A method for preparing a hierarchical porous copper-based material, the resulting product and applications thereof

By using vapor phase alloying and dealloying techniques, a hierarchical porous copper-based material was prepared, which solved the problems of high stability and high cost of porous materials in the existing technology. This method achieves efficient and environmentally friendly preparation of hierarchical porous structures with excellent mechanical properties and industrialization potential.

CN123152913APending Publication Date: 2026-11-24SHANDONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611178880.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the efficient and environmentally friendly preparation of hierarchical porous metal materials. Furthermore, traditional processes are complex, costly, and fail to achieve the construction of multi-level channels, resulting in insufficient material stability.

Method used

By employing vapor phase alloying and dealloying techniques, alloying with a hierarchical pore structure is achieved through vapor phase deposition and selective dealloying processes combined with solid-state diffusion.

Benefits of technology

It achieves a complex and highly controllable hierarchical porous structure, which improves the mechanical stability and structural integrity of the material, reduces production costs, and has broad prospects for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152913A_ABST
    Figure CN123152913A_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a hierarchical porous copper-based material, and a product and application thereof. The method selects pure copper or a copper-based alloy with a thickness of 30-300 microns as a substrate, and adopts a combined process of "gas phase alloying-gas phase dealloying-second alloying-second dealloying" to successfully prepare the copper-based material with a hierarchical porous structure. The method has the advantages of easy raw material, high process repeatability, low equipment requirement and easy batch production. The obtained material is continuous and free of macroscopic cracks, and has a hierarchical structure of primary pores (about 5-30 microns) and secondary pores (about 0.1-3 microns). The material has a high specific surface area and a self-supporting conductive framework, can provide abundant active sites and promote electron transmission, and has a wide application prospect in the fields of electrocatalysis (such as carbon dioxide reduction, water electrolysis), lithium ion batteries, solar water evaporation and biomedicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a hierarchical porous copper-based material, specifically a method for preparing a hierarchical porous copper-based material based on vapor phase alloying and dealloying technology, and also relates to the product obtained by this method and its application, belonging to the field of porous metal materials technology. Background Technology

[0002] Porous metallic materials, as a novel type of functional material, exhibit broad application prospects in fields such as filtration and separation, catalytic reactions, electrochemical sensing, and energy storage and conversion due to their high specific surface area, unique surface activity, and excellent mass transfer properties. Metallic materials with hierarchical porous structures, in particular, can simultaneously achieve high-efficiency mass transport and abundant active sites, making them a current research hotspot in porous materials. In existing technologies, while chemical / electrochemical dealloying methods are relatively simple, the preparation of precursor alloys typically requires complex processes such as melting and rapid solidification. Furthermore, the alloy composition is limited by thermodynamic equilibrium, and the use of reagents such as acids and alkalis during dealloying is environmentally unfriendly (e.g., CN122235518A, CN111254309A). Although template methods can prepare ordered porous structures, the template removal process often affects the integrity of the pore structure and makes it difficult to construct hierarchical channels.

[0003] Combining vapor deposition with dealloying technology, alloying is achieved through solid-state diffusion, and then porous structures are obtained through selective dealloying, providing a new technical approach for the preparation of hierarchical porous metallic materials. Therefore, developing a simple, low-cost method for preparing metallic materials that can precisely control hierarchical pore structures has significant scientific and practical application value. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a method for preparing hierarchical porous copper-based materials. This method is simple, low-cost, and easy to mass-produce, and the resulting product has a hierarchical porous structure and excellent performance.

[0005] The specific technical solution of this invention is as follows: A method for preparing a hierarchical porous copper-based material, the method comprising the following steps: (1) Using pure copper or copper-based alloy with a thickness of 30-300μm as the substrate, the substrate and zinc particles are placed in a reactor in a non-contact manner, the air in the reactor is replaced with inert gas, and then the first gas phase alloying treatment is carried out by heating under low pressure. After the treatment is completed, the sample is cooled to room temperature in the furnace to obtain the first alloyed sample. (2) The first alloyed sample was subjected to the first gas phase dealloying treatment in a mixed atmosphere of flowing inert gas and hydrogen under low pressure. After the treatment, it was cooled to room temperature in the furnace to obtain the first dealloyed sample. (3) Place the first dealloyed sample and zinc granules into both ends of the glass tube, and place a barrier with a diameter smaller than that of the glass tube between the first dealloyed sample and zinc granules. Replace the air in the glass tube with inert gas and evacuate it. Then seal the glass tube. (4) The sealed glass tube is heated to perform a second vapor phase alloying treatment. After the treatment, it is cooled to 300-450℃ in the furnace and then taken out and cooled to room temperature in air to obtain the second alloyed sample. (5) The second alloyed sample was taken out of the glass tube and subjected to a second vapor-phase dealloying treatment under a mixed atmosphere of flowing inert gas and hydrogen at low pressure. After the treatment, it was cooled to room temperature with the furnace to obtain a graded porous copper-based material.

