A method for efficient recovery of copper based on hyperaccumulator sedum plumbizincicola
By preparing materials such as straw ash, pyrolytic char, and hydrothermal char, the problems of heavy metal disposal and resource recovery after hyperaccumulating phytoremediation have been solved, achieving efficient copper recovery and wastewater treatment, and forming a closed-loop system of pollution control and resource recycling.
Patent Information
- Application Number
- CN202611439394.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, heavy metal disposal after hyperaccumulating phytoremediation is difficult, and valuable metals cannot be effectively recovered, resulting in resource waste and environmental risks, making it difficult to achieve a closed loop of pollution control and resource recycling.
By heat-treating and hyper-enriching Sedum sarmentosum stalks (a plant-based mineral byproduct), straw ash, pyrolytic char, and hydrothermal char are prepared. Combined with acid dissolution precipitation and displacement reactions, this achieves efficient copper recovery and the preparation of wastewater treatment materials, forming a closed-loop system.
High-performance carbon materials were prepared, enabling the safe disposal and resource utilization of heavy metals, improving the sustainability of environmental governance and the efficiency of resource utilization, and bridging the "last mile" of phytoremediation technology.
Smart Images

Figure CN123152889A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hazardous waste disposal and resource utilization technology, and in particular to a method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant associated with minerals. Background Technology
[0002] Using hyperaccumulating plants to remove heavy metals from soil is a green and low-cost ecological restoration method. However, a key challenge remains in the practical application of this technology: the harvested plants after restoration contain large amounts of heavy metals, and the appropriate method for disposing of this biomass is crucial. Traditional landfilling or indiscriminate disposal methods can easily lead to the re-release of heavy metals, causing pollutants to spread to the surrounding environment and rendering the previous remediation efforts futile.
[0003] The safe disposal and resource utilization of hyperaccumulating plants is a core challenge hindering the widespread adoption of phytoremediation technologies. Current mainstream methods (such as pyrolysis carbonization) focus on passivating copper (Cu) within a carbon matrix. While this reduces environmental risks and achieves carbon sequestration, it neglects the recovery value of Cu as a valuable metal, resulting in resource waste. Furthermore, existing preparation techniques fail to effectively couple material structure optimization with functional enhancement, leading to insufficient treatment performance of the resulting carbon materials for Cu-containing wastewater. This hinders the targeted transformation and value leap from "polluting plants" to "high-efficiency wastewater treatment materials."
[0004] Therefore, there is an urgent need to develop an integrated resource utilization technology that can, on the one hand, solve the disposal dilemma of hyperaccumulating plants, and on the other hand, transform their residual carbon into high-performance materials that can be used to treat Cu-containing wastewater, while simultaneously recovering valuable metallic Cu. This is of great practical significance and important application prospects for bridging the "last mile" of phytoremediation technology and forming a complete closed loop of pollution control and resource recycling. Summary of the Invention
[0005] The present invention aims to provide a resource recovery method for wastewater treatment and valuable metal recovery based on hyperaccumulating plants, so as to realize the subsequent disposal and resource utilization of heavy metal phytoremediation.
[0006] This invention provides a method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant associated with minerals, characterized by the following steps:
[0007] S1: Material preparation, the super-enriched copper plant-associated mineral Sedum straw is heat-treated to prepare straw ash, pyrolytic char and hydrothermal char.
[0008] S2: Wastewater treatment. The material prepared in S1 is put into copper-containing wastewater, shaken, and allowed to stand. Then the treated water is filtered out, and the adsorbed material is collected.
[0009] S3: Ashing. Grind the material collected in S2 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash.
[0010] S4: Acid dissolution precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is added to displace copper.
[0011] S5: Collection and drying. The sponge copper displaced in S4 is filtered, collected, and dried. The copper recovery content under the three methods is compared, and the superior materials - straw ash and pyrolysis char - are selected.
[0012] S6: Preparation and fixation. According to the path selected in S5, the super-enriched copper plant-associated mineral Sedum straw and sodium hydroxide or calcium hydroxide solid are mixed and heat-treated to prepare straw ash and pyrolytic carbon.
