Low-chlorine high-activity light-burned return material-based magnesia neutralizer, and preparation method and application thereof
By using water washing and low-temperature calcination, the problems of high chlorine content and activity fluctuations in lightly calcined recycled materials were solved, and a low-chlorine, high-activity magnesium neutralizing agent was prepared. This agent was then applied to the precipitation process of nickel-cobalt solutions, achieving high-value utilization and stable precipitation of lightly calcined recycled materials.
Patent Information
- Application Number
- CN202611353102.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are unable to effectively address the high chlorine content and activity fluctuations in light-burned recycled materials, resulting in poor process adaptability in the wet precipitation process of nickel-cobalt solutions and making it difficult to achieve high-value utilization.
By washing and dechlorinating with water and calcining at medium and low temperatures, the chlorine content in the lightly calcined recycled material is reduced while maintaining its reactivity. This process produces a low-chlorine, high-activity magnesium-based neutralizing agent for use in the precipitation process of nickel-cobalt solutions.
It significantly reduces the chlorine content in light-burned recycled materials, increases the main MgO content, maintains excellent reactivity, reduces costs, and achieves high-value utilization and stable precipitation effect of light-burned recycled materials.
Smart Images

Figure CN123152893A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of industrial solid waste resource utilization and hydrometallurgical neutralization and precipitation technology, specifically to a low-chlorine, high-activity light-burned recycled magnesium neutralizing agent, its preparation method, and its application. Background Technology
[0002] In the industrial production process of preparing magnesium oxide from magnesium hydroxide by calcination, a large amount of recycled material and dust are generated, collectively referred to in the industry as light-calcined recycled material. This type of material contains a certain proportion of magnesium oxide and theoretically has value as a magnesium source for recycling; if it is directly disposed of as solid waste, it will not only waste magnesium resources, but also bring environmental pressure and disposal costs.
[0003] However, due to fluctuations in upstream production processes and material entrainment, lightly calcined recycled materials generally suffer from quality defects such as high chloride content (typically 1.0%–2.0%), large fluctuations in phase composition, and unstable MgO reactivity, resulting in poor process adaptability when used directly as industrial raw materials. Especially in wet precipitation systems containing nickel-cobalt solutions, soluble chloride salts in the material are easily introduced into the solid phase product during precipitation. Simultaneously, fluctuations in activity make it difficult to stably control the final pH and reaction rate, ultimately leading to unstable precipitation process operation and decreased purity of the nickel-cobalt product. Limited by these issues, this type of recycled material has long been unable to achieve high-value utilization in high-end hydrometallurgical applications.
[0004] Currently, industrial magnesium oxide, magnesium hydroxide, or lime are commonly used as neutralizing and precipitating agents in the neutralization and precipitation process of nickel-cobalt solutions. Industrial magnesium oxide offers stable reactivity and controllable precipitation effects, but its high raw material procurement cost significantly increases the operating costs of hydrometallurgy. Lime-based neutralizing agents are widely available and inexpensive, but they introduce large amounts of calcium impurities, affecting the quality of nickel-cobalt products and easily causing scaling in production system pipelines. Magnesium hydroxide systems have a mild reaction, but the reaction rate is slow, and precipitation selectivity is insufficient, making it difficult to balance nickel-cobalt recovery rate with slag grade. Overall, existing neutralizing agent systems have consistently failed to achieve a balance between cost control and precipitation performance stability.
[0005] Existing technologies have been used to study the preparation of metallurgical activated magnesium oxide. For example, Chinese patent CN110921688A discloses a method for preparing activated magnesium oxide, using lightly calcined magnesium powder as raw material. The method involves decalcification and phase inversion, ammonium chloride leaching, magnesium precipitation reaction, and high-temperature calcination to prepare high-purity activated magnesium oxide. The product can be used as a metallurgical precipitant for nickel and cobalt precipitation. However, this method uses virgin lightly calcined magnesium powder as raw material and relies on multiple reagents such as ammonium chloride and carbon dioxide. The process is lengthy and the reagent costs are high. Furthermore, the process design does not address the dechlorination needs of high-chlorine magnesium-containing solid waste and cannot handle industrial byproducts such as lightly calcined recycled materials.
