A method for extraction of in-situ leaching uranium in the later stage of neutral acid leaching

By dividing the mining area according to the carbonate content of the ore and selectively using acid mining methods, the problems of low uranium recovery rate in the later stage of carbon-oxygen neutral leaching and the risks of acid mining methods have been solved, achieving efficient recovery and safe mining of uranium resources.

CN123152901APending Publication Date: 2026-11-24BEIJING RESEARCH INSTITUTE OF CHEMICAL ENGINEERING AND METALLURGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611344643.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the later stages of carbon-oxygen neutral leaching mining, uranium mineral residues are difficult to dissolve, resulting in low recovery rates. Furthermore, switching to acid leaching in situ across the entire block can lead to problems such as high acid consumption, formation damage, and pore blockage.

Method used

Based on the carbonate content of the ore, blocks are divided, and acid mining is selectively adopted. Uranium mining is carried out in zones, including acid-tolerant zones, restricted acid-tolerant zones, and prohibited acid-tolerant zones. Mining methods are matched to each zone, and the acidity of acidizing agents and process conditions are optimized.

Benefits of technology

It improved uranium ore recovery rate, reduced acid consumption, avoided formation damage and permeability loss, and achieved safe and efficient uranium resource recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152901A_ABST
    Figure CN123152901A_ABST
Patent Text Reader

Abstract

A method for improving uranium mining by transitioning from neutral to acid leaching in the later stages of in-situ leaching, belonging to the field of sandstone-type uranium mining technology, includes: acquiring production data of a carbon-oxygen neutral leaching stope; when the production data deteriorates, collecting the carbonate content of the ore rock corresponding to each well group within the stope; dividing the stope into subsequent mining zones with different mining methods based on the carbonate content of the ore rock corresponding to each well group; matching corresponding mining methods to each subsequent mining zone and carrying out uranium mining operations in the stope in each zone; wherein, the subsequent mining zone includes an acid-resistant zone, and the carbonate content of the ore rock corresponding to the acid-resistant zone is less than or equal to 2%; the step of matching corresponding mining methods to each subsequent mining zone and carrying out uranium mining operations in the stope in each zone includes: switching the mining process of the acid-resistant zone to acid in-situ leaching, and carrying out uranium mining operations in the acid-resistant zone based on the acid in-situ leaching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of uranium mining technology in sandstone-type uranium deposits, specifically relating to a method for extraction of uranium through neutral-to-acid leaching in the later stages of uranium mining. Background Technology

[0002] Currently, in-situ leaching mining of sandstone-type uranium deposits commonly employs the carbon dioxide-oxygen neutral leaching process, or simply carbon-oxygen neutral leaching. This process relies on oxygen to oxidize tetravalent uranium to hexavalent uranium. The carbon dioxide injected into the ore layer dissolves in the groundwater, generating bicarbonate and carbonate ions, which then complex with uranyl ions to form soluble uranyl carbonate complexes, thus achieving the leaching and migration of uranium minerals. This process is characterized by low reagent costs, mild erosion of formation carbonate minerals, and minimal disturbance to the groundwater environment, and is widely used in the early stages of in-situ leaching uranium mines.

[0003] However, in the later stages of carbon-oxygen neutral leaching, the uranium concentration in the leachate continues to decline, and the uranium yield per unit reagent decreases significantly. A large amount of residual uranium within the ore body cannot be further dissolved through bicarbonate complexation, resulting in an overall uranium recovery rate of only 60% to 80%, limiting resource utilization. Acid in-situ leaching, on the other hand, has a stronger ability to dissolve uranium minerals, achieving a recovery rate of 80% to 90%, making it the preferred method for recovering residual uranium. However, the long-term continuous addition of carbon dioxide in carbon-oxygen neutral leaching leads to the accumulation of high concentrations of bicarbonate in the aquifer, forming a strong buffer system. If the entire block is directly switched to acid in-situ leaching, a large amount of acid reagent will be consumed to neutralize bicarbonate and formation carbonate minerals, causing a surge in acid consumption, difficulty in acidification control, and potential problems such as formation gas production, pore blockage, impaired formation permeability, and acid leakage. Summary of the Invention

[0004] In view of this, this application provides a method for converting neutral to acid leaching in the later stage of in-situ leaching of uranium. The method aims to divide the ore into blocks according to the carbonate content of the ore and selectively switch to acid mining, so as to avoid the formation damage and soaring acid consumption costs caused by blind acidizing the entire area, and improve the recovery rate of residual uranium in the ore body in the later stage of carbon-oxygen neutral leaching.

