A method for gallium extraction by selective separation and cascade recovery of gallium and vanadium from bayer liquor
Patent Information
- Application Number
- CN202611520634.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-24
AI Technical Summary
后续无论采用化学沉淀、溶剂萃取还是电解,均需额外增加镓钒分离工序,流程冗长、成本高昂
Smart Images

Figure CN123152899A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gallium extraction processes, and in particular to a gallium extraction method for selective separation and graded recovery of gallium and vanadium from Bayer mother liquor. Background Technology
[0002] Gallium, as a core material for second- and third-generation semiconductors, is widely used in 5G communications, radar, satellites, optoelectronic displays, and power devices, possessing extremely high strategic value. Bauxite typically contains 0.002-0.008% metallic gallium. In the Bayer process for alumina production, approximately 70% of the gallium dissolves with the alumina into the mother liquor, where it is enriched through recycling to reach concentrations of 100-300 mg / L. Currently, about 90% of the world's primary gallium originates from the recycled mother liquor of the Bayer process for alumina production.
[0003] Bayer mother liquor is characterized by strong alkalinity (caustic alkali concentration 150-250 g / L), high aluminum concentration (Al₂O₃ approximately 80-120 g / L), and low gallium concentration (100-300 mg / L). More importantly, Bayer mother liquor typically contains vanadium (V), which has chemically very similar properties to gallium; both exist as oxygen-containing anions in alkaline systems (Ga(OH)₄). - With VO4 3- or HVO4 2- This leads to significant co-adsorption of vanadium during gallium adsorption by the amine oxime chelating resin. Studies have shown that in the Bayer mother liquor system, the co-adsorption rate of vanadium can reach over 70%, while the gallium / vanadium separation factor is only around 2.56.
[0004] Currently, the mainstream technology for recovering gallium from Bayer mother liquor is the resin adsorption method, and its basic process flow is as follows: (1) Traditional resin adsorption-single-stage desorption process This process is currently the most common method for gallium extraction in industry. A metallo-oxime chelating resin (such as LSC-600, LSC-700, etc.) is packed into a resin column, and a gallium-containing Bayer mother liquor is allowed to flow through the resin column at a certain flow rate. The metallo-oxime functional groups on the resin undergo coordination chelation with gallate ions to achieve adsorption. After adsorption saturation, single-stage desorption is performed using NaOH-Na2S eluent or hydrochloric acid. The desorbed solution is then purified, concentrated, and electrolyzed to obtain the metallic gallium product.
[0005] This process has the following main technical defects: Firstly, vanadium co-adsorption and selectivity are poor—the selectivity difference between gallium and vanadium in the vanadium-amine oxime resin is insufficient, and vanadium competes with gallium for active sites on the resin. In industrial practice, while the gallium adsorption rate is only 60%-65%, the vanadium co-adsorption rate is as high as 70% or more. A large amount of vanadium occupies the effective adsorption sites of the resin, leading to a continuous decay of the resin's working capacity for gallium.
[0006] Secondly, vanadium causes irreversible accumulation and poisoning on the resin. Vanadium can form a more stable N,O-bident coordination structure with the amylopectin group than gallium, making it difficult for conventional desorbers to effectively elute vanadium from the resin. As the operating cycle increases, the vanadium accumulated on the resin gradually occupies the active sites, the resin's working capacity decreases year by year, and its service life is significantly shortened.
[0007] Third, the contamination of gallium and vanadium in the desorption solution increases the difficulty of purification. In single-stage desorption mode, the adsorbed gallium and vanadium are eluted simultaneously, resulting in a mixture of gallium and vanadium in the desorption solution. Subsequent processes, whether chemical precipitation, solvent extraction, or electrolysis, require an additional gallium-vanadium separation step, making the process lengthy and costly.
[0008] Fourth, the NaOH-Na2S rinsing agent introduces S 2- Pollution – Traditional processes use a NaOH-Na2S system for desorption, with a desorption rate of only 60%-90%. The introduction of Na2S introduces sulfur into the desorption solution. 2- Impurities, S must be removed with an oxidant before electrolysis. 2- Removal increases process complexity and production costs.
[0009] Fifth, the overall gallium recovery rate is low throughout the entire process. Due to multiple factors such as poor adsorption selectivity, low desorption efficiency, and vanadium accumulation poisoning, the overall gallium recovery rate is usually less than 55%, resulting in a serious waste of a large amount of strategic metal resources.
[0010] (2) Resin adsorption-solvent extraction coupled process In recent years, researchers have proposed a synergistic process of adsorption with a methylamine oxime chelating resin, hydrochloric acid elution, tributyl phosphate (TBP) extraction, and water back-extraction. This process involves eluting with hydrochloric acid after resin adsorption to obtain a gallium-containing desorbate, followed by selective extraction of gallium using a TBP / kerosene hydrochloric acid system, thus achieving gallium-vanadium separation.
[0011] Although this process can achieve deep separation of gallium and vanadium, it has the following drawbacks: it adds a complete extraction-back-extraction section, which significantly increases equipment investment and operating costs; the TBP / kerosene system suffers from organic phase loss and emulsification problems; and the process is lengthy, making it uneconomical for industrial-scale promotion.