[0006] In summary, there is currently a lack of a low-cost modification process for light-burned recycled materials. It is difficult to effectively remove chlorine impurities and increase the main MgO content while simultaneously controlling and retaining the material's reactivity to ensure its stable compatibility with the precipitation process containing nickel and cobalt solutions. Therefore, developing a simple and environmentally friendly method for the high-value modification of light-burned recycled materials, and preparing a low-chlorine, highly active magnesium neutralizing agent, is of significant practical importance for realizing solid waste resource utilization and reducing hydrometallurgical production costs. Summary of the Invention
[0007] Based on the aforementioned technical problems, this invention reduces the chloride content in lightly calcined recycled materials and increases the MgO content while maintaining the material's reactivity through water washing dechlorination and low-temperature calcination. The aim is to realize its application in nickel-cobalt solution precipitation, achieving high-value utilization of lightly calcined recycled materials. The objective is to provide a low-chlorine, high-activity magnesium-based neutralizing agent for lightly calcined recycled materials, its preparation method, and its application.
[0008] This invention protects a method for preparing a low-chlorine, highly active, lightly calcined recycled magnesium neutralizer, specifically comprising the following steps: Step 1, Raw material preparation: Take lightly calcined recycled material as raw material, wherein the mass content of MgO in the lightly calcined recycled material is 70% to 80%, the mass content of chlorine is 0.8% to 2.0%, and the citric acid activity is 40-70. Step 2, water washing and dechlorination: Mix the above lightly calcined return material with water in a certain proportion, and wash it with water under stirring conditions to dissolve the soluble chloride salts in the material into the liquid phase; Step 3, solid-liquid separation: After washing, solid-liquid separation is carried out by filtration to obtain the dechlorinated light calcined return filter cake. The filter cake is placed in a drying device and dried to constant weight. Step 4, low-temperature calcination: The dried filter cake is placed in a calcination device and calcined at 400-600℃. After calcination, it is naturally cooled to obtain a low-chlorine, high-activity light-calcined recycled magnesium neutralizer. The magnesium neutralizer has an MgO mass content ≥93%, a chlorine mass content ≤0.40%, and a citric acid activity value ≤31s.
[0009] Further, in step 1, the lightly burned return material is any one or a combination of two of the following: recycled return material generated during the calcination of magnesium hydroxide to prepare magnesium oxide, dust removal ash, or magnesium-containing return material.
[0010] Further, in step 2, the liquid-to-solid mass ratio of the water washing is (3-8):1, the stirring time is 10-60 min, the water washing temperature is room temperature, and the stirring speed is 100-300 rpm.
[0011] Furthermore, in step 3, the filter cake is dried at a temperature of 85–105°C until the moisture content of the material is ≤2%.
[0012] Furthermore, in step 4, the calcination time is 20–60 min, and the heating rate is 5–10 °C / min; the calcination equipment is any one of a muffle furnace, rotary kiln, or pusher kiln.
[0013] This invention also protects the low-chlorine, high-activity light-burned recycled magnesium neutralizer prepared by the above method.
[0014] This invention also protects the application of the low-chlorine, high-activity light-burned recycled magnesium neutralizer prepared by the above method in the precipitation of nickel-cobalt solutions. The magnesium neutralizer is added as a neutralizing precipitant to the nickel-cobalt solution, so that nickel and cobalt precipitate out in the form of precipitates.
[0015] Furthermore, in the application, the magnesium neutralizing agent is added to the nickel-cobalt solution using either a dry or wet method; wherein, the wet method slurry preparation time is 0.5 to 1.5 hours, and shortening the slurry preparation time helps to reduce MgO hydration loss.
