A powder metallurgy process for the production of graphene-aluminum alloy composites
By performing surface functionalization and low-temperature mixing on graphene, combined with graded pressure hot isostatic pressing, pulsed current sintering and multi-step heat treatment, the problems of insufficient comprehensive performance of aluminum alloy materials and uneven graphene dispersion were solved, significantly improving the interfacial bonding force and comprehensive performance of the materials.
Patent Information
- Application Number
- CN202510663586.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional aluminum alloy materials have shortcomings in terms of electrical conductivity, thermal conductivity, thermal shock resistance, wear resistance, and corrosion resistance. Graphene has weak interfacial bonding with aluminum alloys, and graphene is not evenly dispersed in powder metallurgy processes, which affects the material properties.
By surface functionalizing graphene, oxygen- or nitrogen-containing functional groups are introduced. Combined with low-temperature mixing, graded pressure hot isostatic pressing, pulsed current assisted sintering and multi-step heat treatment, carbon nanotubes and silver nanoparticles are added to optimize the microstructure of the composite material and perform surface coating treatment.
It significantly improved the interfacial bonding force between graphene and aluminum alloy, achieved uniform dispersion of graphene, and enhanced the comprehensive performance of the composite material, including hardness, tensile strength, electrical conductivity, thermal conductivity, thermal shock resistance, and corrosion resistance.
Smart Images

Figure CN123152912A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of graphene technology, and in particular to a powder metallurgy preparation process for graphene-aluminum alloy composite materials. Background Technology
[0002] With the development of modern industry and technology, the requirements for materials are no longer limited to high strength and lightweight; they also demand comprehensive properties such as excellent electrical conductivity, thermal conductivity, thermal shock resistance, dimensional stability, wear resistance, and corrosion resistance. While traditional aluminum alloys have certain advantages, they are significantly insufficient in meeting these specific performance requirements. Graphene, due to its ultra-high strength and excellent electrical and thermal conductivity, is an ideal material for enhancing the performance of aluminum alloys. However, introducing graphene into aluminum alloys faces many challenges, such as weak interfacial bonding and difficulty in achieving uniform dispersion of graphene during preparation, which affects the performance of the final product. Summary of the Invention
[0003] Based on the above analysis, the embodiments of the present invention aim to provide a powder metallurgy preparation process for graphene-aluminum alloy composite materials, in order to at least solve one of the following problems:
[0004] (1) Insufficient bonding force between graphene and aluminum alloy interface.
[0005] (2) In traditional powder metallurgy processes, graphene is unevenly dispersed and easily agglomerates, which affects the material properties.
[0006] (3) The overall performance improvement of composite materials, such as electrical conductivity and thermal conductivity, is limited.
[0007] On one hand, embodiments of the present invention provide a powder metallurgy preparation process for graphene-aluminum alloy composite materials, including the following steps:
[0008] S1. Pretreatment stage: Graphene is surface functionalized by introducing oxygen- or nitrogen-containing functional groups. After the treatment is completed, the functionalized graphene is dried.
[0009] S2. Mixing stage: Aluminum alloy powder, nano-sized ceramic particles and functionalized graphene powder are mixed in a low temperature environment of -100℃ to -150℃ to obtain mixture A.
[0010] S3, Adding materials: Add additional nanoscale ceramic particles as a reinforcing phase to mixture A obtained in S2; simultaneously add carbon nanotubes and / or silver nanoparticles;
[0011] S4. Pressing stage: The mixture after S3 treatment is pressed using staged pressure hot isostatic pressing technology.
[0012] S5, Sintering stage: The product pressed in S4 is sintered with pulsed current assisted sintering.
[0013] S6. Post-treatment stage: The composite material after S5 sintering is subjected to a multi-step heat treatment combined with rapid cooling; then the composite material is coated with a surface coating.
[0014] Furthermore, the oxygen-containing functional groups introduced by the surface functionalization treatment include carboxyl and hydroxyl groups, and the nitrogen-containing functional groups include amino groups.
[0015] Furthermore, in S2, based on the total mass m of mixture A, the mass of the functionalized graphene powder is m×(0.5~5)%, and the mass of the aluminum alloy powder is m×(95~99.5)%.
[0016] Furthermore, the nanoscale ceramic particles described in S2 and / or S3 include one or more of silicon carbide, aluminum nitride, or titanium diboride.
[0017] Furthermore, in S3, based on the total mass m of mixture A, the amount of additional nano-sized ceramic particles added is m×(0.1~3)%, and the amount of carbon nanotubes and / or silver nanoparticles added is m×(0.05~1)%.
[0018] Furthermore, in the S4 pressing stage, staged pressure hot isostatic pressing technology is used for pressing, and the specific steps are as follows:
[0019] Initial stage: Under the protection of inert gas, a pressure of 50-100MPa is first applied, while the temperature is controlled within the range of 300-400℃, in order to form a preform with a certain strength;
[0020] Gradual pressurization stage: The pressure is then gradually increased to 150-300 MPa, while the temperature is raised to 400-600℃ to ensure complete densification of the material and promote directional crystal growth.
[0021] Furthermore, in the S5 sintering stage, pulsed current-assisted sintering is used, with a sintering temperature of 500℃-700℃, a sintering time of 5-30 minutes, and a current density set at 100-500 A / cm². 2 .
[0022] Furthermore, in the S5 sintering stage, the pulsed current-assisted sintering employs a multi-stage heating program, with the specific steps as follows:
[0023] (1) Preheating stage: slowly increase the temperature to 200-300℃ at a rate of 10-50℃ / min to remove volatiles and adsorbed gases from the sample;
[0024] (2) Rapid heating stage: rapidly heat to sintering temperature of 500℃-700℃ at a rate of 100-300℃ / min to shorten sintering time and reduce grain growth;
[0025] (3) Sintering stage: Hold at a sintering temperature of 500℃-700℃ for 5-30 minutes to ensure that the material is fully sintered and forms a stable microstructure;
[0026] (4) Cooling stage: Natural cooling or forced cooling is adopted; the cooling rate of forced cooling is ≥50℃ / min.
[0027] Furthermore, in the S6 post-processing stage, the multi-step heat treatment includes annealing and aging; the surface coating treatment is to form a ceramic, metal, or metal oxide coating on the surface of the graphene aluminum alloy composite material.
