A method for pretreating an aluminum alloy melt and applications thereof
By adding composite seeding agents and stabilizers during the transfer of aluminum alloy melt and using magnetic field treatment, the problems of purification and microstructure refinement during the transfer of aluminum alloy melt were solved, achieving efficient pretreatment, shortening the production cycle, reducing energy consumption, and improving the performance of aluminum alloy products.
Patent Information
- Application Number
- CN202610926980.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-25
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies cannot simultaneously achieve purification, modification and reconstruction, and microstructure refinement during the transfer of aluminum alloy melt, resulting in extended production cycles and increased energy consumption. In particular, for aluminum-silicon alloy mother liquor extracted from solid waste, there are problems such as unstable melt structure, easy segregation of microalloying elements, coarse and unevenly distributed eutectic silicon phase, and high content of impurity elements.
During the transfer process, a composite seeding agent and a composite melt stabilizer are added, and a magnetic field is superimposed in the transfer package. Through the synergistic effect of the composite seeding agent and the magnetic field, phase precipitation is promoted and harmful impurities are removed, thus achieving efficient pretreatment of the melt.
It shortens the process cycle, significantly reduces energy consumption and carbon emissions, refines the grain structure, improves compositional uniformity, reduces the content of impurity elements, and provides high-quality aluminum alloy billets, suitable for the preparation of high-performance aluminum alloy products.
Smart Images

Figure CN123152907A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy melt processing technology, and in particular to a method for pre-treatment of aluminum alloy melts and its application. Background Technology
[0002] Melt treatment of aluminum alloys is a crucial step in determining the uniformity of the microstructure and mechanical properties of castings. Currently, the mainstream industrial technologies for aluminum alloy melt treatment are mainly divided into two categories: one is melt refining and filtration technology, which uses a refining and degassing device to purge the melt, removing gases and inclusions to achieve purification; the other is seed refiner induction technology, such as adding seed refiners like titanium boron wire or aluminum titanium carbon at the end of casting, which refines the grains by controlling the nucleation process and improving material properties. These technologies are usually implemented during the melting or holding stage before casting. However, there are no publicly reported methods for dedicated melt pretreatment for the intermediate step of transferring the alloy molten metal from the melting furnace to the casting equipment.
[0003] Furthermore, with the development of resource recycling, aluminum-silicon alloy mother liquor extracted from solid waste has gradually attracted attention. However, this type of mother liquor suffers from problems such as unstable melt structure, easy segregation of microalloying elements, coarse and unevenly distributed eutectic silicon phase, high content of impurity elements (such as iron and titanium), and poor melt stability. When directly used in subsequent forming processes, it is difficult to obtain high-performance products. Existing technologies cannot simultaneously achieve melt purification, modification and reconstruction, and microstructure refinement during the transfer process, resulting in the need for additional modification time and repeated heating processes in subsequent treatments. This not only prolongs the production cycle but also increases energy consumption and carbon emissions.
[0004] Therefore, how to achieve efficient pretreatment during the aluminum alloy melt transfer stage, fully utilize the advantages of the multi-component composition of the mother liquor, induce the precipitation of refined phases in advance, and remove harmful impurities has become an urgent technical problem to be solved. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a method and application for pretreatment of aluminum alloy melts, which achieves efficient pretreatment during the transfer stage of aluminum alloy melts and fully utilizes the advantages of the multi-component composition of the mother liquor to induce the precipitation of refined phases and remove harmful impurities in advance.
[0006] In order to achieve the objective of this invention, the following technical solution is adopted: This invention provides a method for pretreatment of aluminum alloy melt, comprising the following steps: S1. Add composite seeding agent to the transfer package, and add composite melt stabilizer after an interval of 0~45 minutes; S2. After the aluminum-silicon alloy mother liquor is discharged into the aluminum, it is sucked into the transfer bag for transfer. S3. During the transfer process, the temperature is maintained at 700℃~900℃, and a magnetic field of 0.5mT~200mT is superimposed to obtain a melt treated by the magnetic field. S4. The melt treated with the magnetic field is kept at 735℃~765℃, and then the melt is purified and cleaned.
[0007] Furthermore, the heat preservation time is 30 to 45 minutes.