[0005] To achieve the above objectives, this application mainly provides the following technical solutions: This application provides a method for extracting uranium through a late-stage neutral-to-acid leaching process in in-situ leaching, comprising: Obtain production data from the carbon-oxygen neutral leaching site; When the production data deteriorates, the carbonate content of the corresponding ore rocks in each well group within the mining area is collected; Based on the carbonate content of the ore rocks corresponding to each well group, the mining area is divided into subsequent mining areas with different mining methods; For each of the subsequent mining zones, a corresponding mining method is matched, and uranium mining operations are carried out in the mining area of ​​each zone. The subsequent mining area includes an acid-resistant zone, and the carbonate content of the ore rock corresponding to the acid-resistant zone is less than or equal to 2%. The process of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas includes: The mining process in the acid-resistant zone is switched to in-situ acid leaching, and uranium mining operations in the acid-resistant zone are carried out based on the in-situ acid leaching process.

[0006] Optionally, switching the mining process of the acid-resistant zone to in-situ acid leaching, and conducting uranium mining operations in the acid-resistant zone based on the in-situ acid leaching, includes: Stop or reduce the addition of carbon dioxide used in the neutral carbon-oxygen leaching process in the acidifiable zone; Displacement fluid is introduced into the injection well of the acid-resistant zone to displace the formation groundwater, thereby reducing the formation bicarbonate concentration to a preset range. The acid leaching process is carried out by injecting acidizing agents of different acidities into the injection wells in the acid-resistant zone in stages to reduce acidity; The acid leaching process is stopped when the preset termination condition is met.

[0007] Optionally, the total injection volume of the displacement fluid is 0.3 to 1.5 times the total pore volume of the mineral layer corresponding to the acid-resistant zone.

[0008] Optionally, before the acid leaching process is carried out by injecting acidizing agents of different acidities into the injection wells in the acid-resistant zone, the method further includes: An oxygen-containing acidic pretreatment solution is injected into the injection well in the acid-resistant zone.

[0009] Optionally, the total injection volume of the oxygen-containing acidic pretreatment solution is 0.1 to 0.3 times the total pore volume of the mineral layer corresponding to the acid-resistant zone.

[0010] Optionally, during the acid leaching process, the extraction volume is controlled to be greater than or equal to the injection volume.

[0011] Optionally, during the acid in-situ leaching process, the process parameters of the acid in-situ leaching are monitored, and the process conditions of the acid in-situ leaching are dynamically adjusted based on the process parameters.

[0012] Optionally, switching the mining process of the acid-resistant zone to in-situ acid leaching, and conducting uranium mining operations in the acid-resistant zone based on the in-situ acid leaching, further includes: Neutral fluid is introduced into the injection well in the acid-resistant zone to regulate and remediate the groundwater environment of the acid-resistant zone.

[0013] Optionally, the subsequent mining area may further include a restricted acidification zone, wherein the carbonate content of the ore rock corresponding to the restricted acidification zone is greater than 2% and less than or equal to 3%. The step of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas of each zone also includes: Acidification feasibility tests were conducted in the restricted acidification zone. When the acidizing feasibility test is passed, the mining process in the restricted acidizing zone will be switched to the acid in-situ leaching method, and uranium mining operations in the restricted acidizing zone will be carried out based on the acid in-situ leaching method. The pH control range of the acidifying agent used in the restricted acidification zone and the acidifiable zone during the formal leaching stage is different. The pH control of the acidifying agent in the acidifiable zone during the formal leaching stage is 2.0 to 3.5, while the pH control of the acidifying agent in the restricted acidification zone during the formal leaching stage is 3.5 to 5.0.