[0012] (3) Traditional continuous ion exchange device Existing technologies disclose continuous ion exchange apparatus and methods for extracting gallium from Bayer mother liquor, employing at least four sets of resin columns in series to alternately achieve adsorption, washing, rinsing, and conversion. However, this apparatus still uses a traditional single-stage rinsing mode, failing to address the core issues of selective separation of gallium and vanadium and vanadium accumulation poisoning. Summary of the Invention
[0013] This invention addresses the technical problem in Bayer's gallium extraction process where insufficient selective adsorption difference between gallium and vanadium by the amine oxime chelating resin leads to excessive vanadium co-adsorption, resin poisoning, gallium-vanadium contamination in the desorption solution, and an overall gallium recovery rate of less than 55%. It provides a method for selective separation and graded recovery of gallium and vanadium from Bayer's mother liquor. This invention achieves efficient gallium recovery and resource utilization of vanadium through a triple innovation of enhanced selective adsorption, graded desorption, and in-situ resin regeneration.
[0014] The present invention is achieved by the following technical solution.
[0015] A gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor includes the following steps: S1. Homogenization and selective chemical conditioning pretreatment of Bayer mother liquor: The Bayer process seed mother liquor is allowed to stand and homogenize, and then transferred to a selective chemical conditioning reactor. The temperature inside the reactor is controlled at 30-40℃, the NaOH concentration is adjusted to 0.8-1.5mol / L, and the residence time is 30-60min. S2. Precision filtration pretreatment; S3. Continuous ion exchange adsorption: The purified mother liquor is distributed to ≥4 sets of resin columns connected in series through the feed main; S4. Gradient-segmented desorption: First, pure water is introduced for forward washing. After washing, the three-stage desorption process is performed sequentially: a. Pre-elution stage: The saturated resin is pre-eluted using 2-3 BV, 1-2 N NaOH at 30-40℃; b. Main desorption section: The resin is mainly desorbed using 3-4 BV, 4-6 N NaOH at 40-50℃ to obtain a high-concentration gallium-rich desorption solution; c. Transformation and regeneration section: The resin is deeply transformed and regenerated using 2-3 BV, 1-2 M HCl or H2SO4 at 20-30℃ to obtain vanadium-containing transformation acid solution. S5. Gallium-rich desorption solution electrolytic refining; S6. Transformation of vanadium recovery from acidic solutions.
[0016] By employing the above technical solution, this invention addresses the industry challenge of insufficient selectivity of amylopectin resins for gallium and vanadium by adding a selective chemical conditioning pretreatment unit before the Bayer mother liquor enters the resin column. By precisely controlling the temperature (30-40℃) and alkalinity of the mother liquor, and utilizing the differences in coordination chemistry between gallium and vanadium under specific conditions, the ionic form of vanadium is selectively altered, reducing the coordination competition between vanadium and amylopectin groups. When the temperature is increased to 60℃, the vanadium extraction rate increases by 2.4 times; therefore, this invention strictly controls low-temperature conditions to inhibit vanadium adsorption, weakening the co-adsorption driving force of vanadium at the source. After pretreatment, the effective adsorption rate of vanadium in the mother liquor is reduced by more than 40%, and the gallium / vanadium adsorption selectivity ratio is increased by more than 3 times.
[0017] This invention abandons the traditional NaOH-Na2S single-stage rinsing mode and innovatively designs a three-stage gradient desorption process: a low-concentration alkaline solution pre-washing vanadium removal stage, a high-concentration alkaline solution main gallium desorption stage, and a regenerated acid deep transformation stage. Utilizing the difference in coordination strength between gallium and vanadium on the resin (vanadium forms a more stable N,O-bidentate structure, while gallium is a monodentate O-coordinate), the low-concentration alkaline solution preferentially breaks the coordination bonds of gallium to elute it off. The high-concentration alkaline solution then deeply desorbs residual gallium, and finally, the acid solution thoroughly removes stubbornly adsorbed vanadium from the resin, achieving deep regeneration of the resin. The collected vanadium-enriched solution enters the vanadium recovery stage, while the gallium-enriched solution directly enters the electrolysis stage, realizing the stepped separation and separate recovery of gallium and vanadium.
[0018] This invention addresses the persistent industry problem of irreversible vanadium accumulation and poisoning in resins by utilizing the transition acid solution, traditionally considered waste liquid. The transition acid solution contains a high concentration of vanadium eluted from the resin; after neutralization and precipitation, ammonium vanadate or vanadium pentoxide products can be obtained, achieving the resource recovery of vanadium. This design integrates resin regeneration and vanadium recovery, extending the resin's lifespan (from 6-12 months to over 24 months per filling cycle) and increasing vanadium product revenue, turning waste into treasure.
[0019] This invention designs a continuous ion exchange device with at least four sets of resin columns connected in series. Each set is switched periodically via a main valve to perform five processes: adsorption, washing, pre-washing to remove vanadium, main desorption of gallium, and transformation regeneration. The desorbent from each process is collected in stages according to its grade: low-concentration pre-wash (containing a small amount of gallium) is returned to the adsorption front end for reprocessing; high-concentration main desorbent (rich in gallium) is directly fed into the electrolysis section; and the transformation acid (rich in vanadium) is fed into the vanadium recovery section. The system achieves fully continuous operation of adsorption-stage desorption-regeneration, increasing the processing capacity of a single unit by more than three times.
[0020] This invention constructs a four-stage closed-loop reuse system: adsorption tail liquid - alumina plant reuse + pre-washing and descaling liquid - adsorption front-end reuse + conversion acid liquid - vanadium recovery + electrolytic residue - leaching agent preparation and reuse. The entire process achieves zero liquid phase discharge, full recovery of valuable metals, and reduces water consumption by more than 60%, fully meeting the requirements of clean production.