[0008] Furthermore, based on the mass percentage of the composite seed agent, the composite seed agent is composed of the following raw materials: sodium chloride 5%–40%, potassium chloride 2.5%–36%, potassium nitrate 0.9%–14%, sodium carbonate 0%–20%, sodium hexafluoroaluminate 0.5%–27%, sodium fluoride 0.1%–13%, aluminum fluoride 0.1%–17%, borax 0.03%–8%, boron oxide 0.001%–5%, aluminum-titanium-boron master alloy 0.001%–5%, aluminum-titanium master alloy 0.001%–5%, aluminum-zirconium master alloy 0.001%–5%, aluminum-titanium-carbon master alloy 0.001%–5%, aluminum-titanium-boron-zirconium-carbon master alloy 0.001%–5%, aluminum-lanthanum master alloy 0.0001%–5%, aluminum-yttrium master alloy 0.0001%–5%, and aluminum-cerium master alloy 0.0001%–5%.
[0009] Furthermore, the composite melt stabilizer is composed of a salt-based composite refining agent and an aluminum-based master alloy; The salt-based compound refining agent, by mass fraction, is composed of the following raw materials: 15%~75% sodium chloride, 25%~80% potassium chloride, 10%~50% potassium fluoride, 5%~60% aluminum fluoride, and 8%~30% sodium hexafluoroaluminate.
[0010] Furthermore, based on the mass percentage of the composite melt stabilizer, the salt-based composite refining agent comprises 30% to 85%, and the aluminum-based master alloy comprises 15% to 70%. Furthermore, the mass ratio of the aluminum-silicon alloy mother liquor, the composite seed agent, and the composite melt stabilizer is (900~1000):(0.01~80):(0.05~69).
[0011] Furthermore, the chemical composition of the aluminum-titanium-boron-zirconium-carbon master alloy, by mass percentage, consists of the following raw materials: Ti 2%–6%, B 0.5%–1.5%, Zr 0.1%–0.8%, C 0.01%–0.35%, with the balance being Al.
[0012] Furthermore, the aluminum-silicon alloy mother liquor, by mass percentage, contains: Si 2%–30%, Fe ≤ 1.5%, Ti ≤ 0.8%, Zr ≤ 0.6%, other impurity elements ≤ 1.0%, and the balance is Al.
[0013] The present invention also provides aluminum alloy products prepared by the above-mentioned aluminum alloy melt pretreatment method.
[0014] This invention also provides the application of the above-mentioned aluminum alloy products in the preparation of high-performance aluminum alloy products.
[0015] Furthermore, high-performance aluminum alloy products include: aluminum alloy bars, sheets, wires, or filaments.
[0016] Furthermore, the high-performance aluminum alloy products are used in lightweight structural components for new energy vehicles, AI data centers, or high-megawatt energy storage power stations.
[0017] The present invention has the following technical effects: (1) Shorten the process cycle and save energy and reduce carbon emissions: The modification and purification process is completed simultaneously during the transfer of aluminum alloy melt. No additional modification process is required, which can save ≥15 minutes of modification time and eliminate the need for repeated heating process of ≥45 minutes, significantly reducing energy consumption and carbon emissions.
[0018] (2) The structure is significantly refined and the composition is uniform: The aluminum-silicon alloy mother liquor treated by the method of the present invention has a fine distribution of eutectic silicon phase, the grain structure is significantly refined, and there is no obvious component segregation, which provides high-quality billets for the subsequent preparation of high-performance aluminum alloy rods, plates, wires and other products.
[0019] (3) Efficient removal of impurities: Through the synergistic effect of composite seed agent, composite melt stabilizer and external magnetic field, the precipitation of heavy iron-rich phase and adsorption of salt flux are promoted, effectively reducing the content of impurity elements such as iron and titanium and improving the purity of melt.