[0028] On the other hand, embodiments of the present invention provide a graphene-aluminum alloy composite material, which is prepared by the above-described preparation process.
[0029] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0030] 1) Enhance the interfacial bonding between graphene and aluminum alloy
[0031] By introducing oxygen- or nitrogen-containing functional groups through surface functionalization, the chemical bonding strength between graphene and aluminum alloy is significantly improved, solving the problem of insufficient interfacial bonding in traditional processes, thereby enhancing the overall performance of the composite material.
[0032] 2) Achieve uniform dispersion of graphene
[0033] During the mixing stage, a nanoscale dispersion technique at a specific temperature (-100℃ to -150℃) was employed. By combining ultrasonic assistance with high shear force stirring, the agglomeration of graphene was effectively avoided, ensuring its uniform distribution in the aluminum alloy matrix and further optimizing the mechanical and physical properties of the material.
[0034] 3) Improve the overall performance of composite materials
[0035] This invention significantly enhances the chemical bonding between graphene and aluminum alloys through surface functionalization, thereby improving the overall mechanical properties and electrical conductivity of the material. A low-temperature mixing process ensures uniform dispersion of nanoparticles and optimizes the microstructure. Precisely controlled pressing and sintering parameters further improve the material's density and strength. The addition of carbon nanotubes and silver nanoparticles improves electrical and thermal conductivity and enhances antibacterial properties. Multi-step heat treatment and rapid cooling processes refine the microstructure, enhancing thermal shock resistance and dimensional stability. A surface coating significantly improves corrosion resistance.
[0036] Compared with existing technologies, the material of this invention has significant advantages in comprehensive performance. Its hardness reaches 135-245 HV, tensile strength is 320-580 MPa, electrical conductivity is 0.5-0.9 IACS, thermal conductivity is 160-280 W / m·K, and wear resistance is 0.5-3.5 × 10⁻⁶. -5 mm 3 / N·m, corrosion resistance is 600-1500 hours. In contrast, materials without surface functionalization or with improper mixing conditions have significantly lower performance than this invention, with a hardness of only 95-180 HV, tensile strength of 280-450 MPa, electrical conductivity of 0.4-0.72 IACS, thermal conductivity of 120-205 W / m·K, and wear resistance of 2.5-8 × 10⁻⁶ N·m. -5 mm 3 / N·m, corrosion resistance is 200-700 hours.
[0037] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0038] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0039] Figure 1 This is a flow chart of the powder metallurgy preparation process of the graphene-aluminum alloy composite material described in this invention. Detailed Implementation
[0040] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0041] This invention addresses the limitations of traditional aluminum alloys in terms of electrical conductivity, thermal conductivity, thermal shock resistance, wear resistance, and corrosion resistance, as well as the weak interfacial bonding between graphene and aluminum alloys and the difficulty in achieving uniform graphene dispersion using traditional powder metallurgy processes. It proposes an innovative solution:
[0042] By functionalizing the graphene surface and introducing oxygen- or nitrogen-containing functional groups, the interfacial bonding strength between graphene and aluminum alloy is significantly enhanced. Based on this, a low-temperature ball milling process is used for mixing, leveraging the low-temperature environment to reduce particle surface energy, minimize agglomeration, and ensure uniform dispersion at the nanoscale. Simultaneously, appropriate amounts of carbon nanotubes or silver nanoparticles are added; these reinforcing phases not only improve the material's electrical and thermal conductivity but also synergize with the functionalized graphene, further optimizing the composite material's microstructure. Next, in the pressing stage, graded pressure hot isostatic pressing technology is used to form a dense preform and promote crystal growth, laying a solid foundation for subsequent sintering. Following this, in the sintering stage, pulsed current-assisted sintering technology precisely controls the temperature rise process, ensuring the material's high-temperature stability and density. Finally, optimized post-processing, including a combination of multi-step heat treatment and rapid cooling, and surface coating treatments selected according to the application scenario, further enhances wear resistance and corrosion resistance.
[0043] Through close integration and synergistic optimization of each step in the process design, the composite material exhibits excellent comprehensive performance in terms of electrical conductivity, thermal conductivity, thermal shock resistance, wear resistance, and corrosion resistance.
[0044] On one hand, a specific embodiment of the present invention discloses a powder metallurgy preparation process for graphene-aluminum alloy composite materials, such as... Figure 1 As shown, it includes the following steps:
[0045] S1. Pretreatment stage: Graphene is surface functionalized by introducing oxygen- or nitrogen-containing functional groups to enhance its chemical bonding with aluminum alloy. After the treatment is completed, the functionalized graphene is dried.
[0046] S2. Mixing stage: In a low temperature environment of -100℃ to -150℃, aluminum alloy powder, nano-sized ceramic particles and functionalized graphene powder are mixed to achieve uniform dispersion at the nanoscale, ensure that each component is uniformly distributed at the microscale, avoid particle agglomeration, thereby optimizing the performance of the composite material and finally obtaining mixture A.
[0047] S3, Adding materials: Add additional nanoscale ceramic particles as a reinforcing phase to A in the mixture obtained in S2; at the same time, add carbon nanotubes and / or silver nanoparticles to improve electrical and thermal conductivity.
[0048] S4, Pressing stage: The mixture after S3 treatment is pressed using staged pressure hot isostatic pressing technology;
[0049] S5, Sintering stage: The product pressed in S4 is sintered with pulsed current assisted sintering.
[0050] S6. Post-processing stage: The composite material after S5 sintering is subjected to a multi-step heat treatment combined with rapid cooling to optimize its microstructure, giving it excellent thermal shock resistance and dimensional stability; then the composite material is coated with a surface coating to further improve its corrosion resistance and electromagnetic shielding effect.
[0051] Furthermore, in S1, the oxygen-containing functional groups introduced by the surface functionalization treatment include carboxyl and hydroxyl groups, and the nitrogen-containing functional groups include amino groups. This surface functionalization treatment significantly enhances the chemical bonding between graphene and aluminum alloy, thereby improving the overall mechanical properties and electrical conductivity of the material. Compared with the untreated comparative example, the composite material of the present invention exhibits higher hardness, tensile strength, and electrical conductivity.
[0052] Specifically, the steps and parameters for surface functionalization are as follows:
[0053] Introduction of hydroxyl functional groups: Graphene was treated with oxygen plasma for 30-60 minutes, with a power of 100-150W and a pressure of 0.3-0.7Pa.
