Method of improving strength of heat affected zone of 6xxx series aluminum alloy weld joints, alloys, and products

By adding 0.1%-0.6% pure zinc to 6XXX series aluminum alloys and combining it with specific processing techniques, the problem of insufficient strength in the heat-affected zone of welded joints was solved, resulting in increased weld penetration, improved joint strength, and enhanced welding efficiency, while reducing welding costs.

CN123152906APending Publication Date: 2026-11-24WEIQIAO LIGHTWEIGHT RESEARCH CENTER AT SOOCHOW +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611540924.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

When welding 6XXX series aluminum alloys, the strength of the heat-affected zone of the weld joint is significantly reduced, which limits the structural safety and service life. Existing technologies are unable to effectively solve this problem.

Method used

Adding 0.1%-0.6% pure zinc to aluminum alloys and controlling the temperature and holding time during the casting process allows the zinc to dissolve uniformly in the aluminum melt. Combined with high-purity argon gas purification and degassing, as well as subsequent homogenization, hot extrusion, and T5 treatment, welding parameters are optimized to reduce welding heat input.

Benefits of technology

It significantly improves weld penetration and joint strength, reduces strength loss in the heat-affected zone, enhances welding efficiency, and lowers costs. Zinc is a safe and inexpensive element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152906A_ABST
    Figure CN123152906A_ABST
Patent Text Reader

Abstract

This invention discloses a method, alloy, and product for improving the heat-affected zone strength of 6XXX series aluminum alloy welded joints. The method includes at least the following steps: preparing 6XXX series aluminum alloy and 0.1%-0.6% pure zinc by mass; melting and casting the 6XXX series aluminum alloy, adding pure zinc after the temperature of the molten metal reaches 720-750℃ and holding at that temperature. This invention reduces the surface tension of the aluminum molten metal by dissolving a certain amount of Zn in the weld pool, making it easier for the molten wire droplets to excessively penetrate the molten pool during MIG welding. Under the same welding conditions, this increases the weld penetration depth, improves welding speed, reduces welding heat input, and improves welding quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy technology, specifically relating to a method, alloy, and product for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints. Background Technology

[0002] 6XXX series (Al-Mg-Si series) aluminum alloys are typical heat-treatable aluminum alloys, possessing advantages such as excellent formability, medium-to-high strength, and good corrosion resistance. They are among the most widely used and produced aluminum alloy series. However, 6XXX series aluminum alloys suffer from joint softening during welding. This occurs when the nanoscale precipitates generated by age-strengthening in the aluminum alloy coarsen after welding, significantly reducing the mechanical properties of the heat-affected zone of the joint. The joint strength is only about 60% of that of the base metal, directly impacting the safety and lifespan of the structure and greatly limiting its application scenarios. Currently, solutions to the softening problem of aluminum alloy welded joints mainly focus on three core directions: controlling heat input, post-weld heat treatment, and optimizing weld microstructure.

[0003] First, controlling heat input typically employs novel welding processes such as laser welding or laser-arc hybrid welding, which can effectively reduce heat input and improve joint strength. However, these new equipment are expensive, leading to high production costs. Second, post-weld heat treatment can effectively restore the mechanical properties of the alloy, but for some large components, deformation may occur after heat treatment, thus limiting its application. Finally, optimizing weld microstructure can be achieved through developing new welding wires, coating the weld surface with activators, and using ultrasonic vibration to increase weld penetration.

[0004] The closest techniques involve using surfactants or ultrasonic vibration to increase weld penetration. Details are as follows:

[0005] (1) Before TIG welding, a surfactant is applied to the surface of the material. The surfactant is a mixture of Cr2O3 powder, TiO2 powder and La2O3 powder. During welding, the heat source of the welding arc is more concentrated and the weld penetration depth is increased.

[0006] (2) Add an ultrasonic impactor next to the CMT welding torch. The ultrasonic vibration causes the molten metal in the welding pool to flow, thereby increasing the welding penetration.

[0007] Therefore, in order to address the above-mentioned technical problems, it is necessary to provide a method, alloy, and product for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints. Summary of the Invention

[0008] The purpose of this invention is to provide a method, alloy, and product for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints.