[0006] Furthermore, in step (1), the substrate is a pure copper foil or a copper-based alloy foil, and the thickness of the substrate is 30-300 μm, for example, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 150μm, 200μm, 250μm, 300μm.

[0007] Furthermore, in step (1), the copper-based alloy is an alloy formed by Cu and other metals, and the other metals are at least one of Sn, Si, Sb, Ni, Pt, Pd, Ag, Au, and Ti; preferably, the atomic fraction of copper in the copper-based alloy is greater than 50%, for example, 51%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, etc.

[0008] Furthermore, in step (1), the substrate is cut to a preset size, then ultrasonically cleaned with anhydrous ethanol and dried, and then set aside for use.

[0009] Furthermore, in step (1), the mass ratio of the substrate to zinc granules is 1:2-3 to ensure sufficient zinc vapor is provided during alloying. The substrate and zinc granules are placed at opposite ends of the reactor, without contact, so that the zinc vapor generated during heating can diffuse evenly to the substrate surface. A gas replacement operation is required before alloying: the pressure inside the reactor is evacuated to below 20 Pa using a vacuum pump, and then inert gas is introduced to atmospheric pressure. This replacement operation is repeated 2 to 3 times. The inert gas is argon, nitrogen, etc.

[0010] Furthermore, in step (1), the first vapor phase alloying treatment can be carried out in a tube furnace with a system vacuum degree of less than 20 Pa and a temperature of 550-700℃, such as 550℃, 600℃, 650℃, 700℃, and a holding time of 60-150 min, such as 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min.

[0011] Furthermore, in step (2), the first vapor-phase dealloying treatment is carried out in a tube furnace. The first alloying sample is placed in the tube furnace, and the air in the furnace is replaced with a mixture of inert gas and hydrogen. Then, the vacuum valve is kept open, and the intake volume of the mixture of inert gas and hydrogen is controlled by adjusting the intake valve to maintain the system vacuum at 100-300 Pa. In the mixture of inert gas and hydrogen, the volume fraction of hydrogen is 5-10%, for example, 5%, 6%, 7%, 8%, 9%, or 10%. The inert gas is nitrogen, argon, or other inert gases.

[0012] Furthermore, in step (2), during the first vapor phase dealloying treatment, the dynamic evacuation and inlet are kept in balance, the vacuum degree in the system is maintained at 100-300 Pa, the temperature is 600-750 ℃, for example 600℃, 650℃, 700℃, 750℃, and the holding time is 70-120 min, for example 70 min, 80 min, 90 min, 100 min, 110 min, 120 min.

[0013] Furthermore, the first dealloyed sample obtained after the first vapor-phase dealloying treatment has a primary porous structure.

[0014] Furthermore, in step (3), the mass ratio of the first dealloyed sample to zinc particles is 1:2-3 to ensure that there is a saturated zinc vapor partial pressure in the system during the secondary vapor phase alloying process.

[0015] Furthermore, in step (3), the first dealloyed sample and zinc granules are placed in a glass tube, and a barrier is placed between them to isolate them spatially, so that only a small amount of zinc vapor comes into contact with the first dealloyed sample. The barrier can be a glass plug with a diameter smaller than that of the glass tube, and the glass plug can slide freely in the glass tube.

[0016] Furthermore, in step (3), the air inside the glass tube is replaced with an inert gas, and then the glass tube is evacuated to a vacuum level of less than 20 Pa. Then, the glass tube is welded and sealed under vacuum.

[0017] Furthermore, in step (4), the second vapor phase alloying treatment is carried out in a muffle furnace at a temperature of 550-650℃, for example, 550℃, 600℃, or 650℃, and a holding time of 5-20 min, for example, 5 min, 10 min, 15 min, or 20 min. By controlling the holding time and a specific cooling procedure, the penetration depth and concentration of zinc are controlled through short-time alloying, thereby obtaining a surface alloy with low zinc content.

[0018] Furthermore, in step (5), the second vapor-phase dealloying treatment is carried out in a tube furnace. The sample to be alloyed in the second stage is placed inside the tube furnace, and the air inside the furnace is replaced with a mixture of inert gas and hydrogen. Then, the vacuum valve is kept open, and the intake volume of the mixture of inert gas and hydrogen is controlled by adjusting the intake valve to maintain the system vacuum at 100-300 Pa. In the mixture of inert gas and hydrogen, the volume fraction of hydrogen is 5-10%, for example, 5%, 6%, 7%, 8%, 9%, or 10%. The inert gas is nitrogen, argon, or other inert gases.

[0019] Furthermore, in step (5), during the second vapor-phase dealloying treatment, the vacuum level in the system is 100-300 Pa, the temperature is 550-650 ℃ (e.g., 550℃, 600℃, 650℃), and the holding time is 5-20 min (e.g., 5 min, 10 min, 15 min, 20 min). Through short-term holding, secondary pores are generated in situ on the primary pore ligaments of the sample, while inhibiting the coarsening or "healing" phenomenon of the primary pores due to prolonged high-temperature heat exposure.