[0054] Introduction of amino functional groups: Graphene is soaked in an ammonia solution with a concentration of 20% to 30% for 12 to 36 hours, then washed with water and dried at 50 to 70°C for 2 to 6 hours.
[0055] Introduction of carboxyl functional groups: Graphene was acid-treated with a mixture of concentrated sulfuric acid and nitric acid (volume ratio of 2:1 to 4:1) for 6 to 24 hours, then washed with deionized water until neutral, and dried at 60 to 100°C for 1 to 4 hours.
[0056] Simultaneous introduction of hydroxyl and amino functional groups: First, oxygen plasma treatment is performed for 30-60 minutes at a power of 100-150 W and a pressure of 0.3-0.7 Pa; then, graphene is immersed in an ammonia solution with a concentration of 20%-30% for 12-36 hours, and finally dried at 50-70°C for 2-6 hours.
[0057] Using the above methods, functional groups such as hydroxyl, amino, and carboxyl groups were successfully introduced into the surface of graphene, thereby realizing the surface functionalization treatment of graphene and laying the foundation for improving the performance of composite materials.
[0058] Specifically, in S2, this invention effectively solves the problem of easy agglomeration of graphene and nanoparticles in traditional room-temperature mixing by using liquid nitrogen for mixing at a low-temperature environment (approximately -100°C to -150°C). The low-temperature environment reduces the surface energy of the particles, decreasing van der Waals forces and electrostatic forces, thereby preventing particle agglomeration. Simultaneously, it enhances the activity of oxygen-containing functional groups (such as hydroxyl and carboxyl groups) on the graphene surface, promoting their interaction with nanoparticles and achieving nanoscale uniform dispersion of graphene in the aluminum alloy powder. This uniform dispersion helps form a tighter contact between graphene and the aluminum alloy matrix, enhancing interfacial bonding. Furthermore, the addition of nanoscale ceramic particles further improves the material's strength and high-temperature resistance, optimizes the microstructure, and thus significantly improves mechanical properties.
[0059] In S2, graphene powder, aluminum alloy powder, and silicon carbide (SiC) nano-sized ceramic particles are mixed in a ball mill with a ball-to-powder ratio of 10:1 to 20:1, a milling speed of 50 to 400 rpm, and a milling time of 4 to 8 hours. By controlling the ball milling energy input, low-temperature environment, and protective atmosphere, graphene and SiC nanoparticles are uniformly dispersed at the nanoscale in the aluminum alloy matrix without structural damage or powder agglomeration.
[0060] Furthermore, in S2, the total mass of mixture A is defined as m, the mass of the functionalized graphene powder accounts for 0.5% to 5% of the total mass of mixture A (i.e., mass m × (0.5% to 5)%), and the mass of the aluminum alloy powder accounts for 95% to 99.5% of the total mass of mixture A (i.e., mass m × (95% to 99.5)%). In addition, the mass of the nano-ceramic particles accounts for 0.5% to 5% of the total mass of mixture A (i.e., mass m × (0.5% to 5%)).
[0061] Furthermore, in S2, the graphene powder has a particle size of 50–500 nm, the aluminum alloy powder has a particle size of 1–100 μm, and the nano-ceramic particles have a particle size of 20–500 nm; preferably, the graphene particle size is 100–300 nm, the aluminum alloy particle size is 10–50 μm, and the nano-ceramic particles are 50–200 nm.
[0062] During the mixing process, graphene powder, aluminum alloy powder, and nano-ceramic particles are mixed at a low temperature of -100℃ to -150℃ for 4 to 8 hours, with the mixing equipment rotating at a speed of 50 to 400 rpm. There are no other special requirements during the mixing process; the main purpose is to ensure that each component is fully and uniformly dispersed.
[0063] Furthermore, the nanoscale ceramic particles described in S2 and / or S3 include, but are not limited to, one or more of silicon carbide, aluminum nitride, or titanium diboride. These nanoscale ceramic particles can act as a "bridge" connecting the graphene and aluminum alloy matrix, enhancing interfacial stability.
[0064] Furthermore, in S3, based on the total mass m of mixture A, the amount of additional nano-sized ceramic particles added is m×(0.1~3)%, and the amount of carbon nanotubes and / or silver nanoparticles added is m×(0.05~1)%.
[0065] Furthermore, in S3, the electrical and thermal conductivity of the material is enhanced by adding appropriate amounts of carbon nanotubes (CNTs) and / or silver nanoparticles (Ag). These reinforcing phases not only improve the electrical and thermal conductivity of the material but also optimize the microstructure of the composite material through synergistic effects with graphene, thereby indirectly enhancing the interfacial bonding between graphene and aluminum alloy. Specifically, the addition of carbon nanotubes and silver nanoparticles provides more contact points and bonding sites between graphene and the aluminum alloy matrix, promoting electronic and thermal conduction between the two and further improving the interfacial bonding strength. Carbon nanotubes have extremely high thermal conductivity; the thermal conductivity of a single-walled carbon nanotube at room temperature is higher than 6000 W / (m·K), and the thermal conductivity of multi-walled carbon nanotubes is also higher than 3000 W / (m·K). The addition of silver nanoparticles further optimizes the conductive network and enhances the electromagnetic shielding effect. In particular, the combination of high-content graphene with multiple reinforcing phases (such as CNTs and silver nanoparticles) optimizes the material's electrical conductivity, thermal conductivity, and electromagnetic shielding performance. Compared to the comparative example, the materials in the embodiments exhibit significant advantages in these properties.
[0066] It should be noted that in stage S2, the main purpose of the low-temperature mixing process is to achieve nanoscale uniform dispersion of aluminum alloy powder, nano-sized ceramic particles, and functionalized graphene powder, ensuring that the components are fully mixed at the microscale without agglomeration. Adding carbon nanotubes and silver nanoparticles at this stage may interfere with this crucial dispersion process, increasing mixing complexity and reducing dispersion effectiveness. Therefore, adding a reinforcing phase in stage S3 allows for further optimization of the composite material's performance based on the already well-dispersed mixture A, while avoiding agglomeration problems that might arise from the addition of the reinforcing phase during low-temperature mixing, thus ensuring that the overall performance of the composite material reaches its optimal level.