[0016] Compared with existing technologies, the present invention has the following beneficial effects: 1. Significant dechlorination and quality improvement effects By washing away soluble chloride salts and combining this with low-temperature calcination to remove bound water and residual easily decomposable components, the chlorine content of the light-burned return material can be reduced from a minimum of 1.20% to 0.16%, and the MgO main content can be increased from a maximum of 73.37% to 97.95%, meeting the requirements for hydrometallurgical applications.
[0017] 2. Excellent activity retention and controllability By using medium-low temperature calcination at 400-600℃, the material quality is improved while avoiding MgO grain growth and activity decay caused by high-temperature over-calcination. The citric acid activity value of the product can be stabilized at 10-31s, maintaining excellent reactivity.
[0018] 3. Simple process and low cost Modification can be completed through only three core processes: washing, drying, and calcination. There is no need for complex wet purification and reagent addition. The equipment investment is low, the operating cost is low, and it is easy to scale up industrially.
[0019] 4. High-value utilization of solid waste Using the light-burned recycled material, a byproduct of magnesium oxide production, as raw material, low-value solid waste is transformed into a high-value metallurgical neutralizing agent. This not only solves the problem of solid waste disposal but also reduces the procurement cost of neutralizing agents for hydrometallurgical enterprises, achieving both environmental and economic benefits.
[0020] 5. Flexible application methods The resulting product is used for precipitation in nickel-cobalt solutions and is compatible with both dry powder addition and wet slurry preparation methods. The appropriate method can be flexibly selected based on site conditions. The nickel-cobalt precipitation effect is stable, and both the nickel-cobalt precipitation rate and slag grade meet industrial production requirements. Specifically, the highest nickel precipitation rate can reach 87.73% and the cobalt precipitation rate can reach 95.83% when using wet slurry preparation for nickel precipitation, with a consumption of 0.75 t / t. Attached Figure Description
[0021] Figure 1 This is a process flow diagram for the preparation and application of the low-chlorine, high-activity, lightly calcined recycled magnesium neutralizer of the present invention. Detailed Implementation
[0022] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0023] The preparation method of the present invention will be further described in detail below with reference to specific industrial embodiments.
[0024] In the following examples and comparative examples, the lightly calcined recycled material used was taken from the dust removal ash and circulating recycled material mixture of the magnesium hydroxide calcination production line of a magnesium oxide plant. The basic properties were: MgO mass content 73.37%, chlorine mass content 1.20%, and citric acid activity value 54'09 (i.e., 54 minutes and 09 seconds, the test standard is YB / T 4019-2006 "Method for Determination of Chemical Activity of Lightly Calcined Magnesium Oxide").
[0025] Performance testing methods: MgO content: EDTA complexometric titration; Chlorine content: ion chromatography; Activity: Citric acid value method (YB / T4019-2006), the smaller the value, the higher the activity; Metal ion concentration: Inductively coupled plasma optical emission spectrometry (ICP-OES).
[0026] In addition, unless otherwise specified, the raw materials used in the embodiments and comparative examples of this invention are all commercially available industrial-grade products in the art.
[0027] Example 1 illustrates the preparation method of the magnesium neutralizing agent of the present invention; Examples 2-3: Application of the magnesium neutralizer prepared in this invention (dry nickel plating); Example 4: Application of the magnesium neutralizer prepared in this invention (wet nickel plating); Examples 5-7: Application of the magnesium neutralizer prepared in this invention (wet nickel immersion, effect of slurry preparation time on magnesium neutralizer); Example 8: Comparison of dry nickel plating and wet nickel plating.
[0028] Example 1
[0029] A method for preparing a low-chlorine, high-activity, lightly calcined recycled magnesium-based neutralizing agent 1. Water washing and dechlorination Take lightly calcined recycled material and water and mix them at a liquid-solid mass ratio of 5:1. At room temperature, stir at a stirring speed of 260 for 30 minutes to dissolve the soluble chloride salts in the material into the liquid phase.