[0009] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:

[0010] A method for improving the heat-affected zone strength of welded joints of 6XXX series aluminum alloys includes at least the following steps: preparing 6XXX series aluminum alloys and pure zinc accounting for 0.1%-0.6% of its mass; melting and casting the 6XXX series aluminum alloys, adding pure zinc after the temperature of the melt reaches 720-750℃ and holding it at that temperature.

[0011] In one or more embodiments of the present invention, the holding time for the heat preservation operation is 30-50 minutes. The heat preservation conditions in this scheme are used to ensure that pure zinc is fully dissolved and uniformly diffused in the aluminum melt. When the temperature is below 720°C, the viscosity of the aluminum melt increases, the zinc dissolution rate slows down, and local Zn enrichment and compositional segregation easily occur in the melt; when the temperature is above 750°C, zinc oxidation and burn-off intensify, the melt's gas absorption tendency increases, and the risk of ingot inclusions and porosity increases. When the holding time is less than 30 minutes, zinc is difficult to distribute uniformly in the melt; after 50 minutes, the homogenization effect is limited, and energy consumption and burn-off increase instead. Preferably, the present invention involves holding at 750°C for 30 minutes, resulting in a uniform Zn distribution in the ingot, and a stable and repeatable improvement in weld penetration and post-weld strength.

[0012] In one or more embodiments of the present invention, the pure zinc addition method is any of the following:

[0013] The three methods of adding pure zinc are as follows: 1) Adding pure zinc ingots to the melt in one go; 2) Adding pure zinc wire with a diameter of 1-3 mm within a range from the center to 1 / 2R off-center of the molten pool, where R is the average distance from the center to the edge of the molten pool; 3) Blowing pure zinc powder into the melt with high-purity argon gas to a depth of 3-8 cm. These methods adapt to different production scales, equipment conditions, and requirements for compositional uniformity. Adding pure zinc ingots in one go is simple to operate, highly efficient, and suitable for mass production. Adding pure zinc wire with a diameter of 1-3 mm within a range from the center to 1 / 2R off-center of the molten pool utilizes melt convection to accelerate dissolution and prevent localized zinc accumulation. Blowing pure zinc powder into the melt with high-purity argon gas (to a depth of 3-8 cm) results in the most uniform dispersion of zinc powder in the melt, rapid dissolution, and high yield, suitable for applications requiring high compositional uniformity. All three methods ensure uniform zinc distribution in the melt, achieving consistent increases in melt depth and post-weld strength, and are highly adaptable to industrial applications.

[0014] In one or more embodiments of the present invention, the particle size of the pure zinc powder is 50-500 micrometers, and the flow rate of the high-purity argon gas used for blowing is 1-3 L / min. This scheme controls the particle size of the pure zinc powder to 50-500 micrometers and the argon gas flow rate to 1-3 L / min to ensure that the zinc powder can be stably blown to a predetermined depth (3-8 cm) inside the melt and melt rapidly. When the particle size is less than 50 micrometers, the zinc powder is easily carried to the surface of the melt by the argon gas flow, increasing oxidation loss; when the particle size is greater than 500 micrometers, the zinc powder settles quickly and tends to accumulate at the bottom of the melt, resulting in incomplete dissolution. When the argon gas flow rate is less than 1 L / min, the blowing power is insufficient, and the zinc powder cannot reach the predetermined depth; when it is greater than 3 L / min, the melt is violently agitated, increasing the risk of gas intake and inclusions. Within the above ranges, the zinc yield and dispersion uniformity are optimal.

[0015] In one or more embodiments of the present invention, the melt is further purified and degassed with high-purity argon gas after heat preservation.

[0016] In one or more embodiments of the present invention, the purity of the high-purity argon gas during purification and degassing is not less than 5N.