[0067] Furthermore, in the S4 pressing stage, this invention employs graded pressure hot isostatic pressing (HIP) technology. By precisely controlling the pressure, temperature, and pressurization / heating rate, the densification and microstructure optimization of the composite material are achieved. The specific process control is as follows:
[0068] Initial stage: Under an inert gas protective environment, apply a pressure of 50-100 MPa while controlling the temperature within the range of 300-400℃ for 1 hour. During this process, closely monitor the pressure, temperature, and physical state of the mixture using a real-time monitoring system to ensure stable parameters and uniform pressure application. If pressure or temperature fluctuations are detected, the system will automatically adjust by increasing or decreasing the pressure or adjusting the heating power to maintain the set values. The allowable deviation range for pressure is ±2 MPa, and the allowable deviation range for temperature is ±5℃. This process aims to form a preform with a certain strength.
[0069] Gradual pressurization phase: Subsequently, the system gradually increases the pressure to 150-300 MPa at a pressurization rate of 4-5 MPa / min according to a preset program, while simultaneously raising the temperature to 400-600℃ at a heating rate of 4-5℃ / min. After reaching the target parameters, this temperature is maintained for 2 hours to ensure complete material densification and promote directional crystal growth. Throughout the pressing process, the data acquisition and control system continuously records various parameters for subsequent analysis and process optimization.
[0070] This graded pressing method, with its initial lower pressure and temperature, effectively prevents excessive deformation or agglomeration of graphene and nanoparticles under high temperature and pressure. This maintains the dispersion of nanoparticles while preventing damage to the graphene structure, laying a solid foundation for subsequent interfacial bonding. As the pressure and temperature gradually increase, the contact between graphene and the aluminum alloy matrix becomes increasingly tight, and the interfacial bonding force is significantly enhanced. This gradual densification process not only improves the material's density and strength but also optimizes its microstructure, providing a solid foundation for the subsequent sintering process.
[0071] It should be noted that the reason this invention employs graded pressure hot isostatic pressing (HIP) technology is that without gradual pressurization and heating, the internal porosity of the material cannot be completely eliminated, resulting in uneven density and significantly reduced mechanical properties in the final product. Furthermore, the lack of high-temperature and high-pressure conditions restricts directional crystal growth, reducing the material's toughness and strength. In addition, an unoptimized pressing process can easily lead to microstructural defects, thereby affecting the material's electrical conductivity, thermal conductivity, and electromagnetic shielding effectiveness. Therefore, graded pressure hot isostatic pressing is a crucial step in ensuring that the composite material achieves optimal performance, especially significant in enhancing the interfacial bonding between graphene and the aluminum alloy matrix.
[0072] Furthermore, a real-time monitoring system was introduced during the S4 pressing stage to improve the accuracy and stability of the material preparation process. This real-time monitoring system includes:
[0073] a) Pressure sensor, used to monitor the isotropic pressure distribution during the pressing process in real time, to ensure uniform pressure application and avoid material defects caused by uneven pressure.
[0074] b) Temperature sensor, used to accurately measure and control sintering temperature, avoid the impact of temperature fluctuations on material properties, and ensure the stability of microstructure and performance;
[0075] c) Displacement sensors are used to monitor dimensional changes in preforms, reduce material deformation during the pressing process, and ensure the accuracy and consistency of the final molding.
[0076] d) Data acquisition and control system: The computer control system automatically records and adjusts various parameters to improve the stability and repeatability of the process, reduce human error, and thus optimize product quality and production efficiency.
[0077] Specifically, the system utilizes a data acquisition module to collect data in real time from pressure, temperature, and displacement sensors, and transmits it to the central control unit. Based on preset process parameters and control algorithms, the central control unit analyzes and processes the collected data, automatically adjusting parameters such as pressure, temperature, and displacement during the pressing process. Simultaneously, the system supports real-time data recording and historical data retrieval, facilitating traceability and optimization of the production process. Furthermore, the system has an alarm function; when an anomaly is detected, it can promptly issue an alert and take appropriate measures.
[0078] By introducing a real-time monitoring system, this invention significantly improves the controllability and repeatability of the production process, providing a reliable technical guarantee for the preparation of high-performance composite materials.
[0079] Furthermore, in the S5 sintering stage, pulsed current assisted sintering (SPS) is used, with a sintering temperature of 500℃-700℃, a sintering time of 5-30 minutes, and a current density set at 100-500 A / cm². 2 .
[0080] Furthermore, in the S5 sintering stage, pulsed current-assisted sintering combined with a multi-stage heating program is adopted. The specific steps are as follows:
[0081] (1) Preheating stage: The temperature is slowly increased to 200-300℃ at a rate of 10-50℃ / min. The control of the heating rate and temperature in this stage is intended to effectively remove volatiles and adsorbed gases in the sample and prevent the formation of pores during subsequent sintering, thereby ensuring the compactness and performance of the material.
[0082] (2) Rapid heating stage: The temperature is rapidly increased to 500℃-700℃ at a rate of 100-300℃ / min. The higher heating rate helps to shorten the sintering time and reduce grain growth, thereby improving the strength and toughness of the material.
[0083] (3) Sintering stage: Hold at a sintering temperature of 500℃-700℃ for 5-30 minutes. This temperature and time range can ensure that the material is fully sintered and forms a stable microstructure.
[0084] (4) Cooling stage: Choose between natural cooling or forced cooling based on application requirements to optimize the microstructure and properties of the material. Forced cooling rate ≥ 50℃ / min can avoid grain growth or residual stress caused by improper cooling rate, thereby ensuring the final performance of the material.
[0085] This multi-stage heating program effectively controls temperature changes during sintering, ensuring the formation of a uniform and stable microstructure, thereby improving the overall performance of the material. Pulsed current-assisted sintering technology rapidly heats up and distributes heat evenly, promoting chemical reactions and diffusion between graphene and the aluminum alloy matrix, further enhancing interfacial bonding. Simultaneously, the multi-stage heating program prevents excessive grain growth, ensuring the material's high-temperature stability and density, thus improving its overall performance.
[0086] By optimizing the pressing and sintering parameters, the graphene-aluminum alloy composite material of this invention exhibits excellent hardness, tensile strength, and thermal shock resistance. Compared with traditional unoptimized aluminum alloy composite materials, this invention demonstrates superior performance in these aspects, particularly in the interfacial bonding force between graphene and aluminum alloy. Through optimization during the sintering stage, the interfacial bonding force is significantly enhanced, providing a crucial guarantee for the high-performance of the composite material.
