situ suppression of Fe / Al impurities.

[0025] Figure 1 A flowchart of a wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to an embodiment of the present invention is shown, as follows: Figure 1 As shown. The present invention provides a wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass, comprising the following steps: Step 1, mixing the beryllium glass to be treated, a strong acid leaching aid, and water, and placing the mixture in an autoclave for slurry processing.

[0026] Step 2: The autoclave is heated and CO2 gas is introduced to bring the autoclave to a preset leaching temperature and pressure for leaching reaction. In a specific embodiment, in Step 2, CO2 gas is first introduced into the autoclave to replace the air inside, and the temperature is raised to a first set temperature, then the exhaust valve is closed; wherein, the first set temperature is 95-100℃; CO2 gas is continued to be introduced into the autoclave, the pressure inside the autoclave is adjusted to 0.5~2.0MPa, the temperature is raised to 150~180℃, and the leaching reaction is carried out under constant temperature and pressure for 1~4 hours.

[0027] It should be noted that although beryllium glass undergoes high-temperature dissociation using alkaline flux, and most of the beryllium-containing phases have transformed from beryl phases into easily leached amorphous silicate phases, a certain amount of stable silicate phases that are difficult to leach still remain. The existing sulfuric acid aging followed by water leaching process for beryllium glass still faces the following technical challenges: 1) Insufficient ability to decompose the beryllium-containing phases in beryllium glass, with beryllium leaching rates typically below 85%, resulting in low resource utilization. 2) Traditional enhanced leaching methods cannot simultaneously improve the extraction of valuable elements and suppress impurities; the leaching rates of iron and aluminum increase synchronously with the extraction of valuable elements, leading to higher Fe²⁺ levels in the leachate. + / Fe³ + Al³ +Excessive concentration leads to the need for large amounts of alkaline solution for subsequent neutralization and impurity removal, and easily generates colloidal hydroxides, making solid-liquid separation difficult; 3) High consumption of acid / alkali reagents, cumbersome subsequent impurity removal processes, and high loss rate of valuable metals result in high overall production costs, making it difficult to meet the needs of industrial-scale applications; 4) Excessive use of acid / alkali can easily increase the wastewater treatment load, which is not in line with the development trend of green metallurgy. Based on the above problems, the process of using CO2 pressure leaching for wet treatment of beryllium glass in this invention includes the following three stages: 1) Initial stage of reaction: CO2 provides a pressurized atmosphere, enhances mass transfer, and assists strong acid in rapidly destroying the loose structure of beryllium glass, efficiently releasing valuable elements such as beryllium; 2) Mid-stage of reaction: A large amount of acid-consuming components (Al, Ca, etc.) in the system consume strong acid, and the acidity decreases. At this time, the carbonate / bicarbonate buffer system formed by CO2 dissolution dynamically regulates the pH: when the acidity is high, H+ accumulates. + When the acidity is low, H2 is released. + Maintaining a suitable leaching environment ensures the continuous and stable dissolution of valuable elements; 3) Later stage of the reaction: Fe and Al hydrolyze to release H + This leads to a rise in acidity, allowing the CO2 buffer system to precisely control the pH again, promoting the full hydrolysis and precipitation of Fe and Al, resulting in a lower impurity leaching rate. Furthermore, this invention discovers a weak complexing effect between bicarbonate and beryllium. In existing technologies, it is conventionally believed that the precipitation ranges of Fe, Al, and Be highly overlap, and impurity removal inevitably results in beryllium loss; however, this invention reveals a weak complexing effect between bicarbonate and beryllium. While Fe and Al precipitate efficiently, beryllium can be partially retained in the solution, significantly reducing beryllium loss and achieving a selective effect of high beryllium leaching and low Fe / Al leaching.

[0028] In the specific implementation process, the heating process in step two is divided into two stages. The purpose is to ensure that the entire reactor is in a CO2 atmosphere, avoid air interference, prevent water from boiling and escaping, and stabilize the liquid-solid ratio. It is not a step-by-step pressurization or segmented leaching. Specifically, below the first set temperature: the reactor body is connected to the atmosphere, and CO2 is continuously introduced to completely remove the air inside the reactor through gas displacement, ensuring that the system is in a CO2 atmosphere throughout the process and avoiding oxidation or impurity interference; when approaching the first set temperature: the reactor is sealed and pressurized, and CO2 continues to be introduced. If atmospheric pressure is maintained, the water will boil and water vapor will escape, leading to an uncontrolled liquid-solid ratio and affecting leaching stability and test repeatability. Therefore, it is necessary to pressurize in a sealed environment; after pressurization in a sealed environment: CO2 is continuously introduced to gradually increase the pressure inside the reactor to the set range, and heating and ventilation are carried out simultaneously; after reaching the set temperature, if the pressure is insufficient, CO2 is added to maintain a stable CO2 partial pressure. In other words, the entire CO2 pressurized leaching process is a single, continuous CO2 pressurized leaching process: the whole process involves one reactor, one feeding, and one heating and pressurization, without segmentation, pressure relief, material discharge, or secondary heating and pressurization. Essentially, it is a one-stage CO2 pressurized leaching process.