[0020] Furthermore, the resulting hierarchical porous copper-based material has a two-stage porous structure. The size of the primary pores is approximately 5-30 μm, and the size of the secondary pores is approximately 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0021] The present invention also provides a hierarchical porous copper-based material prepared according to the above method.

[0022] The present invention also provides the application of the above-mentioned hierarchical porous copper-based material in electrocatalytic reduction of CO2 and / or electrolysis of water and / or lithium-ion batteries.

[0023] This invention employs a combined process of "vapor phase alloying - vapor phase dealloying - secondary vapor phase alloying - secondary vapor phase dealloying" to successfully prepare copper-based metal materials with a hierarchical porous structure. Compared with existing technologies, this invention has the following significant advantages: (1) A complex and highly controllable hierarchical porous structure has been achieved, completely overcoming the pore collapse problem of traditional processes. Traditional liquid-phase dealloying processes inevitably involve capillary forces during drying, easily leading to pore structure collapse and ligament aggregation, making it difficult to construct a stable hierarchical porous network. This invention innovatively employs a gas-phase reaction mechanism, achieving dealloying through the preferential volatilization of target elements, fundamentally eliminating the damage to the microstructure caused by liquid-gas interfacial tension. The prepared material possesses a typical "dual-modal" hierarchical porous structure, which combines an extremely high specific surface area (providing abundant active sites for applications such as electrocatalysis) with excellent open mass transfer channels (significantly reducing diffusion resistance and improving reaction kinetic efficiency).

[0024] (2) Significantly improved mechanical stability and structural integrity of the material. The vapor-phase dealloying process avoids solvent immersion and surface tension impact in the liquid-phase method. The resulting hierarchical porous material exhibits a highly continuous "ligament-channel" bicontinuous topology with strong node connections and no macroscopic cracks. This structure endows the material with excellent mechanical strength, toughness, and anti-collapse ability, enabling it to maintain extremely high physical stability in complex service environments (such as repeated alternating stress, long-term electrocatalysis, or thermal cycling tests), greatly extending its actual service life as a key functional electrode or core device.

[0025] (3) The process is green and environmentally friendly, with significant energy efficiency and industrial mass production potential. The process of this invention completely eliminates the dependence of traditional liquid-phase dealloying on strong acids, strong alkalis, or corrosive salt electrolytes, achieving "zero waste liquid" discharge in the production process. This pure gas-phase process route is clean and friendly, reducing the economic cost and environmental burden of subsequent "three wastes" treatment from the source. At the same time, the high-temperature gas-phase alloying and dealloying processes are both completed in a closed reaction furnace, resulting in high system thermal energy utilization efficiency, a compact and controllable process flow, and great industrial application prospects for large-scale production.

[0026] (4) The raw materials of the present invention are readily available, the process is highly repeatable, the equipment requirements are low, and it is easy to mass produce. The resulting material is continuous, free of macroscopic cracks, and has a hierarchical structure of primary pores (about 5-30 μm) and secondary pores (about 0.1-3 μm). This material has a high specific surface area and a self-supporting conductive framework, which can provide abundant active sites and promote electron transport. It has broad application prospects in electrocatalysis (such as carbon dioxide reduction and water electrolysis), lithium-ion batteries, solar water evaporation, and biomedicine. Attached Figure Description

[0027] Figure 1 This is the X-ray diffraction pattern of the sample after the first vapor-phase alloying in Example 1 of the present invention. The horizontal axis represents angle, and the vertical axis represents intensity.

[0028] Figure 2This is the X-ray diffraction pattern of the sample after the first vapor-phase dealloying in Example 1 of this invention. The horizontal axis represents angle, and the vertical axis represents intensity.

[0029] Figure 3 This is the X-ray diffraction pattern of the sample after the second vapor-phase alloying in Example 1 of the present invention. The horizontal axis represents angle, and the vertical axis represents intensity.

[0030] Figure 4 This is the X-ray diffraction pattern of the sample after the second vapor-phase dealloying in Example 1 of this invention. The horizontal axis represents angle, and the vertical axis represents intensity.

[0031] Figure 5 These are macroscopic photographs of the alloying and dealloying processes in Example 1 of the present invention, where a is the precursor copper foil, b is the sample after the first alloying, c is the sample after the first dealloying, d is the sample after the second alloying, e is the graded porous copper-based material after the second dealloying, and f is the sample after the second alloying sealed in a glass tube.

[0032] Figure 6 The images are scanning electron microscope (SEM) images of the porous metal material obtained after the first vapor-phase dealloying in Example 1 of this invention (a is the surface, b is the cross-section).