[0021] Furthermore, in step S1, the Bayer process seed mother liquor is allowed to stand for 2-4 hours.
[0022] Furthermore, in step S1, a variable frequency feed pump is used at a speed of 2-5m. 3 The mother liquor is fed into the selective chemical conditioning reactor at a constant flow rate of / h.
[0023] Furthermore, in step S2, the conditioned mother liquor is fed into a precision filter equipped with a micron-level alkali-resistant filter element, with an operating pressure of 0.1-0.3 MPa and an operating temperature of 30-50℃.
[0024] Furthermore, in step S3, the resin column assembly is filled with a methylamine oxime chelating resin.
[0025] Furthermore, in step S3, the flow rate of the liquid through the column is controlled at 2-4 BV / h, and the operating temperature is 30-40℃.
[0026] Furthermore, in step S5, the control parameters for the electrolytic refining of the gallium-rich desorption solution are as follows: cathode current density is 200–800 A / m²; cell voltage is 3.0–4.0 V; electrolysis temperature is 30–50 °C; electrolyte NaOH concentration is 80–150 g / L; electrode distance is 1–3 cm; electrolysis time is 6–12 h, and electrolysis is stopped when the gallium concentration in the electrolyte drops below 1 g / L; the residual electrolyte is returned to the rinsing agent preparation process for reuse.
[0027] Furthermore, in step S6, the vanadium-containing conversion acid solution is fed into the vanadium recovery reactor, the pH is adjusted to 2-4 for neutralization and precipitation, the reaction temperature is controlled at 60-90℃, and the reaction time is 1-2 hours to obtain ammonium vanadate precipitate. After solid-liquid separation and calcination, the precipitate is used to obtain vanadium pentoxide product.
[0028] Furthermore, all adsorption tail liquid is returned to the alumina plant for reuse in various processes; pre-washing liquid is returned to the adsorption front end for reprocessing; the residual liquid of the conversion acid solution after vanadium recovery is returned to the preparation of leaching agents; and the residual liquid of electrolysis is returned to the preparation of leaching agents.
[0029] This application has the following beneficial effects: (1) Solve the problem of selective separation of gallium and vanadium from the source This invention reduces the co-adsorption rate of vanadium from over 70% to below 30% through a combination of selective chemical conditioning pretreatment and low-temperature control, thereby increasing the gallium / vanadium adsorption selectivity ratio by more than three times and fundamentally alleviating the problem of vanadium poisoning in resins.
[0030] (2) Stepwise recovery of gallium and vanadium by gradient segmented desorption This invention employs a three-stage desorption process: low-concentration pre-washing for vanadium removal, high-concentration main gallium desorption, and acid-based regeneration. Compared to the traditional single-stage rinsing method, the gallium desorption rate is increased from 60%-90% to over 95%. Simultaneously, it achieves graded collection and separate treatment of gallium and vanadium desorption solutions, reducing the gallium-vanadium intermixing rate in the desorption solution by over 80%, and significantly simplifying subsequent purification processes.
[0031] (3) Turning waste into treasure to realize vanadium resource utilization This invention recycles vanadium from the waste conversion acid solution in traditional processes, which can additionally produce ammonium vanadate or vanadium pentoxide products, increasing the revenue from associated metals, while completely eliminating the environmental disposal pressure of vanadium-containing hazardous waste.
[0032] (4) The service life of the resin is greatly extended. By inhibiting vanadium adsorption at the source and providing deep acid regeneration, the continuous and stable operation cycle of the amygdoxime chelating resin after a single filling is extended from 6-12 months to more than 24 months, and the resin replacement cost is reduced by more than 50%.
[0033] (5) The overall gallium recovery rate of the entire process has been greatly improved. The combined innovations of enhanced selective adsorption at the source, improved gradient desorption efficiency, and closed-loop recycling to prevent loss have increased the overall gallium recovery rate from less than 55% to 80%-85%, a 25-30 percentage point improvement compared to traditional processes. Simultaneously, the added revenue from vanadium product recovery enhances overall economic benefits by over 40%. Attached Figure Description
[0034] Figure 1 This is a flowchart illustrating the present invention. Detailed Implementation
[0035] The present invention will be further described below with reference to embodiments. Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods. Unless otherwise specified, the materials used in the preparation process in the following embodiments have not undergone further processing and are all commercially available.
[0036] like Figure 1 As shown, this invention employs modular equipment, comprising a selective conditioning pretreatment unit, a continuous ion exchange unit, a gradient segmented desorption unit, a vanadium recovery unit, an electrolytic refining unit, and an automatic control unit. The overall process flow, the composition of each unit, and the upstream and downstream connections are as follows: The raw material is the seed mother liquor produced during the Bayer process of alumina production. The raw liquor first enters a selective chemical conditioning pretreatment reactor, where the ionic form of vanadium is selectively regulated by precisely controlling the temperature (30-40℃) and alkalinity conditions to reduce its coordination competition with the ammonia oxime group. After conditioning, the mother liquor is filtered through a precision filter to remove suspended solid impurities before being fed into four sets of continuous ion exchange resin columns arranged in series.
[0037] Each column group performs five processes in a cycle through switching of the main pipe valve: adsorption station (mother liquor passes through the column, gallium is selectively adsorbed, and vanadium co-adsorption is significantly suppressed) → washing station (pure water washing removes residual mother liquor and free impurities) → pre-elution station (low-concentration alkaline solution preferentially elutes gallium, achieving preliminary separation of gallium and vanadium) → main desorption station (high-concentration alkaline solution deeply desorbs residual gallium, producing high-purity gallium-rich desorption solution) → transformation and regeneration station (acid solution thoroughly removes stubbornly adsorbed vanadium on the resin, restoring resin activity), and returns to the adsorption station after completion.