[0029] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. Solid-liquid separation is then performed on the reaction slurry to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue. Specifically, after the leaching reaction, heating is stopped, and the mixture is allowed to cool naturally to room temperature. The pressure is then slowly released to atmospheric pressure (pressure release rate ≤ 0.1 MPa / min to prevent bumping of the slurry). A vacuum filtration device is used for solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue, respectively. The beryllium-rich leachate is then subjected to conventional purification, extraction, back-extraction, and crystallization treatments to obtain a high-purity beryllium product. The iron-aluminum-rich leaching residue can be used as a comprehensive iron-aluminum raw material, achieving full resource recovery. This invention utilizes a CO2 pressurized buffer system for beryllium glass leaching, leveraging its dynamic pH regulation, enhanced mass transfer, and weak complexation assistance to solve the problem of simultaneous leaching of valuable materials and impurities in traditional strong acid leaching.

[0030] In one specific embodiment, in step one, the strong acid leaching aid is sulfuric acid and / or hydrochloric acid.

[0031] In one specific embodiment, in step one, the acid-to-ore ratio is controlled at 1100~1200 kg / t, and the liquid-to-solid ratio is (15~20):1. It should be noted that when the liquid-to-solid ratio is low, the acid-to-ore ratio should also be low; otherwise, the slurry viscosity will increase rapidly, affecting the smooth progress of the reaction. When the liquid-to-solid ratio is high, the acid content can be appropriately increased to ensure the dissociation effect. In the specific implementation process, the initial pH does not need to be limited.

[0032] In one specific embodiment, in step one, the stirring rate of the slurry treatment is 600~800 rpm.

[0033] In one specific embodiment, in step two, the pH of the leaching endpoint is 1.2 to 1.8. It should be noted that when the endpoint pH is below 1.2, the leaching rate of iron and aluminum impurities increases sharply, disrupting the selective separation effect; when the endpoint pH is above 1.8, the beryllium complex leaching rate decreases significantly, and valuable metals are at risk of hydrolysis loss.

[0034] In one specific embodiment, in step two, the CO2 gas is industrial waste gas. Industrial waste gas refers to CO2-containing exhaust gases emitted during industrial production processes, including but not limited to waste gas from iron and steel smelting, flue gas from thermal power plants, cement kiln exhaust gas, and chemical plant exhaust gas. Using industrial waste gas to replace pure CO2 gas can significantly reduce raw material costs while simultaneously achieving industrial carbon emission reduction and resource utilization. Alternatively, a mixture of industrial waste gas and pure CO2 can be used as the gas source, with the mixing ratio flexibly adjusted according to the actual CO2 concentration of the industrial waste gas, thus reducing the amount of pure CO2 used while ensuring the stability of the leaching effect.

[0035] In one specific embodiment, the high-pressure reactor is either a continuous high-pressure reactor or a batch high-pressure reactor. A continuous high-pressure reactor refers to a reaction device that allows for continuous material feeding and discharging, enabling uninterrupted leaching operations under pressure. Replacing a batch high-pressure reactor with a continuous high-pressure reactor allows for the industrial-scale continuous production of beryllium glass CO2 pressurized leaching, significantly improving processing efficiency and capacity. Through a multi-stage reaction chamber series design, the continuous high-pressure reactor allows the slurry to sequentially undergo stages such as heating, pressurized leaching, and heat preservation in different reaction chambers, achieving gradient management of reaction conditions and optimizing the leaching kinetics. Simultaneously, continuous operation avoids the frequent loading and unloading and heating / cooling energy consumption of batch reactors, reducing energy consumption and labor costs per unit product, making it more suitable for large-scale industrial applications. In specific implementations, batch high-pressure reactors can also be used for batch leaching operations, suitable for small-scale production or experimental research stages. It should be noted that the high-pressure reactor can be extended to a closed reactor, and can be a high-pressure reactor, tubular pressurized reaction equipment, continuous pressurized leaching device, stirred pressure-resistant reaction tank, or other pressurized reaction equipment. No specific limitations are made here.