[0033] Figure 7 The images are scanning electron microscope (SEM) images of the hierarchical porous copper-based material obtained after the second vapor-phase dealloying in Example 1 of the present invention (a and b are the surface, and c and d are the cross-sections).

[0034] Figure 8 The performance and stability of the hierarchical porous copper-based material obtained after the second vapor-phase dealloying in Example 2 of this invention were tested in an H-type electrolytic cell at -1.0 V vs. RHE for the electrocatalytic reduction of CO2. The right axis represents the Faraday efficiency of hydrogen evolution, and the left axis represents the current.

[0035] Figure 9 This invention provides a test of the electrocatalytic reduction performance of porous copper-based material obtained after the first gas-phase dealloying in Comparative Example 1 of the present invention on CO2 reduction under H-type electrolytic cells at -0.6 to -1.2 V vs. RHE. Detailed Implementation

[0036] The present invention will be further described below with reference to the embodiments and accompanying drawings. The following description is only for explaining the present invention and does not limit the content.

[0037] Unless otherwise specified, the argon-hydrogen mixture in the following examples and comparative examples is a mixture of argon and hydrogen, with a hydrogen volume fraction of 8%.

[0038] Example 1 A method for preparing a hierarchical porous copper-based material includes the following steps: (1) Select a pure copper foil substrate with a thickness of 50 μm, cut it to the preset size, ultrasonically clean it with anhydrous ethanol and dry it for later use; (2) Weigh 1.00 g of the copper foil substrate after pretreatment in step (1), and weigh 2.00 g of high-purity zinc granules at a mass ratio of 1:2 for later use; (3) Copper foil and zinc granules are placed in a tube furnace in a non-contact manner. After argon gas washing, the system gas pressure is controlled to below 20 Pa. The temperature is heated to 600 ℃ at a rate of 10 ℃ / min and held for 120 min. After holding, the temperature is cooled to room temperature with the furnace to obtain copper-zinc precursor alloy. (4) The copper-zinc precursor alloy was placed in a tube furnace and washed with argon-hydrogen mixed gas. The vacuum valve was kept open. The system pressure was controlled to be 200 Pa by adjusting the argon-hydrogen mixed gas inlet valve. Then it was heated to 650 °C and held for 90 min. After holding, it was cooled to room temperature with the furnace to obtain the first dealloying sample with a primary porous structure. (5) Weigh 0.50 g of the first dealloyed sample, and then accurately weigh 1.00 g of high-purity zinc granules at a mass ratio of 1:2 for later use; (6) The first dealloyed sample and zinc particles were placed at both ends of a glass tube and isolated between them with a glass stopper. The glass stopper could move in the glass tube. After argon gas washing, the glass tube was welded and sealed under a vacuum of less than 20 Pa. (7) Place the sealed glass tube in a muffle furnace, heat it to 600 ℃ and hold it for 10 min for a short time. After holding, cool it with the furnace to 400 ℃ and take it out. Cool it to room temperature in the air to obtain the second alloying sample. (8) Take out the second alloying sample and place it in a tube furnace. After purging with an argon-hydrogen mixture, keep the vacuum valve open. Control the system pressure to 200 Pa by adjusting the argon-hydrogen mixture inlet valve. Heat to 600 ℃ and hold for 10 min. After holding, cool to room temperature with the furnace to obtain a graded porous copper-based material. The size of the primary pores in the material is 5-30 μm, and the size of the secondary pores is 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0039] Figure 1 The image shows the XRD pattern of the sample after the first vapor phase alloying. It can be seen that the copper-zinc precursor alloy after alloying is Cu5Zn8 phase.

[0040] Figure 2 The image shows the XRD pattern of the sample after the first vapor-phase dealloying, which indicates that the obtained sample is a single Cu phase.

[0041] Figure 3 The image shows the XRD pattern of the sample after the second vapor phase alloying. It can be seen that the sample after the second alloying is of the CuZn phase.

[0042] Figure 4 The image shows the XRD pattern of the sample after the second vapor-phase dealloying, which indicates that the obtained sample is a single Cu phase.

[0043] Figure 5 These are macroscopic photographs of the samples during the alloying and dealloying processes. In the figures, a is the precursor copper foil, b is the sample after the first alloying, c is the sample after the first dealloying, d is the sample after the second alloying, e is the hierarchical porous copper-based material obtained after the second dealloying, and f is the sample sealed in a glass tube after the second alloying. As can be seen from the figures, the sample after the first alloying is silvery-white and slightly expanded in size; after the first dealloying, the color changes to dark orange and the size shrinks; after the second alloying, the sample turns dark yellow and its size does not change significantly compared to the sample after the first dealloying; after the second dealloying, the sample returns to dark orange with minimal size change.

[0044] Figure 6 The images show scanning electron microscope (SEM) images of the porous metallic material obtained after the first vapor-phase dealloying (a is the surface, b is the cross-section). As can be seen from the images, a uniform three-dimensional continuous network structure is formed both inside and outside the sample surface. The material is macroscopically continuous without cracks, and the pore size ranges from 5 to 30 μm.