[0087] Furthermore, in the S6 post-processing stage, the present invention further optimizes the performance of graphene-aluminum alloy composite material through multi-step heat treatment and surface coating treatment, while focusing on enhancing the interfacial bonding force between graphene and aluminum alloy.
[0088] The multi-step heat treatment includes annealing and aging. For example, annealing is first performed at 450℃~600℃ for 1~2 hours, followed by aging at 150℃~220℃ for 3~6 hours, and finally rapid cooling to room temperature using methods such as water cooling, oil cooling, or air cooling. This process can optimize the microstructure of the composite material, significantly improving its thermal shock resistance and dimensional stability. Especially at high temperatures, the material exhibits better stability and resistance to deformation, further enhancing its overall performance under complex working conditions.
[0089] The surface coating treatment involves adding one or two layers of ceramic, metal, or metal oxide coatings to the surface of the graphene-aluminum alloy composite material. The specific coating material is selected based on the application scenario and performance requirements of the composite material. Commonly used surface coating technologies include plasma spraying, physical vapor deposition (PVD), electroless nickel plating, and electrophoretic deposition.
[0090] For example, in highly abrasive and corrosive environments such as chemical and mining industries, ceramic coatings such as alumina (Al2O3) and zirconium oxide (ZrO2) (achieved through plasma spraying) are preferred, utilizing their high hardness and high chemical stability to significantly improve the wear resistance and corrosion resistance of composite materials. In the field of electronic devices, to balance conductivity and protection, metal coatings such as nickel (Ni) (using PVD or electroless nickel plating processes) are more suitable. And in applications requiring self-cleaning and photocatalytic performance, titanium dioxide (TiO2) metal oxide coatings (prepared through electrophoretic deposition) are the ideal choice.
[0091] For applications with extremely high protection requirements, a dual-layer coating structure can further enhance the protective effect. For example, a zirconium oxide (ZrO2) ceramic coating is first applied using electrophoretic deposition, leveraging its excellent corrosion resistance and high hardness to provide a basic protective layer. Then, a titanium dioxide (TiO2) metal oxide coating is applied to its surface using PVD technology. The TiO2 coating not only enhances corrosion resistance but also possesses self-cleaning properties, resisting the erosion of environmental pollutants. This synergistic effect of the dual-layer coating structure significantly enhances the material's wear resistance and corrosion resistance, thereby extending its service life.
[0092] It's important to note that coatings are not essential in all applications. In environments where wear resistance and corrosion resistance are not critical, uncoated composite materials can be used normally. However, the addition of a coating can significantly improve the performance of composite materials, especially in harsh environments. For example, studies have shown that the hardness of Al2O3-TiO2 composite ceramic coatings is approximately three times that of the base material, and its wear resistance is significantly improved, with wear rate only one-sixth that of the base material. Furthermore, the coating can effectively prevent the corrosion of the substrate by liquid heavy metals, providing excellent protection for the substrate.
[0093] Surface coating treatment not only improves the wear resistance and corrosion resistance of the composite material, but also further enhances the interfacial bonding between graphene and aluminum alloy through physical isolation and chemical stability. The coating can prevent external environmental erosion of the graphene-aluminum alloy interface and reduce chemical reactions at the interface, thereby maintaining the integrity and bonding strength of the interface. This enhanced interfacial bonding is one of the key factors for the composite material to maintain high performance under complex working conditions.
[0094] Therefore, the addition of coatings not only improves the surface properties of composite materials, but also plays an important role in protecting their internal structure and interface stability.
[0095] On the other hand, embodiments of the present invention provide a graphene-aluminum alloy composite material, which is prepared by the aforementioned preparation process and has the following composition: based on the total mass of the composite material, it contains 95% to 99.5% aluminum alloy matrix, 0.5% to 5% functionalized graphene, 0.1% to 3% nanoscale ceramic particle reinforcing phase, and 0.05% to 1% carbon nanotubes and / or nano-silver particles.
[0096] Compared with existing technologies, the graphene-aluminum alloy composite material provided in this embodiment achieves significant performance improvements through innovative processes. Surface functionalization treatment enhances the chemical bonding between graphene and aluminum alloy, improving mechanical properties and electrical conductivity. Low-temperature mixing ensures uniform nanoscale dispersion, optimizes the microstructure, and reduces internal defects. Furthermore, by adding carbon nanotubes and silver nanoparticles, the graphene-aluminum alloy composite material of this embodiment significantly improves electrical and thermal conductivity, while also enhancing electromagnetic shielding. Optimized pressing and sintering parameters, combined with multi-step heat treatment and rapid cooling processes, further improve the material's hardness, tensile strength, and thermal shock resistance. Surface coating treatment significantly improves wear resistance and corrosion resistance, extending service life. In summary, the graphene-aluminum alloy composite material of this embodiment has significant advantages in overall performance and can meet the application requirements of high-performance materials.
[0097] The present invention will be further described below with reference to the embodiments in conjunction with the specification, but the embodiments are only for the purpose of using the present invention and are not intended to limit the present invention.
[0098] Example 1
[0099] A powder metallurgical preparation process for graphene-aluminum alloy composite materials, such as Figure 1 As shown, it includes the following steps:
[0100] S1, Preprocessing stage:
[0101] Graphene underwent surface functionalization to introduce hydroxyl functional groups. The graphene was placed in an oxygen plasma treatment device, and the device parameters were adjusted to achieve a plasma power of 100W and maintain the pressure within the treatment chamber at 0.5Pa. Under these conditions, the graphene was treated for 30 minutes to introduce hydroxyl functional groups onto the graphene surface. After treatment, the functionalized graphene was dried in a 60℃ drying oven to remove moisture and complete the drying process, ultimately obtaining a mixture. A portion of this mixture, with a mass m of 1000g, was used for the next experimental step.
[0102] S2, Mixing Stage:
[0103] In a low-temperature environment (-100℃ to -150℃), a ball mill was used to mix 20g of functionalized graphene powder (particle size range 100–300nm), 980g of aluminum alloy powder (particle size range 10–50μm), and 5g of silicon carbide (SiC) nano-sized ceramic particles (particle size range 50–200nm) at a mass of m×2%=20g. The mixing time was 10 hours, the mixing speed was 300rpm, and the ball-to-particle ratio was 10:1.