[0036] In one specific embodiment, prior to step one, a pretreatment step is included: ball milling the beryllium glass to be processed to a particle size of ≥85% (120 mesh). It should be noted that the specific implementation also includes a pretreatment step of crushing and ball milling the beryllium glass to be processed. This pretreatment step aims to reduce the particle size of the beryllium glass, increase its specific surface area, and reduce mass transfer resistance during leaching, thereby enhancing the leaching kinetics of valuable elements. In the specific implementation, after the leaching reaction, the beryllium leaching rate is ≥97%, and the aluminum leaching rate is ≤30%. In other words, directly feeding blocky beryllium glass into the stirred reaction equipment has significant industrial defects; the material is difficult to suspend uniformly, effective stirring cannot be achieved, the stirring paddle is easily worn and broken, and pipeline blockage is easily caused, seriously affecting the continuous and stable operation of the equipment. In industrial practice, beryllium glass must be crushed and ball-milled before being sent to the leaching process. In a control case of pressurized leaching with only air and no CO2, using the same process conditions (e.g., temperature 150°C, liquid-to-solid ratio 20:1, reaction time 1 hour), the beryllium leaching rate was only 65%. Even when the temperature was increased to 180°C, the highest beryllium leaching rate was still less than 95%. Meanwhile, the aluminum leaching rate in this air system consistently exceeded 38%, and at 150°C, it even exceeded 50%. The extraction efficiency of valuable metals was low, and the impurity separation effect was poor, resulting in overall leaching performance significantly inferior to the CO2-coordinated pressurized leaching process of this invention.

[0037] Example 1

[0038] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al.

[0039] Processing procedure: Step 1: Pretreatment. The beryllium glass to be treated is fed into a jaw crusher for coarse crushing to the required particle size. The coarsely crushed material is then fed into a ball mill for fine grinding. After ball milling, the material is sieved through a vibrating screen, with 90% of the material passing through a 120-mesh standard sieve (0.125mm aperture) by mass. The pretreated beryllium glass, sulfuric acid, and water are mixed and placed in an autoclave for slurry treatment. The acid-to-ore ratio is controlled at 1150 kg / t, and the liquid-to-solid ratio at 20:1. The stirring speed during slurry treatment is 700 rpm.

[0040] Step 2: Heat the autoclave and introduce CO2 gas to bring the pressure inside the autoclave to 2.0 MPa and the temperature to 180 °C, and carry out the leaching reaction for 1 hour. The pH at the end of the leaching reaction is 1.2.

[0041] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0042] Treatment results: After the leaching reaction was completed, the leachate rich in beryllium and the leaching residue rich in iron and aluminum were tested. The results showed that the leaching rate of Be was 96.19%; the leaching rate of Fe was 97.83%; and the leaching rate of Al was 21.10%.

[0043] Example 2

[0044] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al.

[0045] Processing procedure: Step 1: Pretreatment. The beryllium glass to be treated is fed into a jaw crusher for coarse crushing to the required particle size. The coarsely crushed material is then fed into a ball mill for fine grinding. After ball milling, the material is sieved through a vibrating screen, with 90% of the material passing through a 120-mesh standard sieve (0.125mm aperture) by mass. The pretreated beryllium glass, sulfuric acid, and water are mixed and placed in an autoclave for slurry treatment. The acid-to-ore ratio is controlled at 1100 kg / t, and the liquid-to-solid ratio at 15:1. The stirring speed during slurry treatment is 600 rpm.

[0046] Step 2: First, CO2 gas is introduced into the autoclave to displace the air inside, and the temperature is raised to the first set temperature. The exhaust valve is then closed. The first set temperature is 100°C. CO2 gas is then continued to be introduced into the autoclave, and the pressure inside is adjusted to 1.5 MPa. The temperature is raised to 160°C, and the leaching reaction is carried out under constant temperature and pressure for 2 hours. The pH at the leaching endpoint is 1.6.

[0047] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0048] Treatment results: After the leaching reaction was completed, the leachate rich in beryllium and the leaching residue rich in iron and aluminum were tested. The results showed that the leaching rate of Be was 97.28%; the leaching rate of Fe was 88.83%; and the leaching rate of Al was 19.52%.

[0049] Example 3

[0050] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al.