[0045] Figure 7 The images show scanning electron microscope (SEM) images of the hierarchical porous copper-based material obtained after the second vapor-phase dealloying process (a and b are surface views, c and d are cross-sections). As can be seen from the images, uniformly shaped secondary pores are formed on the sample surface and within a certain depth range, in addition to the primary pores, and the size of these secondary pores ranges from 0.1 to 3 μm.

[0046] Example 2 In addition to selecting Cu with a thickness of 50 μm in step (1) 95.5 Sn 4.5 Except for the alloy material as the substrate, everything else was the same as in Example 1. The resulting product was a hierarchical porous Cu. 95.5 Sn 4.5 The alloy material has primary pores with a size of 5-20 μm and secondary pores with a size of 0.1-2 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0047] Example 3 A method for preparing hierarchical porous CuAu alloy material: (1) Select Cu with a thickness of 80μm95 Au5 alloy material substrate, cut to the preset size, ultrasonically cleaned with anhydrous ethanol and dried for later use; (2) Weigh the Cu after pretreatment in step (1) 95 3.00 g of Au5 alloy base and 6.00 g of high-purity zinc granules were weighed out at a mass ratio of 1:2 for later use; (3) Cu 95 Au5 alloy substrate and zinc granules are placed together in a tube furnace in a non-contact manner. After argon gas scrubbing, the system gas pressure is controlled to below 20 Pa. The substrate is heated to 650 ℃ at a rate of 10 ℃ / min and held for 120 min. After holding, the substrate is cooled to room temperature with the furnace to obtain copper-zinc precursor alloy. (4) The copper-zinc precursor alloy was placed in a tube furnace and washed with argon-hydrogen mixed gas. The vacuum valve was kept open. The system pressure was controlled to be 300 Pa by adjusting the argon-hydrogen mixed gas inlet valve. Then it was heated to 700 °C and held for 80 min. After holding, it was cooled to room temperature with the furnace to obtain the first dealloying sample with a primary porous structure. (5) Weigh the first dealloyed sample and weigh high-purity zinc granules again at a mass ratio of 1:2 for later use; (6) Place the first dealloyed sample and zinc granules at both ends of the glass tube and separate them with a glass stopper. The glass stopper can move in the glass tube. After argon gas washing, the glass tube is welded and sealed under a vacuum of less than 20 Pa. (7) Place the sealed glass tube in a muffle furnace, heat it to 620 ℃ and hold it for 15 min for a short time. After holding, cool it with the furnace to 400 ℃ and take it out. Cool it to room temperature in the air to obtain the second alloying sample. (8) Take out the second alloying sample and place it in a tube furnace. After purging with an argon-hydrogen mixture, keep the vacuum valve open. Control the system pressure to 300 Pa by adjusting the argon-hydrogen mixture inlet valve. Heat to 620 °C and hold for 10 min. After holding, cool to room temperature with the furnace to obtain the fractionated porous Cu. 95 Au5 alloy material. The size of the primary pores in the material is 5-25 μm, and the size of the secondary pores is 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0048] Example 4 A method for preparing hierarchical porous CuAg alloy material: (1) Select Cu with a thickness of 300 μm 98 Ag2 alloy material substrate, cut to the preset size, ultrasonically cleaned with anhydrous ethanol and dried for later use; (2) Weigh the Cu after pretreatment in step (1)98 2.00 g of Ag2 alloy base and 4.00 g of high-purity zinc granules weighed at a mass ratio of 1:2 for later use; (3) Cu 98 Ag2 alloy substrate and zinc granules are placed together in a tube furnace in a non-contact manner. After argon gas scrubbing, the system gas pressure is controlled to below 20 Pa. The temperature is heated to 700 ℃ at 10 ℃ / min and held for 150 min. After holding, the temperature is cooled to room temperature with the furnace to obtain copper-zinc precursor alloy. (4) The copper-zinc precursor alloy was placed in a tube furnace and washed with argon-hydrogen mixed gas. The vacuum valve was kept open. The system pressure was controlled to be 100 Pa by adjusting the argon-hydrogen mixed gas inlet valve. Then it was heated to 750 °C and held for 120 min. After holding, it was cooled to room temperature with the furnace to obtain the first dealloying sample with a primary porous structure. (5) Weigh the first dealloyed sample and weigh high-purity zinc granules again at a mass ratio of 1:2 for later use; (6) Place the first dealloyed sample and zinc granules at both ends of the glass tube and separate them with a glass stopper. The glass stopper can move in the glass tube. After argon gas washing, the glass tube is welded and sealed under a vacuum of less than 20 Pa. (7) Place the sealed glass tube in a muffle furnace, heat it to 650 ℃ and hold it for 20 min for a short time. After holding, cool it with the furnace to 400 ℃ and take it out. Cool it to room temperature in the air to obtain the second alloying sample. (8) Take out the second alloying sample and place it in a tube furnace. After purging with an argon-hydrogen mixture, keep the vacuum valve open. Control the system pressure to 100 Pa by adjusting the argon-hydrogen mixture inlet valve. Heat to 650 °C and hold for 20 min. After holding, cool to room temperature with the furnace to obtain the fractionated porous Cu. 98 Ag2 alloy material. The size of the primary pores in the material is 5-30 μm, and the size of the secondary pores is 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous and crack-free.