[0017] In one or more embodiments of the present invention, high-purity argon gas is blown by a graphite rotor for purification and degassing. The blowing of high-purity argon gas meets the following requirements: argon gas flow rate of 15-20 L / min and argon gas pressure of 1.2-3.0 atm. Simultaneously, the graphite rotor is stirred at a speed of 400 r / min for 25 min. This method uses high-purity argon gas with a purity of not less than 5N to purify and degas the melt after heat preservation, which can significantly reduce the hydrogen content of the melt, remove oxide inclusions, reduce weld porosity and other defects, and ensure weld density and joint mechanical properties. Using a graphite rotor for blowing, with an argon gas flow rate of 15-20 L / min and a pressure of 1.2-3.0 atm, combined with rotor stirring at 400 r / min for 25 min, efficient degassing can be achieved without introducing contamination into the melt. All embodiments of the present invention use the above-mentioned purification and degassing parameters, resulting in ingots with high density, good weld formation after welding, low porosity, and stable joint performance.

[0018] In one or more embodiments of the present invention, the process further includes, in sequence: homogenization treatment, hot extrusion processing, and T5 treatment. Homogenization treatment involves holding the ingot at 540-560℃ for 10-16 hours, followed by air cooling. Hot extrusion processing involves hot extrusion at 460℃-520℃ after homogenization, with an extrusion ratio controlled at 30-50. After hot extrusion, T5 treatment is performed, i.e., air cooling + artificial aging, with an aging temperature of 170-180℃ and a holding time of 6-10 hours. This scheme uses homogenization treatment (holding at 540-560℃ for 10-16 hours) to eliminate as-cast dendritic segregation, dissolve coarse phases, and improve subsequent extrusion processability and aging response; hot extrusion processing (460-520℃, extrusion ratio 30-50) to refine the microstructure and increase density; and T5 treatment (air cooling after hot extrusion + artificial aging at 170-180℃ for 6-10 hours) to obtain a stable and sufficiently age-strengthened microstructure. The above-mentioned post-processing chain, in synergy with the Zn addition scheme, enables the base material to achieve a good balance of strength and toughness—in this embodiment of the invention, the base material has a yield strength of 360-366 MPa and a tensile strength of 385-392 MPa—and ensures that the strength loss in the heat-affected zone after welding is minimized.

[0019] In one or more embodiments of the present invention, the 6XXX series aluminum alloy is prepared by the aforementioned method for improving the strength of the heat-affected zone of the welded joint of the 6XXX series aluminum alloy.

[0020] In one or more embodiments of the present invention, the welded product is obtained by welding a profile made of the aforementioned 6XXX series aluminum alloy. Preferably, it is obtained by MIG welding, with a welding heat input not exceeding 10. 2 J / mm, welding speed is 8-10mm / s.

[0021] Compared with existing technologies, the method, alloy, and products of this invention for improving the strength of the heat-affected zone (HAZ) of 6XXX series aluminum alloy welded joints mainly achieve this by dissolving a certain amount of Zn in the molten aluminum alloy weld pool, reducing the surface tension of the aluminum molten metal. This allows the molten wire droplets to more easily transition into the molten pool during MIG welding, resulting in increased weld penetration under the same welding conditions. Therefore, welding speed can be increased while ensuring complete weld penetration, and welding heat input can be reduced. The reduced heat input lowers the peak temperature of the HAZ, shortens the high-temperature dwell time, and inhibits the coarsening and re-dissolution of Mg2Si nano-precipitates (β″ / β′), significantly alleviating the softening of the HAZ strength. Simultaneously, Zn metal raw materials are inexpensive, and compared to Li and Ce, they do not pose high costs, flammability, or explosion risks, making them highly adaptable for industrial applications. Attached Figure Description

[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0023] Figure 1 The following are cross-sectional topographic images of alloy welds in one embodiment of the present invention: (a) Comparative Example A1; (b) Example A1; (c) Comparative Example A2; (d) Example A2; (e) Example A3; (f) Example A4; (g) Example A5; (h) Example A6;

[0024] Figure 2 The following are cross-sectional morphological diagrams of welds of different alloys in one embodiment of the present invention: (a) Comparative Example A3; (b) Comparative Example A4; (c) Example A7; (d) Example A8; (e) Example A9; (f) Example A10; (g) Example A11; (h) Example A12. Detailed Implementation

[0025] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments disclosed herein. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.