[0038] The pre-washing solution (containing a small amount of gallium) is returned to the adsorption front end for reprocessing; the main desorption solution (rich in gallium) is stored in the desorption solution tank, and after precision filtration, it is directly sent to the electrolytic cell for electrolytic refining to obtain high-purity metallic gallium products; the conversion acid solution (rich in vanadium) is sent to the vanadium recovery unit, and after neutralization and precipitation, ammonium vanadate or vanadium pentoxide products are obtained.
[0039] All adsorption tail liquid is returned to the alumina plant for reuse in the seed processing stage; electrolysis residue is returned to the leaching agent preparation stage for reuse. The entire process achieves zero liquid phase discharge and full recovery of valuable metals.
[0040] The following is a detailed explanation of the specific process flow.
[0041] Step 1: Homogenization and selective chemical conditioning pretreatment of Bayer mother liquor The Bayer process mother liquor produced by the alumina plant is uniformly collected in the raw liquor storage tank for static homogenization, with the hydraulic retention time controlled at 2-4 hours; then fed through a variable frequency feed pump at a constant flow rate (2-5 m³ / h). 3 The mother liquor is fed into a selective chemical conditioning reactor ( / h). The temperature inside the reactor is precisely controlled at 30-40℃ (low temperature conditions inhibit vanadium adsorption), the NaOH concentration is adjusted to 0.8-1.5mol / L, and the residence time is 30-60min. By utilizing the difference in coordination chemical behavior between gallium and vanadium under specific conditions, the ionic form of vanadium is selectively changed, reducing the coordination competition between vanadium and the amylopectin group.
[0042] Step 2: Precision Filtration Pretreatment The conditioned mother liquor is fed into a precision filter equipped with a 1μm precision PTFE (polytetrafluoroethylene) sintered filter element or a hydrophilic PTFE pleated filter element. The filter element has an outer diameter of 68-69mm, the sealing ring is made of fluororubber or fluoropolymer-coated material, and the shell material is 2205 duplex stainless steel or PP. The operating pressure is 0.1-0.3MPa, and the operating temperature is 30-50℃. The filter removes suspended solid impurities larger than 1μm from the mother liquor, ensuring the turbidity of the effluent is ≤5NTU, thus guaranteeing the clarity of the mother liquor entering the column meets the standards. The filter is equipped with a differential pressure transmitter; when the inlet and outlet pressure difference reaches 0.08-0.10MPa, an alarm is triggered, and the filter element is replaced. Under normal operating conditions, the filter element replacement cycle is 7-10 days.
[0043] Step 3: Continuous ion exchange adsorption (selective adsorption of gallium) The purified mother liquor is distributed to four sets of resin columns connected in series via the main feed pipe. Each column is filled with a metallo-oxime chelating resin. The feed flow rate through the columns is controlled at 2-4 BV / h, and the operating temperature is 30-40℃ (consistent with the conditioning temperature to continuously suppress vanadium adsorption). After conditioning pretreatment, the co-adsorption rate of vanadium decreases from over 70% to below 30%. The main adsorption column completes over 85% gallium ion adsorption, while the subsequent series columns intercept trace amounts of gallium ions that leak through. The five processes are carried out periodically and alternately by switching the main pipe valve among the columns.
[0044] Step 4: Gradient segmented desorption – stepwise recovery of gallium and vanadium After adsorption saturation, the resin column assembly is switched to the washing station. First, pure water is introduced for forward washing to remove residual mother liquor and free impurities entrained on the resin surface. After washing, it proceeds to the three-stage desorption stage: a. Pre-elution stage: A low-concentration alkaline solution (1-2N NaOH) is used to pre-elute the saturated resin. Taking advantage of the relatively weak coordination bonds of gallium, gallium is preferentially eluted from the resin. The pre-elution solution contains a small amount of gallium and some vanadium, and is refluxed to the adsorption front end for reprocessing.
[0045] b. Main desorption section: High-concentration alkaline solution (4-6N NaOH) is used for main desorption of the resin to deeply desorb residual gallium. A high-concentration gallium-rich desorption solution (Ga≥5g / L, gallium / vanadium ratio≥20:1) is produced, stored in the desorption solution storage tank, and directly sent to the electrolysis section.
[0046] c. Transformation and Regeneration Section: The resin undergoes deep transformation and regeneration using acid (1-2M HCl or H2SO4) to thoroughly remove stubbornly adsorbed vanadium. The resulting vanadium-containing transformation acid (V≥2g / L) is sent to the vanadium recovery unit. The three-stage desorption process achieves a gallium desorption rate ≥95% and a gallium / vanadium separation efficiency ≥90%.
[0047] Step 5: Electrolytic refining with gallium-rich desorption solution After precision filtration to remove trace suspended solids, the gallium-rich main desorption solution is directly fed into the electrolytic cell (without additional impurity removal and concentration). Electrolytic refining is carried out in an alkaline system, resulting in the deposition of high-purity metallic gallium (purity ≥99.99%) on the cathode. The residual electrolyte is returned to the eluent preparation process for reuse. The electrolytic refining control parameters are as follows: Cathode current density: 200–800 A / m². Production efficiency is low when the current density is below 100 A / m²; when the current density exceeds 400 A / m², impurities such as Pb, Zn, Fe, and Sn will exceed the standard for 99.9999% high-purity gallium. In this invention, the Ga content in the gallium-rich desorption solution is ≥5 g / L. Considering impurity control requirements, the cathode current density is controlled within the range of 200–800 A / m², preferably 300–500 A / m².