[0104] S3. Add materials:
[0105] An additional 15g of silicon carbide (SiC) nano-ceramic particles (m×1.5%=15g) were added as a reinforcing phase; simultaneously, 3g of carbon nanotubes (CNTs) (m×0.3%=3g) were added to improve electrical and thermal conductivity. All powders were dispersed in an ultrasonic bath for 30 minutes to ensure uniform distribution.
[0106] S4, Suppression Phase:
[0107] Under argon protection, a hot isostatic press (HIP) was used for pressing. The initial pressure was 60 MPa, and the temperature was 350°C, maintained for 1 hour. During this process, a real-time monitoring system closely monitored the pressure, temperature, and physical state of the mixture to ensure stable parameters and uniform pressurization. If the pressure or temperature deviated from the set values, the system would automatically adjust, either by increasing or decreasing the pressure or adjusting the heating power to maintain the set values. The allowable deviation range for pressure was ±2 MPa, and the allowable deviation range for temperature was ±5°C. After 1 hour, the system gradually increased the pressure to 200 MPa at a pressurization rate of 5 MPa / min, while simultaneously raising the temperature to 500°C at a heating rate of 5°C / min, according to a preset program. After reaching the target parameters, the system maintained a constant pressure and temperature of 200 MPa and 500°C for 2 hours. Throughout the pressing process, the data acquisition and control system continuously recorded various parameters for subsequent analysis and process optimization.
[0108] S5, Sintering Stage:
[0109] A pulsed current-assisted sintering (SPS) apparatus was used, with a sintering temperature of 600℃, a holding time of 10 minutes, and a current density of 300 A / cm². 2 The preheating stage involves heating to 250℃ at a rate of 20℃ / min, the rapid heating stage involves heating to 600℃ at a rate of 200℃ / min, the holding stage involves maintaining the temperature for 10 minutes, and then allowing it to cool naturally.
[0110] S6. Post-processing stage:
[0111] Multi-step heat treatment: First, annealing at 500℃ for 1 hour, followed by aging at 180℃ for 4 hours. Rapid cooling to room temperature using water cooling method. Surface coating treatment: Applying an alumina (Al2O3) ceramic coating with a thickness of approximately 50μm using plasma spraying.
[0112] Example 2
[0113] A powder metallurgical preparation process for graphene-aluminum alloy composite materials includes the following steps:
[0114] S1, Preprocessing stage:
[0115] Graphene underwent surface functionalization to introduce amino functional groups. The graphene was placed in a 30% ammonia solution, ensuring complete immersion. At room temperature, the graphene was immersed in the ammonia solution for 24 hours to allow the amino functional groups to fully integrate onto the graphene surface. After immersion, the graphene was removed from the ammonia solution and rinsed repeatedly with deionized water to remove residual ammonia. Subsequently, the graphene was placed in a drying oven at 60°C to remove moisture and complete the drying process, ultimately obtaining a mixture. A portion of this mixture, with a mass m of 1000g, was used for the next experimental step.
[0116] S2, Mixing Stage:
[0117] In a low-temperature environment (-100℃ to -150℃), 40g of graphene (particle size range 100–300nm), 960g of aluminum alloy powder (particle size range 10–50μm), and 10g of aluminum nitride (AlN) nano-sized ceramic particles (particle size range 50–200nm) were mixed using a ball mill. The mixing time was 12 hours, the mixing speed was 350 rpm, and the ball-to-particle ratio was 12:1.
[0118] S3. Add materials:
[0119] Additional aluminum nitride (AlN) nano-ceramic particles (m×2%=20g) were added as a reinforcing phase; simultaneously, nano-silver (Ag) particles (m×0.8%=8g) were added to improve conductivity and antibacterial properties. All powders were dispersed in an ultrasonic bath for 40 minutes.
[0120] S4, Suppression Phase:
[0121] Under argon protection, a hot isostatic press (HIP) was used for pressing. The initial pressure was 80 MPa, and the temperature was 350 °C, maintained for 1 hour. During this process, a real-time monitoring system closely monitored the pressure, temperature, and physical state of the mixture to ensure stable parameters and uniform pressurization. If pressure or temperature fluctuations were detected, the system would automatically adjust, either by increasing or decreasing the pressure or adjusting the heating power to maintain the set values. The allowable deviation range for pressure was ±2 MPa, and for temperature, ±5 °C. After 1 hour, the system gradually increased the pressure to 250 MPa at a pressurization rate of 4 MPa / min according to a preset program, while simultaneously raising the temperature to 550 °C at a heating rate of 4 °C / min. After reaching the target parameters, the system maintained a constant pressure and temperature of 250 MPa and 550 °C for 2 hours. Throughout the pressing process, the data acquisition and control system continuously recorded various parameters for subsequent analysis and process optimization.
[0122] S5, Sintering Stage:
[0123] Using an SPS (Spectrophotometer-Sintered Pulse Control) system, the sintering temperature was 650℃, the holding time was 20 minutes, and the current density was 400 A / cm². 2 The preheating stage involves heating to 300℃ at a rate of 30℃ / min, the rapid heating stage involves heating to 650℃ at a rate of 250℃ / min, the holding stage involves maintaining the temperature for 20 minutes, and then forced cooling.
[0124] S6. Post-processing stage:
[0125] Multi-step heat treatment: First, annealing at 550℃ for 1.5 hours, followed by aging at 200℃ for 5 hours. Rapid cooling to room temperature using oil cooling method. Surface coating treatment: A titanium dioxide (TiO2) metal oxide coating with a thickness of approximately 30 μm is applied using physical vapor deposition (PVD) technology.
[0126] Example 3
[0127] A powder metallurgical preparation process for graphene-aluminum alloy composite materials includes the following steps:
[0128] S1, Preprocessing stage:
[0129] Carboxyl functional groups were introduced into the graphene through acid treatment. The graphene was soaked in a mixture of concentrated sulfuric acid and nitric acid for 12 hours, followed by washing and drying.
[0130] S2, Mixing Stage:
[0131] In a low-temperature environment (-100℃ to -150℃), 10g of graphene (particle size range 50–200nm), 990g of aluminum alloy powder (particle size range 10–50μm), and 3g of titanium diboride (TiB2) nano-sized ceramic particles (particle size range 50–200nm) were mixed using a ball mill. The mixing time was 8 hours, the mixing speed was 300 rpm, and the ball-to-particle ratio was 10:1.