[0051] Processing procedure: Step 1: Pretreatment. The beryllium glass to be treated is fed into a jaw crusher for coarse crushing to the required particle size. The coarsely crushed material is then fed into a ball mill for fine grinding. After ball milling, the material is sieved through a vibrating screen, with 85% of the material passing through a 120-mesh standard sieve (0.125mm aperture) by mass. The pretreated beryllium glass, hydrochloric acid, and water are mixed and placed in an autoclave for slurry treatment. The acid-to-ore ratio is controlled at 1200 kg / t, and the liquid-to-solid ratio at 18:1. The stirring speed during slurry treatment is 800 rpm. The autoclave is a continuous high-pressure reactor.

[0052] Step 2: First, CO2 gas is introduced into the autoclave to displace the air inside, and the temperature is raised to the first set temperature. The exhaust valve is then closed. The first set temperature is 95°C. CO2 gas is then continued to be introduced into the autoclave, and the pressure inside is adjusted to 0.5 MPa. The temperature is raised to 150°C, and the leaching reaction is carried out under constant temperature and pressure for 4 hours. The industrial waste gas is selected from blast furnace gas or converter flue gas from a steel plant. After dust removal and dehydration pretreatment, the CO2 volume concentration is 85%~95%, and it is directly introduced into the autoclave to participate in the leaching reaction. The pH at the leaching endpoint is 1.8.

[0053] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0054] Treatment results: After the leaching reaction was completed, the beryllium-rich leachate and the iron-aluminum-rich leaching residue were tested. The results showed that the Be leaching rate was 97.21%; the Fe leaching rate was 88.08%; and the Al leaching rate was 17.17%.

[0055] Comparative Example 1

[0056] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al. After ball milling, 90% of the material mass passes through a 120-mesh standard sieve (0.125mm aperture).

[0057] Step 1: Mix the pretreated beryllium glass, sulfuric acid, and water, and place the mixture in an autoclave for slurry processing. The acid-to-ore ratio is controlled at 1100 kg / t, and the liquid-to-solid ratio at 15:1. The stirring rate during slurry processing is 600 rpm.

[0058] Step 2: Heat the autoclave to 160°C; carry out the leaching reaction for 2 hours.

[0059] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0060] Treatment results: After the leaching reaction was completed, the beryllium-rich leachate and the iron-aluminum-rich leaching residue were tested. The results showed that the Be leaching rate was 99.67%; the Fe leaching rate was 100%; and the Al leaching rate was 100%.

[0061] Comparative Example 2

[0062] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al. After ball milling, 90% of the material mass passes through a 120-mesh standard sieve (0.125mm aperture).

[0063] Step 1: Mix the pretreated beryllium glass, sulfuric acid, and water, and place the mixture in an autoclave for slurry processing. The acid-to-ore ratio is controlled at 1100 kg / t, and the liquid-to-solid ratio at 15:1. The stirring rate during slurry processing is 600 rpm.

[0064] Step 2: First, introduce CO2 gas into the autoclave at a flow rate of 200 mL / min to replace the air inside the autoclave, and then heat the autoclave to a first set temperature; wherein, the first set temperature is 100℃; the pressure inside the autoclave is atmospheric pressure, and the leaching reaction is carried out under constant temperature and pressure at 160℃ for 2 hours. The pH at the endpoint of the leaching reaction is 1.6.

[0065] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0066] Treatment results: After the leaching reaction was completed, the leachate rich in beryllium and the leaching residue rich in iron and aluminum were tested. The results showed that the leaching rate of Be was 99.39%; the leaching rate of Fe was 100%; and the leaching rate of Al was 100%.

[0067] Comparative Example 3

[0068] Raw material to be processed: beryllium glass containing 2.14% Be, 0.46% Fe, and 6.16% Al. After ball milling, 90% of the material mass passes through a 120-mesh standard sieve (0.125mm aperture).

[0069] Step 1: Mix the pretreated beryllium glass, sulfuric acid, and water, and place the mixture in an autoclave for slurry processing. The acid-to-ore ratio is controlled at 1100 kg / t, and the liquid-to-solid ratio at 15:1. The stirring rate during slurry processing is 600 rpm.

[0070] Step 2: Heat the autoclave to 160℃ and adjust the pressure inside the autoclave to 1.5 MPa; carry out the leaching reaction for 2 hours.

[0071] Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

[0072] Treatment results: After the leaching reaction was completed, the leachate rich in beryllium and the leaching residue rich in iron and aluminum were tested. The results showed that the leaching rate of Be was 65.16%; the leaching rate of Fe was 66.89%; and the leaching rate of Al was 58.01%.