[0013] S7: Wastewater treatment. The material prepared in S6 is added to copper-containing wastewater, shaken, and allowed to stand. The treated water is then filtered out, and the adsorbed material is collected.
[0014] S8: Ashing and fixing. Grind the material collected in S7 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash.
[0015] S9: Acid dissolution and precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is obtained. Excess iron filings with a coefficient of 2.0 are added to displace copper. The filtrate is collected and dried.
[0016] Furthermore, in step S1, the pyrolytic carbon preparation temperature is 400℃, and the hydrothermal carbon preparation temperature is 200℃.
[0017] Furthermore, in step S3, the muffle furnace ashing temperature is 700°C.
[0018] Furthermore, in step S4, the sulfuric acid solution is 0-20%, the solid-liquid ratio is 10-1, the leaching time is 40-80 min, and the iron filings used to replace copper are 1.5-2 times the theoretical reaction amount.
[0019] Furthermore, in step S6, the amount of sodium hydroxide or calcium hydroxide added is 0%-10%.
[0020] The beneficial effects of this invention are
[0021] 1. Preparation of high-performance multifunctional carbon materials: The prepared carbon materials have abundant pore structure, high specific surface area and specific surface functional groups, and have excellent adsorption performance for heavy metal ions in wastewater, realizing the upgrade of material function.
[0022] 2. An innovative recycling pathway for valuable metals: Through specific thermochemical conversion and subsequent separation processes, valuable metals such as Cu can be extracted efficiently and selectively from hyperaccumulating plants, significantly improving the economic efficiency of resource recycling compared to simple solidification treatment.
[0023] 3. This design bridges the "last mile" of phytoremediation technology, constructing a closed-loop system integrating "waste resource utilization, wastewater purification, and metal recycling." By converting waste biomass into wastewater treatment materials, it simultaneously achieves safe disposal, pollution control, and metal recycling, significantly improving the sustainability of environmental governance and the efficiency of resource utilization. Attached Figure Description
[0024] Figure 1 This is a flowchart of a method for efficient Cu recovery based on Sedum aizoon, a super-enriched plant associated with minerals, according to the present invention.
[0025] Figure 2 Cu loss during the preparation of straw ash, pyrolytic char, and hydrothermal char
[0026] Figure 3 The adsorption capacity of Cu in wastewater by straw ash, pyrolytic char, and hydrothermal char.
[0027] Figure 4 The Cu content of straw ash, pyrolytic charcoal and hydrothermal charcoal after ashing
[0028] Figure 5 The copper content of sponge was recovered after ashing three materials: straw ash, pyrolysis charcoal, and hydrothermal charcoal.
[0029] Figure 6 The retention effect of adding different proportions of NaOH and Ca(OH)2 in the preparation of straw ash and pyrolysis char.
[0030] Figure 7 The modified straw ash and pyrolysis char adsorbed Cu in wastewater
[0031] Figure 8 The Cu fixation rate during the ashing process of straw ash and biochar
[0032] Figure 9 Sponge copper recovery from straw ash and pyrolytic carbon pathways Detailed Implementation
[0033] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.
[0034] Please see Figure 1 The embodiments of the present invention include:
[0035] S1: Material preparation, the super-enriched copper plant-associated mineral Sedum straw is heat-treated to prepare straw ash, pyrolytic char and hydrothermal char.
[0036] S2: Wastewater treatment. The material prepared in S1 is put into copper-containing wastewater, shaken, and allowed to stand. Then the treated water is filtered out, and the adsorbed material is collected.
[0037] S3: Ashing. Grind the material collected in S2 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash.
[0038] S4: Acid dissolution precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is added to displace copper.
[0039] S5: Collection and drying. The sponge copper displaced in S4 is filtered, collected, and dried. The copper recovery content under the three methods is compared, and the superior materials - straw ash and pyrolysis char - are selected.
[0040] S6: Preparation and fixation. According to the path selected in S5, the super-enriched copper plant-associated mineral Sedum straw and sodium hydroxide or calcium hydroxide solid are mixed and heat-treated to prepare straw ash and pyrolytic carbon.
[0041] S7: Wastewater treatment. The material prepared in S6 is added to copper-containing wastewater, shaken, and allowed to stand. The treated water is then filtered out, and the adsorbed material is collected.