[0048] Cell voltage: 3.0–4.5 V. In alkaline systems, the high conductivity of the strongly alkaline medium results in a relatively low cell voltage. When using stainless steel anodes, the cell voltage can be controlled within the range of 3.0–4.0 V.
[0049] Electrolysis temperature: 30–50 °C. Below 30 °C, gallium wettability is poor, and current efficiency decreases significantly; excessively high temperatures exacerbate gallium dissolution losses in alkaline solutions. This invention controls the electrolysis temperature to 30–50 °C, preferably 40–50 °C. When the gallium concentration in the electrolyte is approximately 40 g / L and the NaOH concentration is approximately 120 g / L, higher current efficiency can be obtained within this temperature range.
[0050] Electrolyte NaOH concentration: 80–150 g / L. The gallium-rich main desorption solution uses 4-6N NaOH for desorption. Due to the high NaOH concentration, it needs to be appropriately diluted or adjusted to 80–150 g / L before entering the electrolytic cell. Too low a NaOH concentration results in insufficient solution conductivity, while too high a concentration exacerbates the chemical dissolution of gallium. A concentration of 100–130 g / L is preferred.
[0051] Electrode spacing: 1–3 cm, preferably 1–2 cm. Appropriately reducing the electrode spacing can decrease the cell voltage and power consumption. Studies have shown that when the electrode spacing is 1 cm, combined with optimized current density and NaOH concentration, the current efficiency can reach over 91%.
[0052] Electrolysis time: 6–12 h. The electrolysis time is determined based on the gallium concentration and current density of the gallium-rich desorption solution. Electrolysis is stopped when the gallium concentration in the electrolyte drops below 1 g / L.
[0053] Electrolysis residue treatment: The electrolysis residue is returned to the rinsing agent preparation process for reuse. The NaOH concentration in the residue remains high after electrolysis, allowing it to be directly used to prepare the alkali solution required for the pre-washing or main desorption stage, thus achieving closed-loop alkali solution reuse.
[0054] Step 6: Transformation of vanadium recovery from acidic solutions Vanadium-containing acid solution is fed into a vanadium recovery reactor, where it is neutralized and precipitated with ammonia. Ammonia is slowly added under stirring to adjust the pH to 2-4, and the reaction temperature is controlled at 60-90℃ for 1-2 hours, yielding ammonium vanadate precipitate. After solid-liquid separation and calcination, the precipitate yields vanadium pentoxide (V₂O₅ ≥ 98%), achieving resource recovery of vanadium. The precipitate solution is returned to the leaching agent preparation process for reuse.
[0055] Step 7: Closed-loop recycling of materials throughout the entire process All adsorption tail liquid is returned to the alumina plant for reuse in various processes; pre-washing liquid is returned to the adsorption front end for reprocessing; the residual liquid of the conversion acid solution after vanadium recovery is returned to the preparation of the leaching agent; and the residual liquid of the electrolysis solution is returned to the preparation of the leaching agent. The entire process achieves zero liquid phase discharge and full recovery of valuable metals.
[0056] In the above process, the key process parameters are controlled as follows: ① Selective chemical conditioning pretreatment (core: inhibiting vanadium co-adsorption) Reaction temperature: 30-40℃ (low temperature inhibits vanadium adsorption); Stay duration: 30-60 minutes; Control targets: reduce the effective adsorption rate of vanadium by more than 40%, and increase the gallium / vanadium adsorption selectivity ratio by more than 3 times; Process function: To weaken the coordination competition between vanadium and the amylopyridine oxime group from the source.
[0057] ② Continuous ion exchange adsorption Resin type: Aminooxime chelating resin (LSC-600 / LSC-700 series); Number of resin column groups: ≥4 groups in series; Column flow rate: 2-4 BV / h; Operating temperature: 30-40℃; Adsorption rate: Gallium ≥ 85%, Vanadium co-adsorption rate ≤ 30%; Process function: Selectively adsorbs and enriches gallium ions in the mother liquor, while maximally suppressing vanadium co-adsorption.
[0058] ③ Gradient-segmented desorption Pre-washing and stripping stage: 1-2N NaOH, 2-3BV, temperature 30-40℃; Main desorption section: 4-6N NaOH, 3-4BV, temperature 40-50℃; Transformation and regeneration section: 1-2M HCl or H2SO4, 2-3BV, room temperature (20-30℃). Gallium desorption rate: ≥95%; Gallium / vanadium separation efficiency: ≥90%; Function of the process: To achieve the cascade separation and separate recovery of gallium and vanadium.
[0059] ④ Vanadium recovery Neutralization precipitation pH: 2-4 (optimal range for ammonium vanadate precipitation); Precipitation temperature: room temperature (20-30℃); Product specifications: V2O5 ≥ 98%; Process function: To recover vanadium from the transformation acid solution.
[0060] Example 1 A gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor includes the following steps: The raw material used in this embodiment is the mother liquor from the Bayer process of an alumina plant. The main components are as follows: Ga 248 mg / L, V 386 mg / L, Al2O3 102 g / L, Na2O (caustic alkali) 168 g / L, SiO2 5.2 g / L, and suspended solids (SS) 186 g / L.