[0026] The 6XXX series aluminum alloy of this invention exhibits lower surface tension during welding. The molten droplets formed by the melting of the welding wire are more easily introduced into the molten pool under the influence of the arc force, resulting in a greater weld penetration. Therefore, complete penetration can be achieved simply by reducing the heat input. With reduced heat input, the peak temperature experienced by the base material decreases, the high-temperature time is shortened, the coarsening degree of the nano-precipitates is reduced, and the joint strength loss is lessened, thereby improving the post-weld strength of the alloy.

[0027] To address the issue of softening in the weld and heat-affected zone during the welding of 6XXX series aluminum alloys, this invention provides a method for improving the strength of the heat-affected zone of welded joints: by adding specific elements to the alloy, optimizing the physical properties of the alloy during welding, reducing the surface tension of the melt, thereby reducing the welding heat input, solving the problem of coarsening, dissolution, and transformation of strengthening phases in the heat-affected zone of aluminum alloy welding, and ultimately improving the weld formability and mechanical properties of the joint.

[0028] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0029] Before casting, 0.1%-0.6% pure zinc was weighed out of the 6XXX series alloys, keeping the proportions of other alloying elements constant. During alloy casting, after the melt temperature reached 750℃, the weighed pure zinc was added to the alloy melt and stirred thoroughly. After the pure Zn was completely dissolved, the mixture was held at this temperature for 30-50 minutes to ensure uniform dissolution of the pure Zn into the aluminum melt. The melt was then purified with high-purity argon gas and subjected to DC casting to obtain Zn-containing aluminum alloy ingots. These ingots were then subjected to homogenization, hot extrusion, and T5 treatment to obtain T5-state aluminum alloy profiles. The T5-state aluminum alloy profiles were cut, ground to remove the surface oxide film, and cleaned with alcohol to remove oil stains. Welding parameters were then set, and MIG welding experiments were conducted. Welding voltage and current were set conventionally, but the welding speed was higher than that of the alloy without Zn, resulting in lower heat input during welding. After welding, a better weld structure and joint strength can be obtained than that of the alloy without Zn.

[0030] Principle: Zinc has a lower surface tension than aluminum. A small amount of Zn (0.1-0.6 wt.%) dissolved in molten aluminum helps reduce the overall surface tension of the system. For alloys with added Zn, during welding, the molten droplets formed by the melting of the welding wire under the action of the arc force more easily enter the molten pool, resulting in a deeper weld. Therefore, by increasing the welding speed to reduce heat input, complete weld penetration can be achieved, resulting in a narrower weld and a better weld microstructure. With reduced heat input, the peak temperature experienced by the base metal decreases, the high-temperature time is shortened, the coarsening degree of nano-precipitates in the alloy decreases, and the joint strength loss is reduced, thus improving the post-weld strength of the alloy.

[0031] Group 1

[0032] Comparative Example A1

[0033] For a 6XXX series aluminum alloy, the alloy composition is Si: 0.9%, Fe: 0.07%, Cu: 0.45%, Mn: 0.6%, Mg: 0.9%, Cr: 0.1%, Ti: 0.08%, with the balance being Al and unavoidable impurity elements. Based on this composition, the alloy is formulated and cast using a conventional process. The melt is purified and degassed using a graphite rotor blowing high-purity argon gas, with the following conditions met: argon flow rate 15 L / min, argon pressure 1.5 atm. Simultaneously, the graphite rotor is used for stirring at a speed of 400 r / min, and the purification and degaussing time is 25 min. Before casting, Al-5Ti-B is added to refine the grain size, and then the aluminum alloy ingot is obtained through casting. Aluminum alloy ingots were sequentially subjected to homogenization, hot extrusion, and T5 treatment to obtain T5-state aluminum alloy profiles. Homogenization involved holding the ingot at 540℃ for 10 hours followed by air cooling. Hot extrusion was performed after homogenization at 460℃ with an extrusion ratio controlled at 30. The T5 treatment involved aging at 170℃ for 6 hours, followed by air cooling to room temperature. The T5 profiles were cut into plates 200mm long, 100mm wide, and 3mm thick. The surface oxide film was removed by grinding, and oil stains were cleaned with anhydrous ethanol. MIG welding tests were then conducted using set welding parameters. ER5356 welding wire was used, the shielding gas was high-purity argon with a flow rate of 20L / min, a wire feed speed of 3.5m / min, a welding speed of 8mm / s, and an arc current of 170% of the rated current. The calculated welding heat input was 80.4J / mm².