[0014] Optionally, the subsequent mining area also includes a prohibited acidification zone, which is the subsequent mining area corresponding to the ore rock with a carbonate content greater than 3% and the restricted acidification zone where the acidification feasibility test has not been passed; The step of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas of each zone also includes: The mining process in the prohibited acidification zone follows the carbon-oxygen neutral leaching process, but with adjusted process conditions. Uranium mining operations in the prohibited acidification zone are carried out based on the adjusted carbon-oxygen neutral leaching process.

[0015] By employing the above technical solution, this application has at least the following beneficial effects: The uranium recovery method for transitioning from neutral to acid leaching in the later stages of in-situ leaching provided in this application effectively solves the problems of difficult residual uranium leaching and low recovery rates in the later stages of traditional carbon-oxygen neutral leaching mining when production data in the mining area deteriorates. It divides the mining area into zones based on the carbonate content of the corresponding ore rocks in each well group and matches appropriate mining methods to different mining zones. Simultaneously, it addresses the problems of excessive acid reagent consumption, formation pore blockage, impaired permeability, difficulty in acid control, and acid boundary violations caused by blindly switching to in-situ acid leaching across the entire block. Furthermore, it employs specific methods for acid-tolerant zones and restricted acid-tolerant zones that have passed acid-tolerant feasibility tests. The decarbonization and graded acid reduction processes, along with differentiated control of acidity ranges for acidizing agents in different blocks, and the optimization and adjustment of carbon-oxygen neutral leaching process conditions in prohibited acid conversion zones, enable the orderly disruption of the original buffer system of the mining strata, the stable oxidation and leaching of residual solid uranium resources within the ore body, and the improvement of uranium resource recovery rate and overall resource utilization rate in the later stages of carbon-oxygen neutral leaching. This also avoids various geological risks and production hazards during in-situ acid leaching, stabilizes ore layer permeability, and reasonably controls the cost of mining reagents, ensuring the safe, efficient, and sustainable recovery of residual uranium resources in sandstone-type uranium mines. Attached Figure Description

[0016] Figure 1 This is a flowchart of a method for extracting uranium from in-situ leaching followed by neutral-to-acid leaching, which is an optional embodiment of this application. Detailed Implementation

[0017] The present application will be described in detail below with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in the embodiments of the present application can be combined with each other.

[0018] This embodiment provides a method for extracting uranium through a neutral-to-acid leaching process in the later stages of in-situ leaching. See [link to relevant documentation]. Figure 1 As shown, the method includes: Step S1: Obtain production data from the carbon-oxygen neutral leaching site.

[0019] The method for recovering uranium from neutral to acid leaching in the later stages of in-situ leaching mining provided in this application embodiment can be applied to the field of in-situ leaching uranium mining in sandstone-type uranium deposits, specifically to the recovery of residual uranium resources in the later stages of carbon-oxygen neutral leaching mining. When performing the recovery of residual uranium resources in the later stages of carbon-oxygen neutral leaching mining, the production data of the carbon-oxygen neutral leaching mining site can first be obtained. Here, the production data of the carbon-oxygen neutral leaching mining site refers to the uranium concentration in the leachate of the carbon-oxygen neutral leaching mining site. The mining site may include multiple well groups, and the production data of the carbon-oxygen neutral leaching mining site can be the uranium concentration in the leachate corresponding to each well group.

[0020] Step S2: When production data deteriorates, collect the carbonate content of the corresponding ore rocks in each well group within the mining area.

[0021] In this embodiment, if the average uranium concentration of the overall leaching solution in a carbon-oxygen neutral leaching stope is below 10 mg / L for 30 to 90 consecutive days, or if the uranium production per unit pumping volume drops to 20% to 30% of the peak value, the production data is considered to have deteriorated, and the carbonate content of the corresponding ore rock in each well group within the stope is then collected.

[0022] It should be noted that the carbonates in the ore can neutralize the acid and form a formation buffer system. The measured carbonate content of the ore is used to divide the mining areas and determine whether the block can be converted to acid leaching mining.