[0049] Example 5 A method for preparing hierarchical porous CuSi alloy material: (1) Select Cu with a thickness of 150 μm 99 Si1 alloy material substrate, cut to the preset size, ultrasonically cleaned with anhydrous ethanol and dried for later use; (2) Weigh the Cu after pretreatment in step (1) 99 5.00 g of Si1 alloy substrate, and 10.00 g of high-purity zinc granules weighed at a mass ratio of 1:2 for later use; (3) Cu99 Si1 alloy substrate and zinc granules are placed together in a tube furnace in a non-contact manner. After argon gas scrubbing, the system gas pressure is controlled to below 20 Pa. The substrate is heated to 650 ℃ at 10 ℃ / min and held for 150 min. After holding, the substrate is cooled to room temperature with the furnace to obtain copper-zinc precursor alloy. (4) The copper-zinc precursor alloy was placed in a tube furnace and washed with argon-hydrogen mixed gas. The vacuum valve was kept open. The system pressure was controlled to be 150 Pa by adjusting the argon-hydrogen mixed gas inlet valve. Then it was heated to 700 °C and held for 120 min. After holding, it was cooled to room temperature with the furnace to obtain the first dealloying sample with a primary porous structure. (5) Weigh the first dealloyed sample and weigh high-purity zinc granules again at a mass ratio of 1:2 for later use; (6) Place the first dealloyed sample and zinc granules at both ends of the glass tube and separate them with a glass stopper. The glass stopper can move in the glass tube. After argon gas washing, the glass tube is welded and sealed under a vacuum of less than 20 Pa. (7) Place the sealed glass tube in a muffle furnace, heat it to 650 ℃ and hold it for 20 min for a short time. After holding, cool it with the furnace to 300 ℃ and take it out. Cool it to room temperature in the air to obtain the second alloying sample. (8) Take out the second alloying sample and place it in a tube furnace. After purging with an argon-hydrogen mixture, keep the vacuum valve open. Control the system pressure to 150 Pa by adjusting the argon-hydrogen mixture inlet valve. Heat to 650 °C and hold for 20 min. After holding, cool to room temperature with the furnace to obtain the fractionated porous Cu. 99 Si1 alloy material. The size of the primary pores in the material is 5-20 μm, and the size of the secondary pores is 0.1-1 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous and crack-free.

[0050] Example 6 A hierarchical porous Cu 99 The preparation method of Ni1 material, compared with Example 3, is different except that in step (1) a Cu material with a thickness of 70 μm is selected. 99 The substrate is Ni1 alloy, and the alloying temperature in step (7) is 650 ℃ with a holding time of 10 min, while the dealloying temperature in step (8) is 650 ℃ with a holding time of 10 min. All other steps are the same as in Example 3. The resulting hierarchical porous Cu... 99 The primary pore size of Ni1 alloy material is 5-30 μm, and the secondary pore size is 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0051] Example 7 A hierarchical porous Cu 97 The preparation method of Ti3 material, compared with Example 5, is different except that in step (1) a Cu material with a thickness of 250 μm is selected. 97 The Ti3 alloy material was used as the substrate. The alloying temperature in step (3) was 750 ℃, and the holding time was 120 min. The dealloying pressure in step (8) was 100 Pa, the dealloying temperature was 750 ℃, and the holding time was 10 min. All other steps were the same as in Example 5. The resulting hierarchical porous Cu... 97 The Ti3 alloy material has primary pores with a size of 5-15 μm and secondary pores with a size of 0.1-2 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0052] Example 8 A hierarchical porous Cu 99 Sn 0.5 Sb 0.5 The preparation method of the material, compared with Example 5, is different except that in step (1) a Cu material with a thickness of 200 μm is selected. 99 Sn 0.5 Sb 0.5 The alloy material is used as the substrate; the alloying temperature in step (3) is 700 ℃ and the holding time is 100 min; the dealloying gas pressure in step (4) is 200 Pa, the dealloying temperature is 750 ℃, and the holding time is 90 min. All other aspects are the same as in Example 5. The resulting hierarchical porous Cu... 99 Sn 0.5 Sb 0.5 The primary pore size of the alloy material is 5-30 μm, and the secondary pore size is 0.1-3 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0053] Example 9 A hierarchical porous Cu 98.5 Sn 0.5 Sb 0.5 Si 0.5 The material preparation method, compared with Example 4, is different except that in step (1) a Cu material with a thickness of 250 μm is selected. 98.5 Sn 0.5 Sb 0.5 Si 0.5 The alloy material is used as the substrate; the alloying temperature in step (7) is 600℃ and the holding time is 15 min; the dealloying gas pressure in step (8) is 200 Pa, the dealloying temperature is 600℃, and the holding time is 15 min; otherwise, it is the same as in Example 4. The resulting hierarchical porous Cu...98.5 Sn 0.5 Sb 0.5 Si 0.5 The primary pore size of the alloy material is 5-30 μm, and the secondary pore size is 0.1-2 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0054] Example 10 A hierarchical porous Cu 98 Pt 0.5 Pb 0.5 Ag 0.5 Au 0.5 The preparation method of the material, compared with Example 5, is different except that in step (1) a Cu material with a thickness of 200 μm is selected. 98 Pt 0.5 Pb 0.5 Ag 0.5 Au 0.5 The alloy material is used as the substrate. The alloying temperature in step (7) is 600 ℃ and the holding time is 15 min. The dealloying temperature in step (8) is 600 ℃ and the holding time is 15 min. All other steps are the same as in Example 5. The resulting hierarchical porous Cu... 98 Pt 0.5 Pb 0.5 Ag 0.5 Au 0.5 The primary pore size of the alloy material is 5-20 μm, and the secondary pore size is 0.1-2 μm. The secondary pores are distributed on the pore walls of the primary pores. The primary pores form a three-dimensional continuous network structure, and the material is macroscopically continuous without cracks.