[0061] Step 1: Homogenization and selective chemical conditioning pretreatment of Bayer mother liquor The mother liquor from the Bayer process was collected in a stock solution storage tank and allowed to stand for 3 hours for homogenization. The mother liquor was then fed into a selective chemical conditioning reactor at a constant flow rate of 3.0 m³ / h using a variable frequency drive (VFD) pump. The temperature inside the reactor was precisely controlled at 35°C, and the NaOH concentration was diluted with deionized water to 1.0 mol / L (corresponding to a mass concentration of 40 g / L), with a residence time of 45 min. Under these alkaline conditions, the maximum adsorption capacities of the amine oxime chelating resin for Ga(III) and V(V) were 23.7 mg / g and 20.1 mg / g, respectively. While gallium maintained a high adsorption capacity, the co-adsorption driving force of vanadium was significantly weakened.
[0062] Step 2: Precision Filtration Pretreatment The conditioned mother liquor is fed into a precision filter equipped with a 1 μm precision PTFE sintered filter element. The filter element has an outer diameter of 68 mm, a sealing ring made of fluororubber, and a shell made of 2205 duplex steel. The operating pressure is 0.2 MPa, and the operating temperature is 35℃. The filter removes suspended solid impurities with a particle size greater than 1 μm from the mother liquor, and the turbidity of the effluent is 3.2 NTU, ensuring that the clarity of the mother liquor entering the column meets the standards.
[0063] Step 3: Continuous ion exchange adsorption The purified mother liquor was distributed to four sets of resin columns connected in series via a feed manifold. Each column was filled with LSC-600 amine oxime chelating resin. The feed flow rate through the columns was controlled at 3.0 BV / h, and the operating temperature was 35℃. After conditioning and pretreatment, the Ga adsorption rate of the main adsorption column reached 89.2%, and the V co-adsorption rate was 26.5%. Subsequent series columns intercepted trace amounts of gallium ions that leaked through. The resin saturation adsorption capacity was: Ga 22.8 mg / g, V 18.9 mg / g.
[0064] Step 4: Gradient segmented desorption – stepwise recovery of gallium and vanadium After adsorption saturation, the resin column assembly is switched to the washing station. First, pure water is introduced for forward washing to remove residual mother liquor and free impurities entrained on the resin surface. After washing, it proceeds to the three-stage desorption stage: a. Pre-elution stage: 1.5 N NaOH, 2.5 BV, and 35℃ were used to pre-elute the saturated resin. The Ga elution rate was 52.3%, the V elution rate was 4.6%, and the Ga / V ratio of the pre-elution solution was 7.1:1. The solution was refluxed to the adsorption front end for reprocessing.
[0065] b. Main desorption section: 4.5 N NaOH, 3.5 BV, and 45℃ are used for main desorption of the resin, deeply desorbing residual gallium. The Ga desorption rate is 44.5%, the Ga concentration of the main desorption solution is 5.8 g / L, and the Ga / V ratio is 26.3:1. The solution is stored in a desorption solution tank and directly sent to the electrolysis section.
[0066] c. Transformation and Regeneration Section: Using 1.5 M HCl, 2.5 BV, and a temperature of 25℃, the resin undergoes deep transformation and regeneration to thoroughly remove stubbornly adsorbed vanadium. The vanadium desorption rate is 91.8%, the vanadium concentration in the transformation acid solution is 2.4 g / L, the residual vanadium in the resin is 1.7 mg / g, and the resin regeneration rate is 98.2%.
[0067] The three-stage desorption process achieved a total Ga desorption rate of 96.8%, a V desorption rate of 96.4%, and a gallium / vanadium separation efficiency of 91.5%.
[0068] Step 5: Electrolytic refining with gallium-rich desorption solution After being precision filtered to remove trace suspended solids, the gallium-rich main desorption solution was directly fed into an electrolytic cell for electrolytic refining in an alkaline system. Control parameters were as follows: cathode current density 400 A / m², cell voltage 3.6 V, electrolysis temperature 42℃, electrolyte NaOH concentration 110 g / L, electrode distance 1.5 cm, and electrolysis time 8 h. Electrolysis was stopped when the gallium concentration in the electrolyte dropped to 0.8 g / L. High-purity metallic gallium was deposited on the cathode, with a purity ≥99.99% after washing and a current efficiency of 91.2%. The residual electrolyte was returned to the leaching agent preparation process for reuse.
[0069] Step 6: Transformation of vanadium recovery from acidic solutions The vanadium-containing conversion acid solution was fed into a vanadium recovery reactor. Ammonia was used as a neutralizing and precipitating agent. Under stirring, ammonia was slowly added to adjust the pH to 2.8, and the reaction temperature was controlled at 75°C for 1.5 hours to obtain ammonium vanadate precipitate. After solid-liquid separation and calcination, vanadium pentoxide product with a V₂O₅ purity of 98.6% was obtained. The precipitate solution was returned to the leaching agent preparation process for reuse.
[0070] Step 7: Closed-loop recycling of materials throughout the entire process All adsorption tail liquid is returned to the alumina plant for reuse in various processes; pre-washing liquid is returned to the adsorption front end for reprocessing; the residual liquid of the conversion acid solution after vanadium recovery is returned to the preparation of the leaching agent; and the residual liquid of electrolysis is returned to the preparation of the leaching agent.
[0071] Product Specifications: High-purity metallic gallium has a purity of ≥99.99% and a comprehensive Ga recovery rate of 83.6%; vanadium pentoxide (V₂O₅) has a purity of 98.6% and a comprehensive V recovery rate of 81.3%.