[0023] Here, in order to accurately assess the feasibility of acidizing the block and avoid mining risks such as formation blockage and excessive acid consumption after acidizing, core samples, cuttings, and groundwater samples were collected from each well group. While measuring the carbonate content of the corresponding ore rocks in each well group, acid consumption, clay mineral content, formation permeability coefficient, and the concentrations of bicarbonate, carbonate, calcium ions, magnesium ions, iron, aluminum, sulfate, chloride ions, and uranium ions in the groundwater were simultaneously measured.

[0024] Among them, acid consumption is used to intuitively evaluate the production cost of acid injection in a block; clay mineral content and formation permeability coefficient are used to predict the risk of clay expansion and pore blockage during the acidification process; bicarbonate and carbonate are used to characterize the formation buffer capacity, and the amount of water required to break the buffer can be calculated based on their concentration to determine whether pre-pumping and decarbonization are necessary; calcium and magnesium ions are used to predict the risk of calcium sulfate gypsum scaling and blockage, and when the content is too high, the corresponding block is limited to slow leaching with weak acid; iron and aluminum are used to predict the hidden danger of hydroxide colloid blockage after acidification, and when the content is too high, the acid reduction rate is slowed down by step acidification; sulfate is used to comprehensively control the amount of acid injected in combination with the original background and the incremental acid injection to avoid gypsum supersaturation and precipitation; chloride ions can be used as tracer ions to identify the formation flow of acid liquid, and their content can also be used to predict equipment corrosion and uranium complex stability interference problems; groundwater uranium concentration is used to evaluate the remaining water-soluble uranium reserves and the potential for increased acid production, and when the water body is uranium saturated and the complexing ligands are exhausted, it can be used as the basis for determining the residual uranium in the solid phase of acid conversion activation.

[0025] Step S3: Based on the carbonate content of the corresponding ore rocks in each well group, the stope is divided into subsequent mining areas with different mining methods.

[0026] In this embodiment, the subsequent mining area can be divided into three categories: blocks with a carbonate content of less than or equal to 2% are designated as acid-tolerant zones; blocks with a carbonate content of greater than 2% and less than or equal to 3% are designated as restricted acid-tolerant zones; and blocks with a carbonate content of greater than 3%, as well as restricted acid-tolerant zones where the acid-tolerant feasibility test is not passed, are collectively designated as prohibited acid-tolerant zones.

[0027] It should be noted that limiting the carbonate content of the ore in the acidizing zone to more than 2% poses risks of high acid consumption, excessive formation buffering, and scaling and pore blockage after acidizing. Therefore, an acidizing feasibility test must be conducted before determining the mining plan. This test may include acid consumption testing, dynamic column immersion testing, and well site testing. In this embodiment, a successful acidizing feasibility test is defined as passing all three tests; failure to pass any one test results in a failed test.

[0028] Among them, the acid consumption test is used to calculate the consumption of acidizing agents in the block, while the dynamic column immersion test and well group field test are used to investigate the changes in formation permeability, scaling and blockage, and acid flow under acidizing conditions. In this embodiment, the restricted acidizing zone where the mass of acidizing agent required to process 1 ton of ore is greater than 35 kg or the formation permeability decreases by more than 20% is classified as a prohibited acidizing zone.

[0029] Step S4: Match the corresponding mining method to each subsequent mining zone and carry out uranium mining operations in the mining area.

[0030] In this embodiment, for acid-tolerant zones and restricted acid-tolerant zones where acid-tolerant feasibility tests have been passed, the original mining process is switched to in-situ acid leaching, and uranium mining operations are carried out using in-situ acid leaching. For restricted acid-tolerant zones, the mining process is not switched, and carbon-oxygen neutral leaching continues to be used, with the process conditions of carbon-oxygen neutral leaching being optimized and adjusted. Uranium mining operations in restricted acid-tolerant zones are completed through the optimized carbon-oxygen neutral leaching.

[0031] The process steps for switching from acid-resistant zones to in-situ acid leaching include: stopping or reducing the injection of carbon dioxide used in neutral carbon-oxygen leaching in the acid-resistant zone; introducing displacement fluid into the injection wells of the acid-resistant zone to displace the formation groundwater and reduce the formation bicarbonate concentration to a preset range; injecting acidifying agents of different acidities through the injection wells of the acid-resistant zone in stages to carry out in-situ acid leaching; and stopping in-situ acid leaching when the preset termination conditions are met.