[0030] 2. Solid-liquid separation After washing, solid-liquid separation is performed by vacuum filtration to obtain dechlorinated lightly burned return filter cake. The filter cake is then placed in a drying device and dried to constant weight. The drying temperature of the filter cake is 100℃, and the material moisture content is dried to ≤2%.
[0031] 3. Low-temperature calcination The dried filter cake was placed in a muffle furnace and calcined at 400℃, 500℃ and 600℃ for 30 min, with a heating rate of 5℃ / min. After calcination, the cake was naturally cooled to obtain low-chlorine, high-activity light-calcined recycled magnesium neutralizing agents at different calcination temperatures.
[0032] After washing with water for 30 minutes, the sample showed a MgO content of 70.49%, an activity of 120'35, and a chlorine content that decreased to 0.41%.
[0033] The MgO content of the water-washed and calcined sample at -400℃ was 93.15%, the activity was 10'31, and the chlorine content was 0.37%; the MgO content of the water-washed and calcined sample at -500℃ was 97.56%, the activity was 27'12, and the chlorine content was 0.32%; the MgO content of the water-washed and calcined sample at -600℃ was 97.95%, the activity was 30'44, and the chlorine content decreased to 0.16% (see Table 1 for details).
[0034] Table 1. Treatment of lightly calcined recycled materials by water washing and calcination
[0035] The results showed that water washing can effectively reduce the chlorine content in the lightly calcined return material, and calcination at 400-600℃ after water washing can further increase the MgO content and achieve low chlorination treatment.
[0036] Example 2
[0037] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for dry nickel plating specifically includes the following steps: 1. Neutralizing agent preparation Weigh 1.255g of the low-chlorine, high-activity light-burned recycled magnesium neutralizer obtained by washing with water for 30min and calcining at 400℃ in Example 1. The amount added is 0.85 times the amount required for theoretical nickel-cobalt precipitation.
[0038] 2. Dry nickel plating Take 500 mL of nickel, cobalt, manganese and magnesium pre-nickel precipitation solution in a beaker, wherein the Ni concentration is 3.83 g / L, the Co concentration is 0.36 g / L, the Mn concentration is 2.5 g / L and the Mg concentration is 6.8 g / L; add the above neutralizing agent directly to the reaction system by dry powder addition, and stir continuously at 60 °C for 3 h.
[0039] 3. Solid-liquid separation After the reaction was completed, solid-liquid separation was performed, the filtrate and precipitate were collected, and the concentration of metal ions in the filtrate and the composition of the precipitate were detected respectively.
[0040] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 2. The calculated nickel precipitation rate was 77.77%, the cobalt precipitation rate was 98.76%, the nickel grade was 38.17%, and the unit consumption was 0.86 t / t.
[0041] Example 3
[0042] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for dry nickel plating specifically includes the following steps: 1. Neutralizing agent preparation Weigh 1.255g of the low-chlorine, high-activity light-burned recycled magnesium neutralizer obtained by washing with water for 30min and calcining at 600℃ in Example 1. The amount added is 0.85 times the amount required for theoretical nickel-cobalt precipitation.
[0043] 2. Dry nickel plating Take 500 mL of nickel, cobalt, manganese and magnesium pre-nickel precipitation solution in a beaker, wherein the Ni concentration is 3.83 g / L, the Co concentration is 0.36 g / L, the Mn concentration is 2.5 g / L and the Mg concentration is 6.8 g / L; add the above neutralizing agent directly to the reaction system by dry powder addition, and stir continuously at 60 °C for 3 h.
[0044] 3. Solid-liquid separation After the reaction was completed, solid-liquid separation was performed, the filtrate and precipitate were collected, and the concentration of metal ions in the filtrate and the composition of the precipitate were detected respectively.
[0045] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 2. The calculated nickel precipitation rate was 78.07%, the cobalt precipitation rate was 98.90%, the nickel grade was 36.98%, and the unit consumption was 0.85 t / t.