[0020] (4) Wide range of applications: This method is not only effective for molten salt co-eutectoid aluminum-silicon alloy mother liquor, but also has a certain refining and purification effect on conventional aluminum alloy liquid, and has good universality and industrial application prospects. Attached Figure Description
[0021] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0022] Figure 1 Metallographic image before processing; Figure 2 : The processed metallographic image; Figure 3 : The fracture interface diagrams before and after processing, where a represents before processing and b represents after processing. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0024] The following is a detailed explanation using specific embodiments: Example 1: After 10.78 tons of aluminum from the aluminum-silicon alloy mother liquor were extracted, the liquid was transferred to a transfer bag, and the aluminum absorption temperature was measured. A certain proportion of composite seed agent and composite melt stabilizer were added to the transfer bag at 30-minute intervals. During the transfer, the temperature was maintained at 800℃, and the electromagnetic field generators installed at the bottom and side of the transfer bag were turned on to generate a superimposed magnetic field of 50mT, which was continuously applied during the transfer. The liquid was then transferred to the aluminum-silicon alloy melting and holding furnace by a transfer vehicle, where it was maintained at 750℃ for 35 minutes. The arrival time was recorded, and the aluminum pouring temperature was measured during the pouring process. The data before and after the transfer were compiled and analyzed. The liquid was then microfiltered with glass fiber cloth at the furnace inlet, and slag in the molten alloy was removed inside the furnace, achieving purification and cleansing during the transfer process.
[0025] The chemical composition of the aluminum-silicon alloy master liquor is 8.7wt% Si, 0.13wt% Fe, 0.19wt% Ti, 0.14wt% Zr, with other impurity elements totaling ≤1.0wt%, and the balance being Al; the chemical composition of the aluminum-titanium-boron-zirconium-carbon master alloy, by weight percentage, contains 5% Ti, 1% B, 0.5% Zr, 1% C, and the balance being Al.
[0026] The raw materials for melt pretreatment include, by weight, 950g of aluminum-silicon alloy mother liquor, 75g of composite seed agent and 65g of composite melt stabilizer.
[0027] The raw materials for preparing the composite seed agent include a salt composite substrate, an aluminum-based master alloy, and a composite rare earth alloy. The raw materials, by percentage, include 29% sodium chloride, 10% potassium chloride, 10% potassium nitrate, 10% sodium carbonate, 5% sodium hexafluoroaluminate, 5% sodium fluoride, 8% aluminum fluoride, 3% borax, 2% boron oxide, 3% aluminum-titanium-boron master alloy (purchased from Qinhuangdao Fengyue Technology Co., Ltd.), 1% aluminum-titanium master alloy (purchased from Qinhuangdao Fengyue Technology Co., Ltd.), 2% aluminum-zirconium master alloy (purchased from Xuzhou Jieke Aluminum Co., Ltd.), 3% aluminum-titanium-carbon master alloy (purchased from Qinhuangdao Fengyue Technology Co., Ltd.), and 4% aluminum-titanium-boron-zirconium-carbon master alloy (Ti 5%, B 1%, Zr 0.5%, C...). The composite melt stabilizer was prepared from 1% (balance: Al), 3% aluminum-lanthanum master alloy (purchased from Shanghai Youfeng Alloy Materials Co., Ltd.), 1% aluminum-yttrium master alloy (purchased from Shanghai Youfeng Alloy Materials Co., Ltd.), and 1% aluminum-cerium master alloy (purchased from Shanghai Youfeng Alloy Materials Co., Ltd.). The salts were mixed and then melt-sintered at 950℃ for 2 hours before being crushed. The master alloys were proportioned and added as solid blocks. The raw materials for the composite melt stabilizer included a salt-based composite refining agent and aluminum-based master alloys. The main components of the composite refining agent were 40% sodium chloride, 20% potassium chloride, 20% potassium fluoride, 10% aluminum fluoride, and 10% sodium hexafluoroaluminate, which were mixed and then melt-sintered at 950℃ for 2 hours before being crushed.
[0028] Experimental Example 1 Compare the metallographic images before and after treatment. The metallographic image before treatment is as follows: Figure 1 As shown, the processed metallographic image is as follows: Figure 2 As shown.
[0029] As can be seen from the figure, in the metallographic image before treatment, the eutectic silicon phase is coarse, distributed in needle-like or blocky shapes, and is uneven in size; in the metallographic image after treatment, the eutectic silicon phase becomes fine, round, and evenly distributed, which is beneficial to improving the mechanical properties of the alloy (especially plasticity and fatigue resistance).
[0030] Before treatment, the grain size was large and there were obvious dendrites or segregation. After treatment, the grains were significantly refined, the equiaxed crystal characteristics were obvious, and there was no obvious compositional segregation, indicating that the melt structure tended to be stable and the nucleation effect was significantly enhanced.