[0032] It should be noted that stopping or reducing carbon dioxide injection can terminate the formation of new bicarbonate ions, avoiding the continuous enhancement of the formation's buffering capacity; injecting replacement fluids to displace groundwater and reduce bicarbonate concentration can break the original buffer system formed by neutral carbon-oxygen leaching, reducing the consumption of subsequent acidizing agents; staged acid reduction and sequential injection of acidizing agents with different acidities can gradually lower the formation pH, avoiding the concentrated precipitation and pore blockage of calcium magnesium sulfate and iron aluminum hydroxide caused by sudden changes in acidity, stabilizing the permeability of the ore layer, and smoothly dissolving solid residual uranium minerals; stopping in-situ acid leaching after reaching the preset termination conditions can promptly end acidizing ore dissolution, avoid excessive acid injection causing acid leakage and precipitation of formation biogenic minerals, and improve the leaching recovery rate of residual uranium resources in the block while controlling mining costs.

[0033] Specifically, after stopping or reducing the injection of carbon dioxide used in neutral carbon-oxygen leaching in the acid-tolerant zone, the well group injection flow rate is simultaneously adjusted to ensure formation hydraulic balance. Decarbonized oxygenated water, low-alkalinity prepared water, or circulating water that has undergone surface aeration to remove carbon dioxide is selected as the replacement fluid, injected through injection wells to displace the formation groundwater. The total injection volume of the replacement fluid is controlled to be 0.3 to 1.5 times the total pore volume of the corresponding ore layer in the acid-tolerant zone. This reduces the formation bicarbonate content to 20% to 40% of the concentration during the stable period of neutral carbon-oxygen leaching, preferably below 500 mg / L, or reduces the mass of acid reagent required to treat 1 ton of ore to below 25 kg. When carrying out graded acid reduction operations, the formation pH is adjusted in three levels sequentially: the first level is controlled between 5.0 and 4.0, the second level... The acidity level is controlled between 4.0 and 3.0 for the first level and between 3.0 and 2.0 for the second level. Each acidity level is operated stably until the monitoring data of pH, acid consumption, uranium concentration, and calcium ion concentration of the leachate show no significant fluctuations before switching to the next acidity level. This avoids precipitation and blockage induced by short-term strong acid impact. During this process, the oxidation-reduction potential is simultaneously adjusted, preferably controlled to be greater than 350mV, to ensure that solid tetravalent uranium in the formation can be successfully oxidized into soluble hexavalent uranium. The preset termination conditions are: for 15 to 30 consecutive days in the stope, the average uranium concentration of the overall leachate in the stope is lower than 10mg / L, or the uranium production corresponding to the unit pumping volume drops to 20% to 30% of the peak value, or the mass of acid reagent required to process 1 ton of ore is greater than 35kg, or the formation permeability decreases by more than 20%.

[0034] Among them, after the acidification feasibility test is passed, the restricted acidification zone is switched to in-situ acid leaching, and the same in-situ acid leaching process steps as the acidifiable zone are adopted. The only restriction is that the pH control range of the acidifying agent used in the formal leaching stage is different between the acidification zone and the acidifiable zone.

[0035] Specifically, in the acid-tolerant zone, the pH range of the acidifying agent during the formal leaching stage is 2.0 to 3.5, while in the restricted acid-tolerant zone, the pH range of the acidifying agent during the formal leaching stage is 3.5 to 5.0. In other words, in the acid-tolerant zone, the acid is gradually reduced, transitioning step-by-step to a final stable pH of 2.0 to 3.5 for the acidifying agent; in the restricted acid-tolerant zone, due to the higher formation carbonate content and stronger buffering capacity, the endpoint of the graded acid reduction is raised, and the pH is gradually adjusted to a stable pH of 3.5 to 5.0 for the acidifying agent.