[0072] To verify the inventiveness and synergistic effect of the gradient concentration and segmented desorption coupling technology of this invention, the following comparative examples were designed. The experiment used a metallo-oxime chelating resin LSC-600, which was saturated with Bayer mother liquor (saturated adsorption capacity: Ga 23.7 mg / g, V 20.1 mg / g), and different desorption schemes were compared.
[0073] Comparative Example 1: Single-segment desorption vs. two-segment desorption vs. three-segment desorption Experimental protocol
[0074] Experimental results
[0075] The results above show that Comparative Example 1-1 (single-stage 4N NaOH) had a gallium desorption rate of only 62.3% and a vanadium desorption rate of only 8.5%, with a large amount of vanadium remaining on the resin, causing cumulative poisoning. Although Comparative Example 1-2 increased the gallium desorption rate to 88.2% by adding Na2S, it introduced S... 2-The desorption process was contaminated, with a vanadium desorption rate of only 15.2% and severe gallium-vanadium contamination in the desorption solution. Comparative Examples 1-3 (two-stage desorption) showed a gallium desorption rate of 78.6% and a vanadium desorption rate of 35.4%, but due to the lack of an acid-to-resin transition stage, 13.0 mg / g of vanadium remained on the resin. In contrast, Example 1 of this invention employed a three-stage gradient desorption process: low-concentration alkali pre-elution + high-concentration alkali main desorption + acid-to-resin transition regeneration. This resulted in a gallium desorption rate of 96.8% and a vanadium desorption rate of 92.1%, with a gallium / vanadium ratio as high as 28.6:1 in the desorption solution. The resin retained only 1.6 mg / g of vanadium, and the resin regeneration rate reached 98.5%. The synergistic effect of the three-stage gradient desorption increased the gallium desorption rate by 34.5 percentage points compared to a single-stage 4N NaOH desorption process and by 18.2 percentage points compared to a two-stage process; the vanadium desorption rate increased by 83.6 percentage points compared to a single-stage process and by 56.7 percentage points compared to a two-stage process.
[0076] Comparative Example 2: Optimization of Low-Concentration Alkali Prewashing and De-washing Concentration Experimental scheme: The main desorption section (4.5N NaOH, 3BV) and the transformation and regeneration section (1.5M HCl, 3BV) were fixed to investigate the effect of NaOH concentration in the pre-elution section on the selective separation of gallium / vanadium.
[0077]
[0078] The results show that as the NaOH concentration in the pre-elution stage increased from 0.5N to 2.0N, the Ga elution rate increased from 18.3% to 78.4%, but the V elution rate increased sharply from 2.1% to 28.7%, and the Ga / V ratio in the pre-elution solution decreased from 4.8:1 to 1.5:1. When the NaOH concentration in the pre-elution stage was 1.0N, the Ga / V ratio in the pre-elution solution reached 6.7:1, and the Ga / V ratio in the main desorption solution reached 28.6:1, achieving optimal fractional separation of gallium and vanadium. Excessively high NaOH concentrations can lead to simultaneous elution of vanadium, compromising the selective separation effect.
[0079] Comparative Example 3: Comparison of Acid Types in the Acid Transition and Regeneration Section Experimental scheme: The pre-elution section (1.0N NaOH, 3BV) and the main desorption section (4.5N NaOH, 3BV) were fixed to investigate the effect of different acid solutions in the transformation and regeneration section on the removal of residual vanadium in the resin.
[0080]
[0081] The results show that 1.5M hydrochloric acid achieved a 92.1% desorption rate for stubbornly adsorbed vanadium on the resin, leaving only 1.6 mg / g of residual vanadium and a regeneration rate of 98.5%, with minimal damage to the resin structure. Sulfuric acid and nitric acid showed vanadium desorption rates of 65.3% and 70.8%, respectively, both lower than hydrochloric acid. Furthermore, while 2.0M hydrochloric acid increased the vanadium desorption rate to 94.5%, it caused moderate damage to the resin structure. Therefore, 1.5M hydrochloric acid is the optimal acid for regeneration.
[0082] Comparative Example 4: Optimization of Hydrochloric Acid Concentration in the Acid Transition Regeneration Section Experimental design: With other conditions fixed, investigate the effect of hydrochloric acid concentration in the transformation and regeneration section on vanadium desorption and resin regeneration.
[0083]
[0084] The results show that when the hydrochloric acid concentration increases from 0.5M to 1.5M, the vanadium desorption rate jumps from 38.7% to 92.1%, the resin regeneration rate increases from 72.5% to 98.5%, and the gallium adsorption capacity retention rate reaches 96.2% after 10 cycles. When the concentration continues to increase above 2.0M, although the vanadium desorption rate slightly improves, resin damage intensifies, and cycle stability decreases. 1.5M hydrochloric acid represents the optimal equilibrium point.
[0085] Comparative Example 5: Optimization of NaOH Concentration in the Main Desorption Section Experimental setup: A fixed pre-elution section (1.5N NaOH, 2.5 BV, 35℃) and a transformation and regeneration section (1.5M HCl, 2.5 BV, 25℃) were used to investigate the effects of NaOH concentration in the main desorption section on gallium desorption rate, vanadium desorption rate, and the Ga / V ratio of the main desorption solution. The main desorption section volume was 3.5 BV, and the temperature was 45℃.