[0055] Comparative Example 1 Compared with Example 2, steps (5)-(8) are omitted, and the resulting product is Cu with a primary porous structure. 95.5 Sn 4.5 The alloy material has a pore size of 5-20μm, and the primary pores are a three-dimensional continuous network structure. The material is also macroscopically continuous and crack-free.

[0056] Comparative Example 2 A method for preparing a hierarchical porous CuSn alloy material includes the following steps: (1) Same as Example 2.

[0057] (2) Same as Example 2.

[0058] (3) Same as Example 2.

[0059] (4) Immerse the copper-zinc precursor alloy in a 2 mol / L hydrochloric acid solution and perform liquid-phase corrosion at room temperature until no more bubbles are generated on the alloy surface. Take out the sample after the reaction, wash it several times alternately with deionized water and anhydrous ethanol, and then dry it to obtain the first dealloyed sample.

[0060] (5) Same as Example 2.

[0061] (6) Same as Example 2.

[0062] (7) Same as Example 2.

[0063] (8) The second alloyed sample was removed and immersed again in a 2 mol / L hydrochloric acid solution to attempt liquid-phase dealloying, but almost no bubbles were generated on the sample surface, making effective corrosion impossible. The immersed sample was removed, washed with deionized water and anhydrous ethanol, and dried.

[0064] The resulting product failed to effectively remove the target element due to the second liquid-phase corrosion, thus failing to form the required hierarchical porous structure, making the scheme impossible to implement in practice.

[0065] Comparative Example 3 A method for preparing a hierarchical porous CuSn alloy material includes the following steps: (1) Same as Example 2.

[0066] (2) Same as Example 2.

[0067] (3) Same as Example 2.

[0068] (4) Immerse the copper-zinc precursor alloy in a 2 mol / L hydrochloric acid solution and perform liquid-phase corrosion at room temperature until no more bubbles are generated on the alloy surface. Take out the sample after the reaction, wash it several times alternately with deionized water and anhydrous ethanol, and then dry it to obtain the first dealloyed sample.

[0069] (5) Same as Example 2.

[0070] (6) Same as Example 2.

[0071] (7) Same as Example 2.

[0072] (8) Same as Example 2.

[0073] Because the ligaments formed during the first liquid-phase dealloying are small in size, the newly formed pores are prone to severe healing and closure due to thermal diffusion during the second high-temperature gas-phase dealloying process. Ultimately, the product loses its multi-level pore characteristics and cannot form a continuous hierarchical porous network.

[0074] Application Example 1 The products prepared in Example 2 and Comparative Example 1 were cut into 1×1 cm pieces. 2 The electrode sheet was used as the working electrode and placed in an H-type electrolytic cell for testing the electrocatalytic reduction performance of CO2. The test procedure was as follows: 15 mL of electrolyte (0.5 M KHCO3 aqueous solution) was injected into both the cathode and anode chambers of the electrolytic cell, and the two chambers were separated by a Nafion 117 membrane. The working electrode was fixed on a graphite clamp and placed in the cathode chamber, with a saturated calomel electrode used as the reference electrode. The cathode chamber cover was equipped with a CO2 inlet and a gas product outlet. In addition, a magnetic rotor was installed in the cathode chamber, which continuously stirred the gas at an appropriate speed during the test to accelerate mass transfer. A platinum electrode was used as the counter electrode in the anode chamber. Then, the it curves at different potentials were obtained by the constant potential current-time method, and the gas products at the cathode chamber outlet were sampled and analyzed at regular intervals using a gas chromatograph to achieve quantitative analysis of the gas products.