[0034] Example A1

[0035] Unlike Comparative Example A1, Example A1 incorporated 0.35 wt.% Zn into the alloy composition, while maintaining the content of other alloying elements unchanged. During casting, after the melt temperature reached 750°C, the weighed pure zinc block was added to the alloy melt and stirred evenly. After the pure Zn was completely dissolved, the mixture was kept at this temperature for 30 minutes to ensure that the pure Zn dissolved uniformly into the aluminum melt. Subsequent processing and welding were the same as in Comparative Example A1 (wire feed speed 3.5 m / min, welding speed 8 mm / s), and the calculated welding heat input was 80.4 J / mm.

[0036] Comparative Example A2

[0037] Unlike Comparative Example A1, the wire feed speed in Comparative Example A2 is 4.0 m / min, and the calculated welding heat input is 99.3 J / mm.

[0038] Example A2

[0039] Unlike Comparative Example A2, Example A2 added 0.1 wt.% Zn to the alloy composition while keeping the contents of other alloying elements unchanged.

[0040] Example A3

[0041] Unlike Comparative Example A2, Example A3 added 0.23 wt.% Zn to the alloy composition while keeping the contents of other alloying elements unchanged.

[0042] Example A4

[0043] Unlike Comparative Example A2, Example A4 added 0.35 wt.% Zn to the alloy composition while keeping the contents of other alloying elements unchanged.

[0044] Example A5

[0045] Unlike Comparative Example A2, Example A5 added 0.48 wt.% Zn to the alloy composition while keeping the contents of other alloying elements unchanged.

[0046] Example A6

[0047] Unlike Comparative Example A2, Example A6 added 0.6 wt.% Zn to the alloy composition while keeping the contents of other alloying elements unchanged.

[0048] Comparative Example A3

[0049] Unlike Comparative Example A1, Comparative Example A3 has a wire feeding speed of 4.5 m / min, a welding speed of 8 mm / s, and a calculated welding heat input of 114.8 J / mm.

[0050] Comparative Example A4

[0051] Unlike Comparative Example A1, Comparative Example A4 has a wire feeding speed of 4.5 m / min, a welding speed of 9 mm / s, and a calculated welding heat input of 102.0 J / mm.

[0052] Example A7

[0053] Unlike Comparative Example A4, Example A7 contains 0.1 wt.% Zn in its alloy composition.

[0054] Example A8

[0055] Unlike Comparative Example A4, 0.23 wt.% Zn was added to the alloy composition in Example A8.

[0056] Example A9

[0057] Unlike Comparative Example A3, 0.35 wt.% Zn was added to the alloy composition in Example A9.

[0058] Example A10

[0059] Unlike Comparative Example A4, Example A10 contains 0.35 wt.% Zn in its alloy composition.

[0060] Example A11

[0061] Unlike Comparative Example A4, 0.48 wt.% Zn was added to the alloy composition in Example A11.

[0062] Example A12

[0063] Unlike Comparative Example A4, Example A12 contained 0.6 wt.% Zn in its alloy composition.

[0064] Comparative Example A5

[0065] Unlike Comparative Example A2, Comparative Example A5 contained 0.05 wt.% Zn in its alloy composition.

[0066] Comparative Example A6

[0067] Unlike Comparative Example A2, Comparative Example A6 contains 0.7 wt.% Zn in its alloy composition.

[0068] In the above embodiments and comparative examples, after welding, the cross-sectional data of the weld were statistically analyzed, and three cross-sections were measured and their average values ​​were calculated. The methods for measuring weld penetration / width (metallographic method and sampling section location) and the mechanical property testing standard GB / T228.1 were used, and the improvement was calculated as (value after adding Zn - value without adding Zn) ÷ value without adding Zn × 100%.