[0132] S3. Add materials:
[0133] An additional m × 0.5% = 5g of titanium diboride (TiB2) nano-ceramic particles were added as a reinforcing phase; no additional carbon nanotubes or silver nanoparticles were added.
[0134] S4, Suppression Phase:
[0135] Under argon protection, a hot isostatic press (HIP) was used for pressing. The initial pressure was 70 MPa, and the temperature was 300 °C, maintained for 1 hour. During this process, a real-time monitoring system closely monitored the pressure, temperature, and physical state of the mixture to ensure stable parameters and uniform pressurization. If pressure or temperature fluctuations were detected, the system would automatically adjust, either by increasing or decreasing the pressure or adjusting the heating power to maintain the set values. The allowable deviation range for pressure was ±2 MPa, and for temperature, ±5 °C. After 1 hour, the system gradually increased the pressure to 220 MPa at a pressurization rate of 5 MPa / min according to a preset program, while simultaneously raising the temperature to 450 °C at a heating rate of 5 °C / min. After reaching the target parameters, the system maintained a constant pressure and temperature of 220 MPa and 450 °C for 2 hours. Throughout the pressing process, the data acquisition and control system continuously recorded various parameters for subsequent analysis and process optimization.
[0136] S5, Sintering Stage:
[0137] Using an SPS (Spectroscopy-Based Pulse Control) system, the sintering temperature was 550℃, the holding time was 15 minutes, and the current density was 250 A / cm². 2 The preheating stage involves raising the temperature to 250°C at a rate of 20°C / min, the rapid heating stage involves raising the temperature to 550°C at a rate of 200°C / min, the holding stage involves maintaining the temperature for 15 minutes, and then allowing it to cool naturally.
[0138] S6. Post-processing stage:
[0139] Multi-step heat treatment: First, annealing at 450℃ for 1 hour, followed by aging at 150℃ for 3 hours. Rapid cooling to room temperature using air cooling. Surface coating treatment: A nickel coating with a thickness of approximately 20μm is formed using electroless nickel plating.
[0140] Example 4
[0141] A powder metallurgical preparation process for graphene-aluminum alloy composite materials includes the following steps:
[0142] S1, Preprocessing stage:
[0143] Graphene was infused with hydroxyl and amino functional groups through treatment with mixed oxygen plasma and ammonia. The treatment time was 45 minutes, the power was 120 W, and the pressure was 0.5 Pa; the graphene was then soaked in ammonia for 24 hours, followed by drying.
[0144] S2, Mixing Stage:
[0145] A ball mill was used to mix 50g of graphene (particle size range 10–100nm), 950g of aluminum alloy powder (particle size range 30–100μm), and 12g of mixed silicon carbide (SiC) and aluminum nitride (AlN) nanoscale ceramic particles (silicon carbide particle size range 20–150nm, aluminum nitride particle size range 30–120nm) in a low-temperature environment (-100℃ to -150℃). The mixing time was 15 hours, the rotation speed was 400 rpm, and the ball-to-particle ratio was 15:1.
[0146] S3. Add materials:
[0147] An additional 25g of mixed silicon carbide (SiC) and aluminum nitride (AlN) nanoscale ceramic particles (m×2.5%=25g) were added as a reinforcing phase; simultaneously, 5g of carbon nanotubes (CNTs) and silver nanoparticles (Ag) were added to improve electrical and thermal conductivity. All powders were dispersed in an ultrasonic bath for 60 minutes.
[0148] S4, Suppression Phase:
[0149] Under argon protection, a hot isostatic press (HIP) was used for pressing. The initial pressure was 100 MPa, and the temperature was 400 °C, maintained for 1 hour. During this process, a real-time monitoring system closely monitored the pressure, temperature, and physical state of the mixture to ensure stable parameters and uniform pressurization. If pressure or temperature fluctuations were detected, the system would automatically adjust, increasing or decreasing the pressure or adjusting the heating power to maintain the set values. The allowable deviation range for pressure was ±2 MPa, and the allowable deviation range for temperature was ±5 °C. After 1 hour, the system gradually increased the pressure to 300 MPa at a pressurization rate of 4 MPa / min according to a preset program, while simultaneously raising the temperature to 600 °C at a heating rate of 4 °C / min, maintaining this temperature for 2 hours. Throughout the pressing process, the data acquisition and control system continuously recorded various parameters for subsequent analysis and process optimization.
[0150] S5, Sintering Stage:
[0151] Using an SPS (Spectrophotometer-Sintered Pulse Control) system, the sintering temperature was 700℃, the holding time was 30 minutes, and the current density was 500 A / cm². 2 The preheating stage involves heating to 300℃ at a rate of 50℃ / min, the rapid heating stage involves heating to 700℃ at a rate of 300℃ / min, the holding stage involves maintaining the temperature for 30 minutes, and then forced cooling.
[0152] S6. Post-processing stage:
[0153] Multi-step heat treatment: First, annealing at 600℃ for 2 hours, followed by aging at 220℃ for 6 hours. Rapid cooling to room temperature using water cooling method. Surface coating treatment: A zirconium oxide (ZrO2) ceramic coating with a thickness of approximately 80 μm was coated using electrophoretic deposition, followed by a titanium dioxide (TiO2) metal oxide coating with a thickness of approximately 20 μm using PVD technology.
[0154] Example 5
[0155] The preparation process is the same as in Example 1, except for the parameters in the S4 pressing stage:
[0156] Initial pressure: 80 MPa
[0157] Temperature: 380℃
[0158] After maintaining this pressure for 1 hour, gradually increase the pressure to 250 MPa at a pressurization rate of 4 MPa / min, while simultaneously raising the temperature to 550 °C at a heating rate of 4 °C / min. Once the target parameters are reached, maintain a constant pressure and temperature of 250 MPa and 550 °C for 2 hours.
[0159] Example 6
[0160] The preparation process is the same as in Example 1, except for the parameters in the S5 sintering stage:
[0161] Sintering temperature: 650℃
[0162] Duration: 15 minutes
[0163] Current density: 350A / cm 2
[0164] During the preheating stage, the temperature is increased to 300℃ at a rate of 30℃ / min. During the rapid heating stage, the temperature is increased to 650℃ at a rate of 250℃ / min. During the heat preservation stage, the temperature is maintained for 15 minutes, followed by natural cooling.