[0036] Among them, the mining process in the prohibited acid conversion zone adopts carbon-oxygen neutral leaching, and the process conditions of carbon-oxygen neutral leaching are adjusted. Uranium mining operations in the prohibited acid conversion zone are carried out based on the adjusted carbon-oxygen neutral leaching.

[0037] Specifically, considering the high carbonate content and unsuitability for acidification in the ore layers of the prohibited acidification zones, the following optimization methods can be used for carbon-oxygen neutral leaching: extending the carbon-oxygen neutral leaching production cycle, increasing the amount of oxygen injected, implementing local formation clearing or hydraulic fracturing in blocked well sections, optimizing the well group injection system and equivalent well network layout, and supplementing the process with microbial activation and adding complexing agents to enhance leaching in the later stages of mining.

[0038] By applying the technical solution of this embodiment, after the production data of a carbon-oxygen neutral leaching stope deteriorates, the stope is divided into zones based on the carbonate content of the corresponding ore rocks in each well group. Appropriate mining methods are matched to different mining zones, effectively solving the problems of difficult residual uranium leaching and low recovery rates in the later stages of traditional carbon-oxygen neutral leaching. Simultaneously, it solves the problems of excessive acid reagent consumption, formation pore blockage, impaired permeability, difficulty in acid control, and acid boundary violations caused by blindly switching to acid leaching in-situ across the entire block. Furthermore, it addresses the issues of decarbonization and separation in acid-tolerant zones and restricted acid-tolerant zones that have passed acid-tolerant feasibility tests. The process of acid reduction and differentiated control of acidity range of acidizing agents in different blocks, along with optimization and adjustment of carbon-oxygen neutral leaching process conditions in prohibited acid conversion areas to continuously carry out mining operations, can systematically break down the original buffer system of the strata in the mining area, smoothly oxidize and dissolve the solid residual uranium resources inside the ore body, improve the uranium resource recovery rate and overall resource utilization rate in the later stage of carbon-oxygen neutral leaching, avoid various strata risks and production hazards in the process of acid in-situ leaching mining, stabilize the permeability of the ore layer, reasonably control the cost of mining agents, and ensure the safe, efficient and sustainable operation of residual uranium resource mining in sandstone-type uranium mines.

[0039] In some possible embodiments disclosed in this application, before acid leaching is carried out by injecting acidizing agents of different acidities through injection wells in the acid-resistant zone, oxygen-containing acidic pretreatment solution is injected through injection wells in the acid-resistant zone.

[0040] In this embodiment, by injecting acidifying agents of different acidities into the injection wells of the acid-resistant zone in stages before carrying out in-situ acid leaching, an oxygen-containing acidic pretreatment solution is pre-injected. This consumes the remaining bicarbonate buffer in the formation of the acid-resistant zone, avoiding excessive gas and pore disturbance caused by the reaction of local instantaneous strong acid with carbonates. At the same time, acid activation and oxidation pretreatment are completed for the ore layer in the acid-resistant zone, breaking down the residual buffer material in the formation, gently modifying the ore layer environment, ensuring the smooth oxidation and conversion of tetravalent uranium in the formation, improving the leaching efficiency and stability of solid residual uranium resources, avoiding formation blockage caused by sudden changes in acidity, optimizing the in-situ acid leaching operation process, and reducing the production risks of acid mining.

[0041] Among them, the oxygen-containing acidic pretreatment solution can be a weakly acidified solution with a pH range of 5.5 to 6.0. This weakly acidified solution can be prepared by any one or more combinations of sulfuric acid, nitric acid, carbon dioxide water, and organic acids, and the solution contains dissolved oxygen or hydrogen peroxide-like oxidizing components, which have oxidizing and activating properties.

[0042] Specifically, the total injection volume of the oxygen-containing acidic pretreatment solution is 0.1 to 0.3 times the total pore volume of the ore layer corresponding to the acid-tolerant zone.

[0043] In some possible embodiments disclosed in this application, during the acid leaching process, the extraction volume is controlled to be greater than or equal to the injection volume.