[0031] The metallographic image before treatment shows a small number of coarse impurity phases (such as iron-rich phases); the metallographic image after treatment shows that the impurity phases are significantly reduced or disappeared, and the matrix is cleaner, which confirms the effect of the synergistic effect of magnetic field and flux on the removal of impurities such as iron and titanium.
[0032] The metallographic image visually demonstrates that the present invention, through the synergistic effect of composite seeding agent, composite melt stabilizer and magnetic field during the transfer process, can effectively refine the structure, purify the melt, and obtain high-quality aluminum-silicon alloy mother liquor.
[0033] The fracture interface of the treated aluminum alloy metal structure is as follows Figure 3 As shown, the treated aluminum alloy has a dense metal structure, and the slag and non-metallic inclusions have significantly disappeared.
[0034] Experiment Example 2: Mechanical Property Testing Aluminum alloy ingots were obtained by casting from the aluminum alloy melt pretreated by the method of this invention and from the untreated control melt. The relevant provisions of GB / T 16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys" and GB / T 228.1-2021 "Metallic Materials - Tensile Testing - Part 1: Test Methods at Room Temperature" were followed.
[0035] Standard tensile specimens are cut and prepared from the same location on the billet by machining. The specimens are circular cross-section proportional specimens (gauge length L0 = 5d0, where d0 is the original diameter of the specimen). The surface should be smooth and defect-free after machining, with a surface roughness Ra not exceeding 1.6 μm. Gauge lines are marked within the original gauge length range of the specimen. The diameter is measured at three cross-sections—at both ends and the middle—within the gauge length range using vernier calipers. Measurements are taken once at each cross-section along mutually perpendicular directions, and the average value is recorded. The minimum of the three average values is taken as the original diameter d0 of the specimen, and the value is calculated using the formula A0 = π(d0 / 2). 2 Calculate the original cross-sectional area A0 of the specimen. Prepare at least 3 parallel specimens for each condition, and take the average value of the test results.
[0036] Test steps: The prepared standard tensile specimen is centered and installed in the upper and lower clamps of the universal testing machine to ensure that the specimen is subjected to axial tensile force and avoid bending. The clamps should be firmly held to prevent slippage during the test.
[0037] An extensometer is installed along the parallel length of the specimen. The gauge length Le of the extensometer should meet the standard requirements. It is used to accurately measure the elongation of the specimen during the elastic and early plastic deformation stages.
[0038] Axial tensile loads were applied according to the test rate control method specified in GB / T 228.1-2021. For aluminum alloys (without obvious yielding), the specified non-proportional elongation strength (Rp) was determined. 0·2 When determining tensile strength, the strain rate control method (typically 0.00025 / s) is used within the elastic range and stress range up to the specified non-proportional elongation strength; when determining tensile strength, the beam displacement rate control method can be used. Tensile force is continuously applied until the specimen breaks.
[0039] The load-displacement data (or stress-strain curve) during the tensile process is recorded in real time by the testing machine control system, generating a complete stress-strain curve and recording the maximum test force Fm of the specimen (the maximum force that the specimen can withstand before it breaks).
[0040] After the specimen breaks, the two broken parts are tightly joined together along the fracture surface to ensure that the axes of the two parts are on the same straight line. The gauge length Lu after the fracture is measured with a measuring tool with a resolution of not less than 0.1 mm, accurate to within ±0.25 mm.
[0041] Results Processing and Calculation Tensile strength (Rm): Calculated using the formula Rm = Fm / A0, where Fm is the maximum force (N) the specimen can withstand before fracture, and A0 is the original cross-sectional area of the specimen (mm²). 2 The results are expressed in megapascals (MPa).
[0042] Elongation after fracture (A): Calculated according to the formula A = [(Lu - L0) / L0] × 100%, where L0 is the original gauge length of the specimen (mm) and Lu is the gauge length of the specimen after fracture (mm). The result is expressed as a percentage (%).
[0043] Data processing: The test results of parallel samples in the same group were arithmetically averaged, and the results were rounded according to GB / T 228.1-2021. The experimental results are shown in Table 1.