[0046] Table 2. Dry and wet nickel deposition results of the magnesium neutralizing agent of this invention.
[0047] Compared with Example 2, the chlorine content of the sample washed with water for 30 min and calcined at 600℃ in this example is lower, the nickel precipitation rate is basically the same, and the cobalt precipitation rate is slightly higher. This indicates that increasing the calcination temperature is beneficial to further reduce the chlorine content and maintain a good cobalt precipitation effect (see Table 2 for details).
[0048] Example 4
[0049] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for wet slurry preparation and nickel deposition specifically includes the following steps: 1. Neutralizing agent preparation Weigh 1.255g of the low-chlorine, high-activity light-burned recycled magnesium neutralizer obtained by washing with water for 30min and calcining at 500℃ in Example 1. The amount added is 0.85 times the amount required for theoretical nickel-cobalt precipitation.
[0050] 2. Neutralizing agent wet slurry preparation The above-mentioned neutralizing agent was mixed with water to form a slurry, and the slurry was adjusted at room temperature for 1.5 hours to obtain a lightly calcined return material-based magnesium neutralizing agent slurry.
[0051] 3. Wet nickel plating Take 500 mL of nickel, cobalt, manganese and magnesium pre-nickel precipitation solution in a beaker, wherein the Ni concentration is 3.83 g / L, the Co concentration is 0.36 g / L, the Mn concentration is 2.5 g / L and the Mg concentration is 6.8 g / L; add the above neutralizing agent directly to the reaction system by dry powder addition, heat in a water bath and maintain the reaction temperature at 60℃, add the slurry of magnesium neutralizing agent after slurry preparation to the reaction system, and continue stirring the reaction for 3 hours.
[0052] 3. Solid-liquid separation After the reaction was completed, solid-liquid separation was performed, the filtrate and precipitate were collected, and the concentration of metal ions in the filtrate and the composition of the precipitate were detected respectively.
[0053] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 2. The calculated nickel precipitation rate was 87.73%, the cobalt precipitation rate was 95.83%, the nickel grade was 35.91%, and the unit consumption was 0.75 t / t.
[0054] The results showed that when the low-chlorinated magnesium neutralizer obtained by calcining the lightly burned recycled material after washing with water for 30 min at 500℃ was added using a wet slurry preparation method, the nickel precipitation rate was significantly improved and the unit consumption was low, resulting in a better nickel precipitation application effect (see Table 2 for details).
[0055] Example 5
[0056] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for wet slurry preparation and nickel deposition specifically includes the following steps: 1. Neutralizing agent preparation Weigh 1.255g of the low-chlorine, high-activity light-burned recycled magnesium neutralizer obtained by washing with water for 30min and calcining at 400℃ in Example 1. The amount added is 0.85 times the amount required for theoretical nickel-cobalt precipitation.
[0057] 2. Neutralizing agent wet slurry preparation The above-mentioned neutralizing agent was mixed with water to form a slurry, and the slurry was adjusted at room temperature for 1.5 hours to obtain a lightly calcined return material-based magnesium neutralizing agent slurry.
[0058] 3. Wet nickel plating Same as Example 4.
[0059] 3. Solid-liquid separation Same as Example 4.
[0060] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 3. The calculated nickel precipitation rate was 78.29%, the cobalt precipitation rate was 89.83%, the nickel grade was 41.41%, and the unit consumption was 0.85 t / t.
[0061] Table 3. Effect of the magnesium neutralizing agent of the present invention on the slurry conditioning time in wet nickel immersion.
[0062] Example 6
[0063] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for wet slurry preparation and nickel deposition specifically includes the following steps: 1. Neutralizing agent preparation Same as Example 5.
[0064] 2. Neutralizing agent wet slurry preparation The above-mentioned neutralizing agent was mixed with water to form a slurry, and the slurry was adjusted at room temperature for 1 hour to obtain a lightly calcined return material-based magnesium neutralizing agent slurry.