[0042] S8: Ashing and fixing. Grind the material collected in S7 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash.
[0043] S9: Acid dissolution and precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is obtained. Excess iron filings with a coefficient of 2.0 are added to displace copper. The filtrate is collected and dried.
[0044] Furthermore, in step S1, the pyrolytic carbon preparation temperature is 400℃, and the hydrothermal carbon preparation temperature is 200℃.
[0045] Furthermore, in step S3, the muffle furnace ashing temperature is 700°C.
[0046] Furthermore, in step S4, the sulfuric acid solution is 0-20%, the solid-liquid ratio is 10-1, the leaching time is 40-80 min, and the iron filings used to replace copper are 1.5-2 times the theoretical reaction amount.
[0047] Furthermore, in step S6, the amount of sodium hydroxide or calcium hydroxide added is 0%-10%.
[0048] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] The specific steps of the method described in this invention will be illustrated below with specific embodiments.
[0050] Example 1: A resource recovery method for wastewater treatment and valuable metal recovery by producing straw ash, pyrolytic charcoal and hydrothermal charcoal from hyperaccumulating plants-associated mineral Sedum.
[0051] Material preparation: The yields of straw ash, pyrolytic char, and hydrothermal char were 18.16%, 38.85%, and 60.25%, respectively, with hydrothermal char showing the highest yield, being 1.55 times and 3.32 times that of pyrolytic char and straw ash, respectively. Different preparation temperatures also led to significant differences in Cu loss during different treatment processes. Figure 2 The results showed that the Cu content of straw ash, pyrolytic char, and hydrothermal char decreased by 61.8%, 41.8%, and 3.5%, respectively, during the preparation process.
[0052] Adsorption: Figure 3 The adsorption capacities of straw ash, pyrolytic char, and hydrothermal char were shown to be 247.69 mg / g, 170.53 mg / g, and 5.64 mg / g, respectively.
[0053] Ashing: The ashing yields of straw ash, pyrolytic charcoal, and hydrothermal charcoal at 700℃ were 77.91%, 58.71%, and 64.5%, respectively. Figure 4 The results show the Cu content of straw ash after ashing of the three solid substances after saturated adsorption. The Cu content of pyrolytic carbon is 263.02 g / kg, the lowest Cu content of hydrothermal carbon is 19.48 g / kg, and the highest Cu content of straw ash is 271.16 g / kg, which is 1.03 and 13.92 times that of pyrolytic carbon and hydrothermal carbon, respectively.
[0054] Recycle: Figure 5 The results showed that after saturated adsorption, 1g of ashed straw ash yielded the highest Cu recovery content of 203.19 mg, which was 1.03 times and 14.97 times that of pyrolytic char and hydrothermal char, respectively. Pyrolytic char yielded the lowest Cu recovery content of 196.80 mg, while hydrothermal char yielded the lowest at 13.57 mg. Therefore, straw ash and pyrolytic char were ultimately selected for further optimization, and the optimal route will be determined later.
[0055] Example 2: A resource utilization method for wastewater treatment and valuable metal recovery by producing straw ash and pyrolytic char from hyperaccumulating plants-associated mineral Sedum.
[0056] Material preparation: Figure 6 The study demonstrated the effects of adding 1%-10% calcium hydroxide (Ca1-10) and sodium hydroxide (Na1-10) on Cu retention during the preparation of straw ash and pyrolysis char. The results showed that adding calcium hydroxide had no significant effect on Cu retention in straw ash; the retention effects of adding 1% and 5% calcium hydroxide were lower than those of the untreated group. However, the Cu retention effect of the sodium hydroxide treatment group significantly improved with increasing dosage. When 5% sodium hydroxide was added, the Cu fixation rate increased by 19.29%, indicating that 5% reached the optimal balance among the various mechanisms. In the pyrolysis char preparation process, both calcium hydroxide and sodium hydroxide improved Cu retention. The retention effect of sodium hydroxide increased significantly with increasing dosage, but the retention effect of calcium hydroxide decreased with increasing dosage. Adding 1% calcium hydroxide increased the Cu fixation rate by 9.31%, a retention effect similar to that of adding 5% and 10% sodium hydroxide. In conclusion, it was ultimately determined that 1% calcium hydroxide should be added during the preparation of pyrolytic carbon.