[0044] Table 1: Mechanical Performance Test Results
[0045] Experiment Example 3: Comparison of tissue refinement effects under different magnetic field strengths Test method: (1) Set the magnetic field strength gradient: 0mT (blank control), 0.5mT, 10mT, 50mT, 100mT, 200mT, 250mT; (2) Under the condition that all other parameters are the same, the above magnetic field gradient is used to treat the aluminum-silicon alloy mother liquor respectively; (3) Metallographic observation was performed on each group of samples, and the average grain size, average length of eutectic silicon phase, and aspect ratio were measured under different magnetic field strengths. The experimental results are shown in Table 2.
[0046] Table 2: Comparison of tissue refinement effects under different magnetic field intensities
[0047] As shown in Table 2, the magnetic field strength has a significant impact on the microstructure refinement of the aluminum alloy melt. When no magnetic field is applied (0 mT), the average grain size is 156 μm, the average length of the eutectic silicon phase is 38.2 μm, and it is distributed in coarse needle-like or blocky shapes with an aspect ratio as high as 5.8, indicating that the melt microstructure is coarse and non-uniform.
[0048] As the magnetic field strength increased from 0 mT to 100 mT, the average grain size, average length of the eutectic silicon phase, and aspect ratio all showed a continuous decreasing trend. Specifically, at 50 mT, the average grain size decreased to 58 μm, a reduction of approximately 62.8% compared to the untreated state; the average length of the eutectic silicon phase decreased to 14.6 μm, a reduction of approximately 61.8%; and the aspect ratio decreased to 2.1, significantly improving the roundness of the microstructure. The microstructure refinement effect reached its optimum at 100 mT, with an average grain size of 55 μm, an average length of the eutectic silicon phase of 13.8 μm, and an aspect ratio of 1.9. The refinement effect was slightly improved compared to 50 mT, but the rate of improvement slowed down.
[0049] When the magnetic field strength was increased to 200 mT, the microstructure refinement effect weakened slightly, the average grain size rebounded to 63 μm, and the average length of the eutectic silicon phase increased to 15.2 μm. When the magnetic field strength was increased to 250 mT, the refinement effect decreased significantly, the average grain size increased to 81 μm, the average length of the eutectic silicon phase increased to 18.7 μm, and the aspect ratio rebounded to 2.8, indicating that excessively high magnetic field strength had an adverse effect on microstructure refinement.
[0050] The above results indicate that a magnetic field of appropriate strength (0.5 mT–200 mT) can effectively promote melt flow, homogenize the temperature and composition fields, accelerate heterogeneous nucleation, and suppress dendrite growth, thereby refining grains and the eutectic silicon phase. However, excessively high magnetic field strength (e.g., when the magnetic field strength > 200 mT) can intensify forced convection of the melt, potentially leading to remelting of already formed fine grains or erosion of dendrite arms, thus weakening the refining effect. Therefore, controlling the magnetic field strength within the range of 0.5 mT–200 mT is reasonable and necessary, with 50 mT–100 mT being the optimal range.
[0051] Experiment Example 4: Optimization Experiment of the Interval Between Additions of Composite Seeding Agent (1) Set the interval time gradient: 0min (add simultaneously), 15min, 30min, 45min, 60min; (2) Under the condition that all other parameters are the same, the grain size, impurity element content (Fe, Ti), melt hydrogen content and other indicators of each group of samples are detected to determine the optimal addition interval.
[0052] The experimental results are shown in Table 3.
[0053] Table 3: Experimental Results of Optimization of Composite Seeding Agent Addition Interval Time
[0054] As shown in Table 3, the time interval between the addition of composite seeding agent and composite melt stabilizer has a significant impact on the grain refinement effect, impurity removal ability and melt purity of the melt.
[0055] Firstly, regarding the effect on grain refinement: when the interval is 0 min (i.e., both are added simultaneously), the average grain size is 92 μm, and the refinement effect is limited. As the interval is extended to 15 min, the grain size decreases to 74 μm; at an interval of 30 min, the optimal value of 58 μm is reached, representing a refinement of approximately 37.0% compared to simultaneous addition. When the interval is further extended to 45 min, the grain size slightly increases to 62 μm; at an interval of 60 min, it significantly increases to 85 μm, and the refinement effect decreases significantly. These results indicate that after the composite seeding agent is added, a certain diffusion and uniform distribution time (approximately 30 min) is required for the seed particles to be fully dispersed and form an effective nucleation interface with Al atoms in the melt; subsequently, the addition of the composite melt stabilizer can rapidly reduce the surface tension of the melt and improve wettability, promoting the nucleation efficiency of the seed particles. If the interval is too short (≤15 min), the composite seed agent will be coated by the stabilizer before it is fully dispersed, and the nucleation sites will be covered, thus limiting the refining effect. If the interval is too long (≥60 min), the seed agent added earlier may become ineffective or agglomerate and settle due to the high temperature of the melt, and the melt structure will become uneven again.