[0073] As can be seen from the observations of Examples 1-3 and Comparative Examples 1-3, the wet processing method for aluminum-inhibiting and enhanced leaching of beryllium glass of the present invention achieves the following dual technical effects by introducing CO2 pressurization conditions into the beryllium glass leaching system and constructing a pH-controllable carbonate / bicarbonate buffer system: On the one hand, the continuous pressurization of CO2 maintains a high concentration of dissolved CO2 in the liquid phase, making the local acid-base environment more stable and reducing the drastic local pH fluctuations at the solid-liquid interface caused by the rapid dissolution of minerals. Simultaneously, the CO2 dissolved in the liquid phase forms a carbonate system, which may react with the leached Be... 2+ Formation of weak coordination or weak complexation reduces the amount of free Be in the solution. 2+ The activity of CO2 increases, thereby promoting further dissolution of beryllium glass and improving the beryllium leaching rate to ≥97%. On the other hand, CO2 has increased solubility under pressure, making it easier to enter the cracks in beryllium glass and precipitate rapidly after cooling. This increases the specific surface area of ​​the internal cracks in the beryllium glass, leading to faster diffusion and the smaller diameter of the Be ions. 2+ Leaching is increased, while Al 3+Due to diffusion control, the improvement is limited, and under high temperature and high pressure conditions, even dissolved Al... 3+ There is also a significant hydrolysis trend, resulting in suppressed leaching on a macroscopic scale, with an aluminum leaching rate of ≤30%, a reduction of over 60% compared to traditional processes (100% Al leaching rate), thus significantly reducing the introduction of impurities at the source. Based on the above selective separation effect, this invention has the following outstanding advantages over existing technologies: Due to the significant reduction in impurity content in the leachate, the consumption of alkali in subsequent neutralization and impurity removal processes is reduced by over 60%, the difficulty of solid-liquid separation is significantly reduced, the process flow is shortened by 30%, and the overall production cost is reduced by 25%~35%; simultaneously, the use of CO2 to construct a buffer system reduces the amount of strong acids and alkalis used, reducing wastewater discharge by 40%; furthermore, industrial waste gas can be directly used as a CO2 source to achieve carbon capture and resource utilization, meeting the "dual carbon" target requirements. This invention is not only applicable to beryllium glass but can also be extended to the leaching treatment of various pyrometallurgical products such as copper, cobalt, and beryllium. The process parameters are controllable and easy to scale up industrially.

[0074] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be embraced within the present invention. No reference numerals in the appended diagrams should be construed as limiting the scope of the claims. Furthermore, it is clear that the word "comprising" does not exclude other elements or steps, and the singular does not exclude the plural.

[0075] However, those skilled in the art should understand that various modifications can be made to the wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass proposed in this invention without departing from the scope of this invention. Therefore, the scope of protection of this invention should be determined by the content of the appended claims.

Claims

1. A wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass, characterized in that, Includes the following steps: Step 1: Mix the beryllium glass to be treated, strong acid leaching agent and water, and place it in an autoclave for pulping treatment; Step 2: Heat the autoclave and introduce CO2 gas to bring the autoclave to the preset leaching temperature and preset leaching pressure, and carry out the leaching reaction. Step 3: After the leaching reaction is completed, the autoclave is cooled and depressurized to atmospheric pressure. The reaction slurry is then subjected to solid-liquid separation to obtain a beryllium-rich leachate and an iron-aluminum-rich leaching residue.

2. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step two, CO2 gas is first introduced into the autoclave to replace the air inside the autoclave, and the temperature is raised to a first set temperature before the exhaust valve is closed; wherein, the first set temperature is 95-100℃. Continue to introduce CO2 gas into the high-pressure reactor, adjust the pressure inside the reactor to 0.5~2.0 MPa, raise the temperature to 150~180℃, and carry out the leaching reaction under constant temperature and pressure for 1~4 hours.

3. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step one, the strong acid leaching aid is sulfuric acid and / or hydrochloric acid.

4. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step one, the acid-to-ore ratio is controlled at 1100-1200 kg / t, and the liquid-to-solid ratio is (15-20):

1.

5. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step one, the stirring rate for the slurry treatment is 600-800 rpm.

6. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step two, the pH at the leaching endpoint of the leaching reaction is 1.2 to 1.

8.

7. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, In step two, the CO2 gas is industrial waste gas.

8. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, The high-pressure reactor is either a continuous high-pressure reactor or an intermittent high-pressure reactor.

9. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, Before step one, a pretreatment step is also included: ball milling the beryllium glass to be treated so that the proportion of material on the 120-mesh sieve is ≥85%.

10. The wet processing method for aluminum-inhibiting and strengthening leaching of beryllium glass according to claim 1, characterized in that, After the leaching reaction is completed, the beryllium leaching rate is ≥97% and the aluminum leaching rate is ≤30%.