[0057] Wastewater treatment: Figure 7 The adsorption capacity of straw ash (NaOH-H) and pyrolytic char (Ca(OH)2-C) for Cu was demonstrated. The adsorption capacity increased significantly with increasing initial concentration, reaching almost the maximum at 1400 mg / L. Further increases in initial concentration did not significantly change the adsorption capacity, with a saturation adsorption capacity of 413.86 mg / g, an increase of 1.71 times. The Cu adsorption capacity of Ca(OH)2-C also increased significantly with increasing initial concentration, reaching almost the maximum at 1200 mg / L. Further increases in initial concentration did not significantly change the adsorption capacity, with a saturation adsorption capacity of 279.33 mg / g, an increase of 1.94 times.
[0058] Ashing: Figure 8 The study demonstrates the Cu fixation rates of straw ash and biochar during the ashing process. The Cu fixation rate of straw ash reached 86.85%, while that of biochar was only 68.74%. After acid dissolution and precipitation, as shown in Table 1, 1g of ashed straw ash (NaOH-H) yielded a Cu recovery of 344.49 mg, corresponding to a total recoverable Cu content of 66.21 g from 1kg of straw ash prepared with Sedum aizoon. Similarly, 1g of ashed pyrolytic char (Ca(OH)2-C) yielded a Cu recovery of 303.25 mg, corresponding to a total recoverable Cu content of 51.21 g from 1kg of pyrolytic char prepared with Sedum aizoon.
[0059] In conclusion, the optimal approach is to process Sedum sarmentosum, a by-product of mineralization, into straw ash for Cu recovery, thereby achieving waste treatment and resource recycling.
[0060] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0061] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant associated with minerals, characterized in that, Includes the following steps: S1: Material preparation, the super-enriched copper plant-associated mineral Sedum straw is heat-treated to prepare straw ash, pyrolytic char and hydrothermal char. S2: Wastewater treatment. The material prepared in S1 is put into copper-containing wastewater, shaken, and allowed to stand. Then the treated water is filtered out, and the adsorbed material is collected. S3: Ashing. Grind the material collected in S2 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash. S4: Acid dissolution precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is added to displace copper. S5: Collection and drying. The sponge copper displaced in S4 is filtered, collected, and dried. The copper recovery content under the three methods is compared, and the superior materials - straw ash and pyrolysis char - are selected. S6: Preparation and fixation. According to the path selected in S5, the super-enriched copper plant-associated mineral Sedum straw and sodium hydroxide or calcium hydroxide solid are mixed and heat-treated to prepare straw ash and pyrolytic carbon. S7: Wastewater treatment. The material prepared in S6 is added to copper-containing wastewater, shaken, and allowed to stand. The treated water is then filtered out, and the adsorbed material is collected. S8: Ashing and fixing. Grind the material collected in S7 and pass it through a 100-mesh sieve. Place it in a crucible and put it in a muffle furnace. Ash it at 700℃ for 3 hours and collect and store the ash. S9: Acid dissolution and precipitation. The ash collected in S3 is added to sulfuric acid solution for acid leaching reaction. After filtration, the filtrate is obtained. Excess iron filings with a coefficient of 2.0 are added to displace copper. The filtrate is collected and dried.
2. The method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant, according to claim 1, is characterized in that, In step S1, the pyrolytic carbon preparation temperature is 400℃, and the hydrothermal carbon preparation temperature is 200℃.
3. The method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant, according to claim 1, is characterized in that... In step S3, the muffle furnace ashing temperature is 700℃.
4. The method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant, according to claim 1, is characterized in that... In step S4, the sulfuric acid solution is 0-20%, the solid-liquid ratio is 10-1, the leaching time is 40-80 min, and the amount of iron filings used to replace copper is 1.5-2 times the theoretical reaction amount.
5. The method for efficient copper recovery based on Sedum aizoon, a hyperaccumulating plant, according to claim 1, is characterized in that... In step S6, the amount of sodium hydroxide or calcium hydroxide added is 0%-10%.