[0056] Secondly, regarding the impact on impurity removal: the trends of Fe and Ti content changes with time intervals are basically consistent with the grain size. At a 30-minute interval, the Fe content decreased from the initial 0.13 wt% to 0.08 wt%, and the Ti content decreased from 0.19 wt% to 0.13 wt%, showing the best removal effect. The impurity removal effects were second best at 15 and 45 minutes, while the removal effects were worst at 0 and 60 minutes. This indicates that there is an optimal synergistic window between the composite seed agent and the composite melt stabilizer. Adding the composite melt stabilizer after the seed agent is fully dispersed is beneficial for the salt refining agent to capture and adsorb the heavy iron-rich phase in the melt, causing the iron-rich phase to form composite agglomerates with the flux and float to the melt surface for removal.
[0057] Finally, regarding the effect on degassing: the hydrogen content of the melt also reached its lowest value of 0.25 mL / 100g after a 30-minute interval, which was about 34.2% lower than when added simultaneously. The salt components (such as sodium hexafluoroaluminate) in the composite melt stabilizer have degassing and slag removal functions. When added after the seeding agent is fully dispersed, unnecessary reaction and consumption between the salt and the seed particles can be avoided, thereby maintaining a high degassing efficiency.
[0058] Based on the above analysis, the optimal interval between adding the composite seed agent and the composite melt stabilizer is 30 min, and 15–45 min is an acceptable preferred range. Adding them outside this range (such as 60 min) or adding them simultaneously will result in a significant decrease in the refining and purification effects due to insufficient dispersion of the seed agent, coverage of nucleation sites, or failure of the seed agent.
[0059] Experimental Example 5: Verification of the synergistic effect of composite seeding agent and composite melt stabilizer To verify the necessity and synergistic enhancement effect of using composite seeding agents and composite melt stabilizers in combination, the following four control experiments were set up: Group A (blank control): No additives added, 0 magnetic field; Group B: No additives added + 50 mT magnetic field; Group C: Only composite seed agent added + 50 mT magnetic field; Group D: Add only composite melt stabilizer + 50 mT magnetic field; Group E (Example 1): Composite seed agent + composite melt stabilizer + 50 mT magnetic field; With other process parameters kept constant, the experimental results are shown in Table 4.
[0060] Table 4: Results of the synergistic effect verification of composite seeding agent and composite melt stabilizer
[0061] The grain size of group B is consistent with the 50 mT data in Table 2, indicating that the magnetic field alone can achieve significant grain refinement (refinement rate of 62.8%), but has almost no removal effect on Fe and Ti impurity elements (Fe is still 0.15% and Ti is still 0.21%). This is because the magnetic field mainly achieves refinement by promoting the homogenization of the melt temperature field and composition field through forced convection, accelerating dendrite breakage and free grain proliferation, and has limited ability to chemically remove impurity elements.
[0062] The grain size of group C was slightly coarser than that of group B (58 μm → 72 μm). This is because the salt components in the seeding agent, without the protection of a stabilizer, partially adsorbed onto the surface of the nucleation sites, inhibiting heterogeneous nucleation efficiency. However, its grain refining effect was still better than that of group D, indicating that the seeding agent played a dominant role in grain refining.
[0063] Group D showed significant removal effects on Fe and Ti (Fe decreased from 0.15% to 0.10%, and Ti decreased from 0.21% to 0.17%), but the grain size coarsened to 95 μm. This is because the flux covering the melt surface reduced the surface tension, weakened the magnetic field-driven melt convection intensity, and reduced the grain refining effect.
[0064] Group E achieved the optimal synergy between grain refinement and impurity removal: the grain size (58 μm) reached the same level of refinement as that of a single magnetic field, the Fe content (0.08%) and Ti content (0.13%) were the lowest among all groups, and the tensile strength (186 MPa) and elongation (3.1%) were both optimal.