[0044] In this embodiment, by setting the pumping volume to be greater than or equal to the injection volume, a hydraulic driving force can be formed pointing towards the injection well, constructing a hydraulic isolation barrier at the boundary of the mining block to prevent the acidizing agent from randomly escaping into the formation outside the mining boundary, locking the effective range of the acidizing agent, avoiding acid from crossing the boundary and polluting the surrounding formation, while continuously maintaining the stability of the hydraulic environment inside the ore layer, ensuring that the acidizing agent penetrates and dissolves the ore uniformly in the target ore layer, reducing the ineffective loss of the acidizing agent, and stabilizing the leaching efficiency of residual uranium minerals.

[0045] Among them, observation wells can be set up around the outer perimeter of the mining block to monitor the pH of the well water in real time by taking water samples and testing the water quality. The monitoring data from the observation wells can be used to help verify the actual blocking effect of the hydraulic barrier.

[0046] Specifically, when abnormal fluctuations occur in the monitored values, the pH of the acidifying agent can be increased and the amount of liquid drawn can be increased.

[0047] In some possible embodiments disclosed in this application, during the process of acid in-situ leaching, the process parameters of acid in-situ leaching are monitored, and the process conditions of acid in-situ leaching are dynamically adjusted based on the process parameters.

[0048] In this embodiment, by monitoring the process parameters of acid in-situ leaching in real time or periodically and dynamically adjusting the process conditions of acid in-situ leaching based on the process parameters, it is possible to control the acidification reaction and seepage changes within the ore layer, suppress the continuous development of abnormal conditions such as scaling and pore blockage, and sudden increase in acid consumption, suppress formation damage, and ensure that the entire acid in-situ leaching process is stable and controllable.

[0049] The process parameters include formation pH, redox potential, conductivity, uranium ion concentration, calcium ion concentration, magnesium ion concentration, iron ion concentration, aluminum ion concentration, sulfate concentration, fluid turbidity, fluid suspended matter content, and well pressure.

[0050] Specifically, for example, when the concentration of calcium ions in the formation is higher than 1000 mg / L, or the concentration of magnesium ions is higher than 500 mg / L, or the concentration of iron ions is higher than 100 mg / L, or the concentration of aluminum ions is higher than 100 mg / L, or the well pressure increases by 20% to 30%, the concentration of the acidizing agent is reduced, the pH of the primary acidizing agent is increased, and if necessary, an organic complex acid is used to prepare the acidizing agent, in conjunction with control measures such as pulse injection, suspension of injection for natural diffusion, or backflushing of the well section.

[0051] In some possible embodiments disclosed in this application, the process steps corresponding to switching the acid-resistant zone to in-situ acid leaching also include: introducing neutral fluid through the injection well in the acid-resistant zone to regulate and remediate the groundwater environment of the acid-resistant zone.

[0052] In this embodiment, after the acid leaching process is completed, neutral fluid is introduced through the injection well in the acid-resistant zone to regulate and restore the groundwater environment in the acid-resistant zone. This can neutralize residual acidic substances in the formation, reduce the content of sulfate and various metal ions in the formation, restore the original pH and water composition of the formation, improve the pore environment of the ore layer, reduce the long-term pollution risks of the formation caused by residual acidizing agents, and allow the groundwater in the mining area to return to its natural physical and chemical state.

[0053] The neutral fluid can be neutral oxygenated water, low-concentration bicarbonate brine, or purified in-situ groundwater. Continuous injection of the neutral fluid helps raise the pH of the pumping well to 6.0 to 8.5. It should be noted that under conditions requiring high formation water remediation, alkalinity adjusting fluid, reducing adjusting fluid, or adsorption-precipitation adjusting fluid can be added to accelerate the restoration of the formation groundwater's chemical composition.

[0054] It will be readily understood by those skilled in the art that the aforementioned advantageous methods can be freely combined and superimposed without conflict.

[0055] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of this application, and these improvements and modifications should also be considered within the protection scope of this application.