[0086] Experimental results:
[0087] The results show that when the NaOH concentration in the main desorption section increases from 3.0N to 7.0N, the Ga desorption rate increases from 32.1% to 46.4%, but the V desorption rate increases sharply from 1.8% to 11.5%, and the Ga / V ratio in the main desorption solution decreases from 32.5:1 to 7.6:1. When the NaOH concentration in the main desorption section is 4.5N, the Ga desorption rate is 44.5%, the V desorption rate is only 4.5%, the Ga / V ratio in the main desorption solution reaches 18.6:1, the resin regeneration rate is 98.2%, and the gallium adsorption capacity retention rate reaches 96.2% after 10 cycles, showing the best overall performance. When the NaOH concentration is below 4.0N, gallium desorption is incomplete, resulting in a low total gallium desorption rate; when the concentration is above 6.0N, the co-desorption of vanadium increases significantly, the Ga / V ratio in the main desorption solution decreases sharply, and resin damage intensifies, leading to reduced cycle stability. Therefore, the NaOH concentration in the main desorption section is preferably 4.0–6.0 N, and more preferably 4.5–5.0 N. In Example 1 of this invention, 4.5 N NaOH was used to achieve the best gallium-vanadium separation effect and resin cycle stability.
[0088] Finally, it should be emphasized that the three-stage gradient desorption of this invention achieves unexpected technical effects compared to traditional single-stage desorption, as shown in the table below:
[0089] The above experimental data fully demonstrates that the three-stage gradient desorption process of this invention—comprising a low-concentration alkali pre-washing vanadium removal stage, a high-concentration alkali main gallium desorption stage, and an acid-based transformation and regeneration stage—achieves excellent results with gallium desorption rate ≥95%, vanadium desorption rate ≥90%, and gallium / vanadium separation efficiency ≥90% through precise matching and synergistic effects of parameters in each stage. Single-stage desorption, two-stage desorption, and other acid solutions cannot simultaneously meet the requirements of high gallium desorption rate, high vanadium removal rate, and high gallium / vanadium separation efficiency. The gradient concentration and staged desorption coupling technology of this invention has significant inventiveness and is irreplaceable.
[0090] The embodiments described herein are preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape, and principle of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor, characterized in that: Includes the following steps: S1. Homogenization and selective chemical conditioning pretreatment of Bayer mother liquor: The Bayer process seed mother liquor is allowed to stand and homogenize, and then transferred to a selective chemical conditioning reactor. The temperature inside the reactor is controlled at 30-40℃, the NaOH concentration is adjusted to 0.8-1.5 mol / L, and the residence time is 30-60 min. S2. Precision filtration pretreatment; S3. Continuous ion exchange adsorption: The purified mother liquor is distributed to ≥4 sets of resin columns connected in series through the feed main; S4. Gradient-segmented desorption: First, pure water is introduced for forward washing. After washing, the three-stage desorption process is performed sequentially: a. Pre-elution stage: The saturated resin is pre-eluted using 2-3 BV, 1-2 N NaOH at 30-40℃; b. Main desorption section: The resin is mainly desorbed using 3-4 BV, 4-6 N NaOH at 40-50℃ to obtain a high-concentration gallium-rich desorption solution; c. Transformation and regeneration section: The resin is deeply transformed and regenerated using 2-3 BV, 1-2 M HCl or H2SO4 at 20-30℃ to obtain vanadium-containing transformation acid solution. S5. Gallium-rich desorption solution electrolytic refining; S6. Transformation of vanadium recovery from acidic solutions.
2. The gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S1, the Bayer process seed mother liquor is allowed to stand for 2-4 hours.
3. The gallium extraction method for selective separation and graded recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S1, a variable frequency feed pump is used at a speed of 2-5m. 3 The mother liquor is fed into the selective chemical conditioning reactor at a constant flow rate of / h.
4. The gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S2, the conditioned mother liquor is fed into a precision filter equipped with a micron-level alkali-resistant filter element, with an operating pressure of 0.1-0.3 MPa and an operating temperature of 30-50℃.
5. The gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S3, the resin column assembly is filled with a methylamine oxime chelating resin.
6. The gallium extraction method for selective separation and graded recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S3, the flow rate of the liquid through the column is controlled at 2-4 BV / h, and the operating temperature is 30-40℃.
7. The gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S5, the control parameters for the electrolytic refining of gallium-rich desorption solution are as follows: cathode current density is 200–800 A / m²; cell voltage is 3.0–4.0 V; electrolysis temperature is 30–50 °C; electrolyte NaOH concentration is 80–150 g / L; electrode distance is 1–3 cm; electrolysis time is 6–12 h. Electrolysis is stopped when the gallium concentration in the electrolyte drops below 1 g / L; the residual electrolyte is returned to the rinsing agent preparation process for reuse.
8. The gallium extraction method for selective separation and graded recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: In step S6, the vanadium-containing conversion acid solution is fed into the vanadium recovery reactor, the pH is adjusted to 2-4 for neutralization and precipitation, the reaction temperature is controlled at 60-90℃, and the reaction time is 1-2 hours to obtain ammonium vanadate precipitate. After solid-liquid separation and calcination, the precipitate is used to obtain vanadium pentoxide product.
9. The gallium extraction method for selective separation and cascade recovery of gallium and vanadium from Bayer mother liquor according to claim 1, characterized in that: All adsorption tail liquid is returned to the alumina plant for reuse in various processes; pre-washing liquid is returned to the adsorption front end for reprocessing; the residual liquid of the conversion acid solution after vanadium recovery is returned to the preparation of the leaching agent; and the residual liquid of electrolysis is returned to the preparation of the leaching agent.