[0069] Figure 1 The cross-sectional morphology of the alloy weld and the weld penetration data are shown in Table 1. It can be concluded that: in Comparative Example A1 without Zn, the average weld penetration was 0.86 mm; in Example A1, with the addition of 0.35 wt.% Zn, the average weld penetration increased to 0.93 mm, an improvement of 8.1% compared to Comparative Example A1. In Comparative Example A2 without Zn, the average weld penetration was 1.39 mm; in Examples A2-6, the addition of a certain amount of Zn resulted in a certain increase in weld penetration. In particular, when the Zn content was 0.35%, the average weld penetration increased to 1.73 mm, an improvement of 24.5% compared to Comparative Example A1.

[0070] Table 1 Weld Penetration of Alloys

[0071]

[0072] Table 1 also shows that: at a wire feed speed of 3.5 m / min (heat input 80.4 J / mm), after adding 0.35% Zn in Example A1, the average weld penetration increased from 0.86 mm in Comparative Example A1 to 0.93 mm, an increase of 8.1%; at a wire feed speed of 4.0 m / min (heat input 99.3 J / mm), after adding 0.1%-0.6% Zn in Examples A2-6, the average weld penetration increased from 1.39 mm in Comparative Example A2 to 1.55 mm, 1.57 mm, 1.73 mm, 1.70 mm, and 1.68 mm, respectively, with increases of 11.5%, 12.9%, 24.5%, 22.3%, and 20.9%. It is evident that under identical welding parameters, the addition of Zn significantly increases the weld penetration, with the largest increase (24.5%) observed at a Zn content of 0.35%. Approximately 0.35% is the preferred Zn content for this invention. The increased weld penetration means that a higher welding speed can be used while ensuring complete penetration, thus creating conditions for further reducing welding heat input and mitigating softening of the heat-affected zone.

[0073] Figure 2 Table 2 shows the weld cross-sectional morphology for different alloys, with average upper / lower weld widths. Figure 2 (b) shows the weld cross-sectional morphology of Comparative Example A4, with a welding speed of 9 mm / s. After reducing the heat input, the alloy did not fully penetrate. In contrast, Example A10 (containing Zn), under the same welding speed of 9 mm / s and with reduced heat input, achieved complete weld penetration and a better weld morphology. Its strength was also improved, with a yield strength of 151.1 MPa and a tensile strength of 242.8 MPa, demonstrating superior post-weld strength.

[0074] Furthermore, the upper and lower weld widths of Examples A7-12 were narrower than those of Comparative Example A3 (Comparative Example A3: upper 7.90 mm / lower 6.60 mm; Examples A7-12: upper 7.37-7.85 mm, lower 5.68-6.27 mm). Among them, Examples A7, 8, 10, 11, and 12 changed from incomplete penetration in Comparative Example A4 to complete penetration at 9 mm / s (102.0 J / mm), exhibiting better weld morphology and a smaller heat-affected zone width. The strength of the alloy base material and the post-weld strength are shown in Table 3. The addition of 0.1%-0.6% Zn to the alloy also improved the post-weld strength to a certain extent.

[0075] As further shown in Table 2, the average upper / lower weld width of Comparative Example A3 (without Zn, welding speed 8 mm / s) was 7.90 / 6.60 mm. After adding 0.1%-0.6% Zn to Examples A7-12, the average upper weld width narrowed to 7.37-7.85 mm, and the average lower weld width narrowed to 5.68-6.27 mm. Example A10 (0.35% Zn, 9 mm / s) had the narrowest weld width (upper weld width 7.62 mm, lower weld width 5.68 mm), with the lower weld width being 13.9% narrower than Comparative Example A3. The narrower weld width indicates a reduction in the heat-affected zone (HAZ) of the base material during welding, resulting in a smaller HAZ width. As shown in Table 3, compared with the fully penetrated Comparative Example A3 (yield strength of 132.7 MPa and tensile strength of 214.8 MPa in the heat-affected zone), the yield strength of the heat-affected zone in Examples A7-12 was increased to 140.5-151.1 MPa (an increase of 5.9%-13.9%), and the tensile strength was increased to 223.1-242.8 MPa (an increase of 3.9%-13.0%). Among them, the yield strength of 151.1 MPa and the tensile strength of 242.8 MPa in the heat-affected zone in Example A10 were the best. Examples A10 and A9 used the same alloy (0.35% Zn). After increasing the welding speed from 8 mm / s to 9 mm / s and decreasing the heat input from 114.8 J / mm to 102.0 J / mm, the yield strength of the heat-affected zone increased from 143.0 MPa to 151.1 MPa (an increase of 5.7%), and the tensile strength increased from 225.0 MPa to 242.8 MPa (an increase of 7.9%), directly verifying the technical path of "reducing heat input → suppressing precipitate coarsening → alleviating heat-affected zone softening." Furthermore, Comparative Example A4 (without Zn, 9 mm / s) showed incomplete weld penetration and substandard weld quality, while Examples A7-12 all achieved complete penetration under the same welding parameters. This indicates that adding Zn allows for higher welding speeds and lower welding heat inputs without sacrificing weld quality.