Claims

1. A method for extracting uranium through a late-stage neutral-to-acid leaching process in in-situ leaching, characterized in that, include: Obtain production data from the carbon-oxygen neutral leaching site; When the production data deteriorates, the carbonate content of the corresponding ore rocks in each well group within the mining area is collected; Based on the carbonate content of the ore rocks corresponding to each well group, the mining area is divided into subsequent mining areas with different mining methods; For each of the subsequent mining zones, a corresponding mining method is matched, and uranium mining operations are carried out in the mining area of ​​each zone. The subsequent mining area includes an acid-resistant zone, and the carbonate content of the ore rock corresponding to the acid-resistant zone is less than or equal to 2%. The process of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas includes: The mining process in the acid-resistant zone is switched to in-situ acid leaching, and uranium mining operations in the acid-resistant zone are carried out based on the in-situ acid leaching process.

2. The method according to claim 1, characterized in that, The step of switching the mining process of the acid-resistant zone to in-situ acid leaching, and carrying out uranium mining operations in the acid-resistant zone based on the in-situ acid leaching method, includes: Stop or reduce the addition of carbon dioxide used in the neutral carbon-oxygen leaching process in the acidifiable zone; Displacement fluid is introduced into the injection well of the acid-resistant zone to displace the formation groundwater, thereby reducing the formation bicarbonate concentration to a preset range. The acid leaching process is carried out by injecting acidizing agents of different acidities into the injection wells in the acid-resistant zone in stages to reduce acidity; The acid leaching process is stopped when the preset termination condition is met.

3. The method according to claim 2, characterized in that, The total injection volume of the replacement fluid is 0.3 to 1.5 times the total pore volume of the mineral layer corresponding to the acid-resistant zone.

4. The method according to claim 2, characterized in that, Before the acid leaching process is carried out by injecting acidizing agents of different acidities into the injection wells in the acid-resistant zone, the method further includes: An oxygen-containing acidic pretreatment solution is injected into the injection well in the acid-resistant zone.

5. The method according to claim 4, characterized in that, The total injection volume of the oxygen-containing acidic pretreatment solution is 0.1 to 0.3 times the total pore volume of the mineral layer corresponding to the acid-resistant zone.

6. The method according to claim 2, characterized in that, During the acid leaching process, the volume of liquid extracted should be greater than or equal to the volume of liquid injected.

7. The method according to claim 2, characterized in that, During the acid in-situ leaching process, the process parameters of the acid in-situ leaching are monitored, and the process conditions of the acid in-situ leaching are dynamically adjusted based on the process parameters.

8. The method according to claim 2, characterized in that, The step of switching the mining process of the acid-resistant zone to in-situ acid leaching, and carrying out uranium mining operations in the acid-resistant zone based on the in-situ acid leaching method, further includes: Neutral fluid is introduced into the injection well in the acid-resistant zone to regulate and remediate the groundwater environment of the acid-resistant zone.

9. The method according to claim 1, characterized in that, The subsequent mining area also includes a restricted acidification zone, wherein the carbonate content of the ore rock corresponding to the restricted acidification zone is greater than 2% and less than or equal to 3%; The step of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas of each zone also includes: Acidification feasibility tests were conducted in the restricted acidification zone. When the acidizing feasibility test is passed, the mining process in the restricted acidizing zone will be switched to the acid in-situ leaching method, and uranium mining operations in the restricted acidizing zone will be carried out based on the acid in-situ leaching method. The pH control range of the acidifying agent used in the restricted acidification zone and the acidifiable zone during the formal leaching stage is different. The pH control of the acidifying agent in the acidifiable zone during the formal leaching stage is 2.0 to 3.5, while the pH control of the acidifying agent in the restricted acidification zone during the formal leaching stage is 3.5 to 5.

0.

10. The method according to claim 9, characterized in that, The subsequent mining area also includes a prohibited acidification zone, which is the subsequent mining area with a carbonate content of more than 3% and the restricted acidification zone where the acidification feasibility test has not been passed. The step of matching corresponding mining methods to each of the subsequent mining zones and carrying out uranium mining operations in the mining areas of each zone also includes: The mining process in the prohibited acidification zone follows the carbon-oxygen neutral leaching process, but with adjusted process conditions. Uranium mining operations in the prohibited acidification zone are carried out based on the adjusted carbon-oxygen neutral leaching process.