[0065] 3. Wet nickel plating Same as Example 4.
[0066] 3. Solid-liquid separation Same as Example 4.
[0067] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 3. The calculated nickel precipitation rate was 78.59%, the cobalt precipitation rate was 91.67%, the nickel grade was 41.05%, and the unit consumption was 0.84 t / t.
[0068] Example 7
[0069] The method for using the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention for wet slurry preparation and nickel deposition specifically includes the following steps: 1. Neutralizing agent preparation Same as Example 5.
[0070] 2. Neutralizing agent wet slurry preparation The above-mentioned neutralizing agent was mixed with water to form a slurry, and the slurry was adjusted at room temperature for 0.5 hours to obtain a lightly calcined return material-based magnesium neutralizing agent slurry.
[0071] 3. Wet nickel plating Same as Example 4.
[0072] 3. Solid-liquid separation Same as Example 4.
[0073] The contents of each component in the filtrate and the resulting nickel slag were tested and are detailed in Table 3. The calculated nickel precipitation rate was 77.81%, the cobalt precipitation rate was 92.50%, the nickel grade was 40.26%, and the unit consumption was 0.85 t / t.
[0074] Compared with Example 5, Examples 6 and 7 shortened the slurry conditioning time, while maintaining the nickel precipitation rate at approximately 78% and the nickel grade above 40%. Simultaneously, the cobalt precipitation rate increased from 89.83% to 91.67% and 92.50%, respectively. The results indicate that appropriately shortening the slurry conditioning time helps reduce premature hydration of MgO and loss of effective activity, thus contributing to improved cobalt precipitation.
[0075] Example 8
[0076] A comparison of the nickel deposition results of Examples 2 to 7 shows that when the lightly calcined recycled low-chlorine magnesium neutralizer prepared in this invention is used for dry direct powder addition nickel deposition, the nickel precipitation rate of the samples calcined at 400℃ after washing with water for 30 min and 600℃ after washing with water for 30 min is about 78%, and the cobalt precipitation rate is close to 99%, indicating that the dry addition method has a better cobalt deposition effect.
[0077] When using the wet slurry preparation method, the nickel precipitation rate of the sample calcined at 500℃ after washing for 30 minutes reached 87.73%, and the cobalt precipitation rate reached 95.83%, with a unit consumption of 0.75t / t. This indicates that the wet slurry preparation method can improve the nickel precipitation effect and reagent utilization efficiency of some samples. Under different slurry preparation time conditions, the nickel grade of the sample calcined at 400℃ after washing for 30 minutes remained above 40%, indicating a high product grade.
[0078] Comparative Example 1 This comparative example uses untreated raw lightly calcined recycled material for dry nickel-cobalt deposition experiments. The steps are the same as in Example 2, except that the neutralizing agent is replaced with the raw lightly calcined recycled material.
[0079] Test results: The filtrate Ni concentration was 1.52 g / L, and the Co concentration was 0.112 g / L; the nickel precipitation rate was 60.31%, and the cobalt precipitation rate was 68.89%; the chlorine content in the nickel slag was 0.82%, indicating a significantly high impurity content. These results suggest that the unwashed, low-temperature calcined recycled material exhibits poor activity, high chlorine content, and its precipitation effect and product quality fail to meet industrial requirements.
[0080] Comparative Example 2 This comparative example only underwent water washing and did not undergo low-temperature calcination. After washing and drying, the sample was subjected to a wet nickel-cobalt immersion experiment, following the same steps as in Example 4.
[0081] Test results: Ni concentration in the filtrate was 1.18 g / L, and Co concentration was 0.086 g / L; nickel precipitation rate was 69.19%, and cobalt precipitation rate was 76.11%. The results indicate that while water washing alone can remove some chloride salts, the MgO content is low, and the activity decreases significantly after hydration, resulting in a precipitation effect far lower than that of the method described in this invention.