[0076] Table 2 Alloy Weld Width Table

[0077]

[0078] Table 3 Mechanical properties of alloy base material and after welding

[0079]

[0080] In summary, the addition of Zn results in a greater weld penetration depth. This is primarily because Zn reduces the surface tension of the alloy melt, allowing molten droplets formed by the melting wire to more easily enter the weld pool under the influence of the arc force. When the welding speed increases from 8 mm / s to 9 mm / s, the welding heat input decreases from 114.8 J / mm to 102.0 J / mm, the peak temperature experienced by the base metal decreases, the high-temperature time is shortened, the coarsening degree of nano-precipitates in the alloy decreases, and the joint strength loss is reduced, thus improving the post-weld strength of the alloy. In conclusion, the addition of Zn to the alloy results in a greater weld penetration depth and narrower weld width, with a better weld morphology. Simultaneously, higher welding speeds can be used, and the increased welding speed reduces heat input, leading to higher post-weld strength of the alloy.

[0081] Furthermore, the addition of Zn reduces the surface tension of the molten aluminum, making it easier for the molten wire droplets to transition into the weld pool during welding: under the same welding parameters, the weld penetration depth is increased by 8.1%-24.5% (optimal at 0.35% Zn, reaching 24.5%); while ensuring complete penetration, the welding speed can be increased from 8 mm / s to 9 mm / s, and the welding heat input is reduced from 114.8 J / mm to 102.0 J / mm (a reduction of 11.1%). The peak temperature of the heat-affected zone is reduced, the high-temperature dwell time is shortened, and the coarsening and re-dissolution of Mg2Si nano-precipitates are suppressed. The yield strength of the heat-affected zone is increased by 5.9%-13.9%, and the tensile strength is increased by 3.9%-13.0%; at the same time, the upper / lower weld width is narrowed (the lower weld width is reduced by a maximum of 13.9%), the width of the heat-affected zone is reduced, the weld formability, density, and joint reliability are improved, welding efficiency is increased, and welding costs are reduced.

[0082] Group 2: The difference between this group's examples and Example A4 is as follows: After the melt temperature reaches the addition temperature, the weighed pure zinc block is added to the alloy melt, stirred evenly, and kept at the temperature after the pure Zn is completely dissolved.

[0083]

[0084] After welding, the cross-sectional data of the weld were statistically analyzed for the samples in the above embodiments and comparative examples. Three cross-sections were measured and their average values ​​were calculated. The weld penetration data are shown in the table below.

[0085]

[0086] Group 3: The difference between this group's embodiments and Embodiment A4 is as follows: the addition of pure zinc blocks is replaced by pure zinc wire delivery.

[0087]

[0088] After welding, the cross-sectional data of the weld were statistically analyzed for the samples in the above embodiments and comparative examples. Three cross-sections were measured and their average values ​​were calculated. The weld penetration data are shown in the table below.

[0089]

[0090] Group 4: The difference between this group's examples and Example A4 is as follows: the addition of pure zinc blocks is replaced by zinc powder blowing.

[0091]

[0092] After welding, the cross-sectional data of the weld were statistically analyzed for the samples in the above embodiments and comparative examples. Three cross-sections were measured and their average values ​​were calculated. The weld penetration data are shown in the table below.

[0093]

[0094] Group 5: The differences between the embodiments in this group and Embodiment A4 are as follows:

[0095]

[0096] Note: Comparative Example E1 is not degassed.