[0075] like Figure 8 As shown, at a constant potential of -1.0 V vs. RHE, this catalyst exhibits excellent electrocatalytic reduction performance and stability for CO2. After a 10-hour constant potential test, its voltage and current stability remained stable and unaffected by fluctuations, and it effectively suppressed the hydrogen evolution side reaction, maintaining a hydrogen evolution Faraday efficiency of approximately 12% within 10 hours. Figure 9 As shown, the catalyst of Comparative Example 1 exhibits higher Faraday efficiency for hydrogen evolution at various test potentials than that of Example 2, indicating that the performance of Comparative Example 1 in suppressing hydrogen evolution side reactions is significantly inferior to that of Example 2. These results fully demonstrate that the hierarchical porous alloy material of this invention possesses good stability and great application potential in the field of electrocatalytic CO2 reduction.

Claims

1. A method for preparing a hierarchical porous copper-based material, characterized in that: Includes the following steps: (1) Using pure copper or copper-based alloy with a thickness of 30-300 μm as the substrate, the substrate and zinc particles are placed in a reactor in a non-contact manner, the air in the reactor is replaced with inert gas, and then the first gas phase alloying treatment is carried out by heating under low pressure. After the treatment is completed, the sample is cooled to room temperature in the furnace to obtain the first alloyed sample. (2) The first alloyed sample was subjected to the first gas phase dealloying treatment in a mixed atmosphere of flowing inert gas and hydrogen under low pressure. After the treatment, it was cooled to room temperature in the furnace to obtain the first dealloyed sample. (3) Place the first dealloyed sample and zinc granules into both ends of the glass tube, and place a barrier with a diameter smaller than that of the glass tube between the first dealloyed sample and zinc granules. Replace the air in the glass tube with inert gas and evacuate it. Then seal the glass tube. (4) The sealed glass tube is heated to perform a second vapor phase alloying treatment. After the treatment, it is cooled to 300-450℃ in the furnace and then taken out and cooled to room temperature in air to obtain the second alloyed sample. (5) The second alloyed sample was taken out of the glass tube and subjected to a second vapor-phase dealloying treatment under a mixed atmosphere of flowing inert gas and hydrogen at low pressure. After the treatment, it was cooled to room temperature with the furnace to obtain a graded porous copper-based material.

2. The preparation method according to claim 1, characterized in that: The copper-based alloy is an alloy formed from Cu and other metals, wherein the other metals are at least one selected from Sn, Si, Sb, Ni, Pt, Pd, Ag, Au, and Ti; preferably, the atomic fraction of copper in the copper-based alloy is greater than 50%.

3. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of the substrate to the zinc particles is 1:2-3; in step (3), the mass ratio of the first dealloyed sample to the zinc particles is 1:2-3.

4. The preparation method according to claim 1, characterized in that: In step (1), during the first vapor phase alloying treatment, the vacuum degree in the reactor is less than 20 Pa, the temperature is 550-700℃, and the holding time is 60-150 min.

5. The preparation method according to claim 1, characterized in that: In step (2), during the first vapor phase dealloying treatment, the vacuum degree in the system is 100-300 Pa, the temperature is 600-750 ℃, and the holding time is 70-120 min.

6. The preparation method according to claim 1, characterized in that: In steps (2) and (5), the volume fraction of hydrogen in the mixed atmosphere of inert gas and hydrogen is 5-10%; preferably, in step (3), the vacuum degree inside the glass tube is less than 20 Pa.

7. The preparation method according to claim 1, characterized in that: In step (4), the temperature during the second vapor phase alloying treatment is 550-650 ℃ and the holding time is 5-20 min.

8. The preparation method according to claim 1, characterized in that: In step (5), during the second vapor-phase dealloying treatment, the vacuum degree in the system is 100-300 Pa, the temperature is 550-650 ℃, and the holding time is 5-20 min.

9. A hierarchical porous copper-based material prepared according to any one of claims 1-8; preferably, the hierarchical porous copper-based material has primary pores with a size of 5-30 μm and secondary pores with a size of 0.1-3 μm, the secondary pores being distributed on the pore walls of the primary pores, the primary pores being a three-dimensional continuous network structure, and the hierarchical porous copper-based material being macroscopically continuous and crack-free.

10. The application of the hierarchical porous copper-based material of claim 9 in electrocatalytic reduction of CO2 and / or electrolysis of water and / or lithium-ion batteries.

Citation Information

Patent Citations

  • Preparation method of nano-porous metal or alloy

    CN111254309A

  • Cu / Zn synergistic photoresponse composite material as well as preparation method and application thereof