[0082] Comparative Example 3 This comparative example only underwent low-temperature calcination treatment without water washing. The original lightly calcined return material was directly calcined at 500℃ for 30 minutes and then subjected to a wet nickel-cobalt immersion experiment. The steps were the same as in Example 4.
[0083] Test results: Chlorine content 0.94%, nickel precipitation rate 72.06%, cobalt precipitation rate 82.31%; the residual chlorine in the nickel slag is high, failing to meet product purity requirements. The results indicate that calcination alone cannot effectively remove soluble chloride salts, and the chlorine content of the product still exceeds the standard.
[0084] In summary, this invention prepares a magnesium neutralizer with low chlorine content, high MgO content, and nickel-cobalt precipitation properties from lightly calcined recycled material through water washing dechlorination and low-temperature calcination at 400-600℃. The addition method can be selected by dry direct powdering or wet slurry preparation according to the precipitation target, thereby realizing the resource utilization and high-value utilization of lightly calcined recycled material.
[0085] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a low-chlorine, high-activity, lightly calcined recycled magnesium-based neutralizing agent, characterized in that, Specifically, the steps include the following: Step 1, Raw material preparation: Take lightly calcined recycled material as raw material, wherein the mass content of MgO in the lightly calcined recycled material is 70% to 80%, the mass content of chlorine is 0.8% to 2.0%, and the citric acid activity is 40-70. Step 2, water washing and dechlorination: Mix the above lightly calcined return material with water in a certain proportion, and wash it with water under stirring conditions to dissolve the soluble chloride salts in the material into the liquid phase; Step 3, solid-liquid separation: After washing, solid-liquid separation is carried out by filtration to obtain the dechlorinated light calcined return filter cake. The filter cake is placed in a drying device and dried to constant weight. Step 4, low-temperature calcination: The dried filter cake is placed in a calcination device and calcined at 400-600℃. After calcination, it is naturally cooled to obtain a low-chlorine, high-activity light-calcined recycled magnesium neutralizer. The magnesium neutralizer has an MgO mass content ≥93%, a chlorine mass content ≤0.40%, and a citric acid activity value ≤31s.
2. The preparation method according to claim 1, characterized in that, In step 1, the lightly burned return material is any one or a combination of two of the following: recycled return material generated during the calcination of magnesium hydroxide to prepare magnesium oxide, dust removal ash, or magnesium-containing return material.
3. The preparation method according to claim 1, characterized in that, In step 2, the liquid-to-solid mass ratio of the water washing is (3-8):1, the stirring time is 10-60 min, the water washing temperature is room temperature, and the stirring speed is 100-300 rpm.
4. The preparation method according to claim 1, characterized in that, In step 3, the filter cake is dried at a temperature of 85–105°C until the moisture content of the material is ≤2%.
5. The preparation method according to claim 1, characterized in that, In step 4, the calcination time is 20-60 min, and the heating rate is 5-10 °C / min; the calcination equipment is any one of a muffle furnace, rotary kiln, or pusher kiln.
6. A low-chlorine, high-activity, lightly calcined recycled magnesium-based neutralizing agent, characterized in that, The magnesium neutralizing agent is prepared by the method described in any one of claims 1-5.
7. The application of the low-chlorine, high-activity light-burned recycled magnesium neutralizing agent according to claim 6, characterized in that, The application of the magnesium neutralizing agent in the precipitation of nickel-cobalt solutions involves adding the magnesium neutralizing agent as a neutralizing and precipitating agent to the nickel-cobalt solution, causing nickel and cobalt to precipitate out in the form of precipitates.
8. The application according to claim 7, characterized in that, The magnesium neutralizing agent is added to the nickel-cobalt solution using either a dry or wet method; wherein, the wet method slurry preparation time is 0.5–1.5 h.
Citation Information
Patent Citations
Activated magnesia, and preparation method and application thereof
CN110921688A