[0165] Comparative Example 1
[0166] The difference from Example 1 is that no graphene surface functionalization treatment was performed; raw graphene was used directly.
[0167] Comparative Example 2
[0168] The difference from Example 1 is that the mixing stage was not carried out in a low-temperature environment, but at room temperature (about 25°C).
[0169] Comparative Example 3
[0170] The difference from Example 1 is that the amount of graphene powder added during the mixing stage is too high (m×10%=100g).
[0171] Comparative Example 4
[0172] The difference from Example 1 is that in the material addition stage, the amount of additional silicon carbide (SiC) nano-sized ceramic particles added is too high (m×5%=50g).
[0173] Comparative Example 5
[0174] The only difference from Example 1 is that no surface coating treatment was performed in the S6 post-processing stage.
[0175] Comparative Example 6
[0176] The difference from Example 1 is that the components that should have been added later were directly added during the mixing stage, which resulted in damage to the microstructure and interfacial bonding strength of the material.
[0177] Table 1 Summary of Performance Data for Examples and Comparative Examples
[0178]
[0179] Characterization results analysis
[0180] Examples 1-6 demonstrate that surface functionalization significantly enhances the bonding strength between graphene and the aluminum alloy substrate, achieving a hardness of 135-245 HV, tensile strength of 320-580 MPa, electrical conductivity of 0.5-0.9 IACS, thermal conductivity of 160-280 W / m·K, and wear resistance of 0.5-3.5 × 10⁻⁶. -5 mm 3 / N·m, corrosion resistance is 600-1500 hours. In contrast, Comparative Examples 1-6, due to lack of surface functionalization treatment or improper mixing conditions, have significantly lower performance than the examples, with hardness only 95-180 HV, tensile strength 280-450 MPa, electrical conductivity 0.4-0.72 IACS, thermal conductivity 120-205 W / m·K, and abrasion resistance (2.5~8)×10 -5 mm 3 / N·m, corrosion resistance is 200-700 hours.
[0181] In summary, the preparation process of this invention significantly improves the overall performance of graphene-aluminum alloy composite materials through surface functionalization treatment, low-temperature mixing, precise control of the additive amount, and optimized post-treatment processes. The synergistic effect between these process steps ensures excellent performance of the material in terms of hardness, tensile strength, electrical conductivity, thermal conductivity, wear resistance, and corrosion resistance.
[0182] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A powder metallurgy preparation process for graphene-aluminum alloy composite materials, characterized in that, Includes the following steps: S1. Pretreatment stage: Graphene is surface functionalized by introducing oxygen- or nitrogen-containing functional groups. After the treatment is completed, the functionalized graphene is dried. S2. Mixing stage: Aluminum alloy powder, nano-sized ceramic particles and functionalized graphene powder are mixed in a low temperature environment of -100℃ to -150℃ to obtain mixture A. S3, Adding materials: Add additional nanoscale ceramic particles as a reinforcing phase to mixture A obtained in S2; simultaneously add carbon nanotubes and / or silver nanoparticles; S4, Pressing stage: The mixture after S3 treatment is pressed using staged pressure hot isostatic pressing technology; S5, Sintering stage: The product pressed in S4 is sintered with pulsed current assisted sintering. S6. Post-treatment stage: The composite material after S5 sintering is subjected to a multi-step heat treatment combined with rapid cooling; then the composite material is coated with a surface coating.
2. The preparation process according to claim 1, characterized in that, In S1, the oxygen-containing functional groups introduced by the surface functionalization treatment include carboxyl and hydroxyl groups, and the nitrogen-containing functional groups include amino groups.
3. The preparation process according to claim 1, characterized in that, In S2, based on the total mass m of mixture A, the mass of the functionalized graphene powder is m×(0.5~5)%, and the mass of the aluminum alloy powder is m×(95~99.5)%.
4. The preparation process according to claim 1, characterized in that, The nanoscale ceramic particles described in S2 and / or S3 include one or more of silicon carbide, aluminum nitride, or titanium diboride.
5. The preparation process according to claim 1, characterized in that, In S3, based on the total mass m of mixture A, the amount of additional nano-sized ceramic particles added is m×(0.1~3)%, and the amount of carbon nanotubes and / or silver nanoparticles added is m×(0.05~1)%.
6. The preparation process according to claim 1, characterized in that, In the S4 pressing stage, staged pressure hot isostatic pressing technology is used for pressing. The specific steps are as follows: Initial stage: Under the protection of inert gas, a pressure of 50-100MPa is first applied, while the temperature is controlled within the range of 300-400℃, in order to form a preform with a certain strength; Gradual pressurization stage: The pressure is then gradually increased to 150-300 MPa, while the temperature is raised to 400-600℃ to ensure complete densification of the material and promote directional crystal growth.
7. The preparation process according to claim 1, characterized in that, In the S5 sintering stage, pulsed current-assisted sintering was used, with a sintering temperature of 500℃-700℃, a sintering time of 5-30 minutes, and a current density set to 100-500 A / cm². 2 .
8. The preparation process according to claim 8, characterized in that, In the S5 sintering stage, the pulsed current-assisted sintering employs a multi-stage heating program, with the specific steps as follows: (1) Preheating stage: slowly increase the temperature to 200-300℃ at a rate of 10-50℃ / min to remove volatiles and adsorbed gases from the sample; (2) Rapid heating stage: rapidly heat to sintering temperature of 500℃-700℃ at a rate of 100-300℃ / min to shorten sintering time and reduce grain growth; (3) Sintering stage: Hold at a sintering temperature of 500℃-700℃ for 5-30 minutes to ensure that the material is fully sintered and forms a stable microstructure; (4) Cooling stage: Natural cooling or forced cooling is adopted; the cooling rate of forced cooling is ≥50℃ / min.
9. The preparation process according to claim 1, characterized in that, In the S6 post-processing stage, the multi-step heat treatment includes annealing and aging; the surface coating treatment forms a ceramic, metal, or metal oxide coating on the surface of the graphene aluminum alloy composite material.
10. A graphene-aluminum alloy composite material, characterized in that, It is prepared by the preparation process described in any one of claims 1-9.