[0097] After welding, the cross-sectional data of the weld were statistically analyzed for the samples in the above embodiments and comparative examples. Three cross-sections were measured and their average values ​​were calculated. The weld penetration data are shown in the table below.

[0098]

[0099] Group Six: The differences between the embodiments in this group and Embodiment A4 are as follows:

[0100]

[0101] After welding, the cross-sectional data of the weld were statistically analyzed for the samples in the above embodiments and comparative examples. Three cross-sections were measured and their average values ​​were calculated. The weld penetration data are shown in the table below.

[0102]

[0103] The method provided by this invention can reduce the surface tension of the molten metal in 6XXX series aluminum alloys during welding. During welding, under the action of the arc force, the molten droplets formed by the melting of the welding wire more easily enter the molten pool, resulting in a greater weld penetration. Therefore, by increasing the welding speed, the plate can be fully penetrated. With increased welding speed, the welding heat input decreases, the peak temperature experienced by the base metal decreases, the high-temperature time is reduced, the coarsening degree of nano-precipitates in the alloy decreases, and the reduction in alloy strength is lessened, thus improving the post-weld strength of the alloy. Simultaneously, the reduced welding heat input reduces welding defects and improves weld bead formability. Furthermore, the increased welding speed also improves welding efficiency and reduces welding costs. Compared to alloying elements such as Li and Ce that can reduce the surface tension of the melt, Zn is inexpensive and safer. Moreover, the addition of Zn has no significant adverse effect on the strength of the base metal (tensile strength fluctuation is within ±1%), and while the elongation decreases slightly, it still meets the requirements for general structural materials.

[0104] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0105] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A method for improving the strength of the heat-affected zone of a welded joint of 6XXX series aluminum alloy, comprising at least the following steps: Prepare 6XXX series aluminum alloy and 0.1%-0.6% pure zinc by mass; For 6XXX series aluminum alloy casting, pure zinc is added and the temperature is maintained after the molten metal reaches 720-750℃.

2. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 1, characterized in that, The heat preservation operation lasts for 30-50 minutes.

3. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 1, characterized in that, The method for adding pure zinc with a purity of not less than 99.99% is any of the following: Pure zinc blocks are added to the molten metal in one go; or Pure zinc wire with a diameter of 1-3 mm is added from the center of the molten pool to a distance of 1 / 2R from the center, where R is the average distance from the center of the molten pool to the pool wall, calculated based on the equivalent radius of the horizontal cross-section of the molten pool; or High-purity argon gas is used to blow pure zinc powder into the melt to a depth of 3-8 cm.

4. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 3, characterized in that, The pure zinc powder has a particle size of 50-500 micrometers, and the flow rate of high-purity argon gas used for blowing is 1-3 L / min.

5. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to any one of claims 1-4, characterized in that, It also includes purifying and degassing the melt with high-purity argon after heat preservation.

6. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 5, characterized in that, The purity of the high-purity argon gas used in the purification and degassing process shall not be less than 5N.

7. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 5, characterized in that, The purification and degassing process involves blowing high-purity argon gas into the melt using a graphite rotor. The blowing of high-purity argon gas meets the following requirements: argon gas flow rate of 15-20 L / min and argon gas pressure of 1.2-3.0 atm. Simultaneously, the graphite rotor is stirred at a speed of 400 r / min, and the purification and degassing time is 25 min.

8. The method for improving the strength of the heat-affected zone of 6XXX series aluminum alloy welded joints according to claim 5, characterized in that, It also includes, in order: homogenization treatment, hot extrusion processing, and T5 treatment, among which... The homogenization process involves holding the ingot at 540-560℃ for 10-16 hours, and then cooling it. Hot extrusion processing involves homogenizing the material and then hot extruding it at 460℃-520℃, with the extrusion ratio controlled at 30-50. 9.6XXX series aluminum alloy, prepared by the method for improving the heat-affected zone strength of welded joints of 6XXX series aluminum alloy according to any one of claims 1-8.

10. A welded product obtained by welding a profile made of 6XXX series aluminum alloy as described in claim 9.