[0065] The composite seeding agent provides heterogeneous nucleation sites under magnetic field assistance, achieving grain refinement; the composite melt stabilizer removes impurities by capturing heavy, iron-rich phases through its salt components; the two are added in stages to avoid mutual interference, each playing its dominant role. The synergistic effect of these three components produces a superior result: the magnetic field promotes seed dispersion and flux diffusion; the seeding agent refines the microstructure, providing more adequate interfacial contact conditions for flux purification; and the flux purification removes impurities, creating a cleaner melt environment for grain refinement. The comprehensive technical effect of this invention cannot be achieved by using any single component alone.
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the technical solutions of the embodiments of the present invention.
Claims
1. A method for pretreatment of aluminum alloy melt, characterized in that, Includes the following steps: S1. Add composite seeding agent to the transfer package, and add composite melt stabilizer after an interval of 0~45 min; S2. After the aluminum-silicon alloy mother liquor is discharged into the aluminum, it is sucked into the transfer bag for transfer. S3. During the transfer process, the temperature is maintained at 700℃~900℃, and a magnetic field of 0.5mT~200mT is superimposed to obtain a melt treated by the magnetic field. S4. The melt treated with the magnetic field is kept at 735℃~765℃, and then the melt is purified and cleaned.
2. The aluminum alloy melt pretreatment method according to claim 1, characterized in that, The composite seeding agent, by mass percentage, is composed of the following raw materials: sodium chloride 5%–40%, potassium chloride 2.5%–36%, potassium nitrate 0.9%–14%, sodium carbonate 0%–20%, sodium hexafluoroaluminate 0.5%–27%, sodium fluoride 0.1%–13%, aluminum fluoride 0.1%–17%, borax 0.03%–8%, boron oxide 0.001%–5%, aluminum-titanium-boron master alloy 0.001%–5%, aluminum-titanium master alloy 0.001%–5%, aluminum-zirconium master alloy 0.001%–5%, aluminum-titanium-carbon master alloy 0.001%–5%, aluminum-titanium-boron-zirconium-carbon master alloy 0.001%–5%, aluminum-lanthanum master alloy 0.0001%–5%, aluminum-yttrium master alloy 0.0001%–5%, and aluminum-cerium master alloy 0.0001%–5%.
3. The aluminum alloy melt pretreatment method according to claim 1, characterized in that, The composite melt stabilizer is composed of a salt-based composite refining agent and an aluminum-based master alloy. Among them, based on the mass percentage of the composite melt stabilizer, the salt composite refining agent is 30%~85%, and the aluminum-based master alloy is 15%~70%; The salt-based compound refining agent, by mass fraction, is composed of the following raw materials: 15%~75% sodium chloride, 25%~80% potassium chloride, 10%~50% potassium fluoride, 5%~60% aluminum fluoride, and 8%~30% sodium hexafluoroaluminate.
4. The aluminum alloy melt pretreatment method according to claim 1, characterized in that, The mass ratio of the aluminum-silicon alloy mother liquor, the composite seeding agent, and the composite melt stabilizer is (900~1000):(0.01~80):(0.05~69).
5. The aluminum alloy melt pretreatment method according to claim 2, characterized in that, The chemical composition of the aluminum-titanium-boron-zirconium-carbon master alloy, by mass percentage, consists of the following raw materials: Ti 2%–6%, B 0.5%–1.5%, Zr 0.1%–0.8%, C 0.01%–0.35%, with the balance being Al.
6. The aluminum alloy melt pretreatment method according to claim 1, characterized in that, The aluminum-silicon alloy mother liquor, by mass percentage, contains: Si 2%–30%, Fe ≤ 1.5%, Ti ≤ 0.8%, Zr ≤ 0.6%, other impurity elements ≤ 1.0%, and the balance is Al.
7. An aluminum alloy product prepared by the aluminum alloy melt pretreatment method according to any one of claims 1 to 6.
8. The application of the aluminum alloy product as described in claim 7 in the preparation of high-performance aluminum alloy products.
9. The application of the aluminum alloy product according to claim 8 in the preparation of high-performance aluminum alloy products, characterized in that, High-performance aluminum alloy products include: aluminum alloy bars, plates, wires or filaments.