Unleaded brass alloys
By adding appropriate amounts of Mg, As, and P to brass alloys and controlling their proportions, the problems of machinability, dezincification resistance, and hot brittleness of lead-free brass alloys were solved. This achieved compliance with REACH regulations on lead content and hot forming capabilities, reduced Cu content, and improved processing performance and economy.
Patent Information
- Application Number
- CN202610710240.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-23
- Filing Date
- 2026-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lead-free brass alloys are inadequate in terms of machinability, resistance to dezincification, and hot brittleness, making it difficult to meet the lead content restrictions of the EU REACH regulation and unsuitable for use in die-cast parts.
By adding 0.09 to 0.45% Mg, 0.03 to 0.2% As, 0.03 to 0.5% P, and an appropriate amount of Pb, and controlling the weight ratio of the sum of As and P to the weight of Mg to be 1.2 or greater, precipitates that facilitate cutting are formed to improve machinability and resistance to dezincification, while controlling the Cu content at 60 to 65% to reduce hot brittleness.
It achieves good machinability, resistance to dezincification and low hot brittleness, meets the lead content requirements of the EU REACH regulation, is suitable for thermoforming, and is cost-effective.
Smart Images

Figure CN123152918A_ABST
Abstract
Description
[0001] This invention relates to a lead-free brass alloy and its uses.
[0002] In the past, up to 4% by weight of lead (Pb) was added to improve the machinability of brass alloys. However, due to regulatory requirements, the addition of Pb will be strictly limited or no longer permitted in various applications. Particularly in the case of drinking water, Europe has regulations on lead migration values that must not be exceeded.
[0003] It has been previously discovered that Bi can be added as a substitute for Pb. However, it has been shown that the addition of Bi leads to hot brittleness in brass alloys. Such brass alloys can only be hot-formed to a limited extent. Therefore, these brass alloys are not used for die-cast parts.
[0004] EP 3 320 122 B1 discloses a brass alloy without the addition of either Pb or Bi. To improve machinability, it is suggested to add 0.005 to 1.0 wt% In to the brass alloy. While the suggested indium addition slightly improves machinability, relatively long spiral chips are still formed during cutting, leading to chip clogging and tool breakage, severely hindering large-scale industrial production. Furthermore, indium is a very expensive alloying element.
[0005] A brass alloy is known from EP 4 124 667 A1, in which the lead content can be adjusted to less than 0.1 wt% by adding 0.1 to 1.5 wt% Mg without forming undesirable long spiral chips during cutting. Furthermore, this brass alloy is characterized by low hot brittleness. However, according to ISO 6509, this alloy is not considered resistant to dezincification.
[0006] EP 2 133 437 A1 describes a lead-free brass alloy containing 0.6 to 2.5 wt% Mg and 0.15 to 0.4 wt% P. However, it also lacks the dezincification resistance required according to ISO 6509.
[0007] A lead-free brass alloy with both good machinability and resistance to dezincification is known from EP 1 812 612 B1. This is a high copper content (70 to 80 wt%) copper-zinc-silicon alloy containing 1 to 5 wt% silicon, 0.0001 to 0.5 wt% B, 0 to 0.2 wt% P and / or As, and the balance Zn.
[0008] Based on the aforementioned prior art, the objective of this invention is to provide a lead-free brass alloy with good machinability and resistance to dezincification, but with a low Cu content. Another objective of this invention is that the brass alloy should have low hot brittleness, thereby allowing it to be processed by hot forming.
[0009] This task is solved by the features of claim 1. Advantageous improvements to the invention are given in the dependent claims. Particularly advantageous uses of the lead-free brass alloy are given in claim 14.
[0010] According to the present invention, a lead-free brass alloy is proposed, comprising...
[0011] 60 to 65% Cu,
[0012] 0.09% to 0.45% Mg
[0013] 0.03% to 0.2% As,
[0014] P from 0.03% to 0.5%
[0015] At most 0.1% Pb,
[0016] Balance of Zn and
[0017] Unavoidable impurities
[0018] The ratio of the sum of the weight parts of As and P to the weight parts of magnesium is at least 1.2.
[0019] In this specification, [%] is understood as weight percentage.
[0020] Alloying with Mg allows lead content to be adjusted to 0.1% or lower without forming undesirable long spiral chips during cutting. P and As are partially bound by Mg, forming precipitates that aid in cutting. The free proportions of P and As inhibit dezincification. However, excessively high As content leads to susceptibility to intergranular corrosion, while excessively high P content results in excessively fluid melt, posing technical challenges in continuous casting processes.
[0021] It has been shown that dezincification resistance can only be obtained by setting a specific ratio between the sum of the alloyed inhibitors (P and As) and the alloyed Mg. According to the invention, this ratio is 1.2 or greater, particularly between 1.2 and 9.0.
[0022] Furthermore, the proposed brass alloy is characterized by improved chip breaking and low hot brittleness (i.e., it can be well processed by hot forming) without requiring a high Cu content.
[0023] According to this invention, "lead-free brass alloy" is understood to be an alloy containing 0.1% or less Pb. This also corresponds to the regulatory threshold for disclosure requirements under the EU REACH Regulation.
[0024] Optionally, the alloy may contain
[0025] - 0 to 0.1%, especially less than 0.1% aluminum, and / or
[0026] - 0 to 0.1%, especially less than 0.1% tin, and / or
[0027] - 0 to 0.1%, especially less than 0.1% silicon, and / or
[0028] - 0 to 0.1%, especially less than 0.1% iron.
[0029] Al and Sn improve coating adhesion. The addition of Si improves machinability. Fe refines the grain size.
[0030] According to another favorable improvement, there is 62.5% to 64.5%, preferably 63% to 64%, and particularly 63.2% to 63.9% Cu.
[0031] The proposed alloy is more cost-effective than, for example, the alloys described in EP 1 812 612 B1 due to its relatively low Cu content.
[0032] According to another improved option, it contains 0.18% to 0.38%, preferably 0.18% to 0.26%, and particularly 0.18% to 0.21% Mg. The suggested Mg content helps improve machinability without causing technical problems during continuous casting.
[0033] The Pb content is suitably below 0.1%, preferably in the range of 0.05 to 0.09%, and particularly 0.08%.
[0034] According to a particularly advantageous improvement, the alloy contains
[0035] Cu content of 62.5% to 64.5%
[0036] 0.09% to 0.14% Mg
[0037] 0.1% to 0.12% As,
[0038] P values ranged from 0.08% to 0.1%.
[0039] Pb content less than 0.1%,
[0040] Balance of Zn and
[0041] Unavoidable impurities.
[0042] According to another particularly advantageous improvement, the alloy contains
[0043] Cu content of 62.5% to 64.5%
[0044] 0.18 to 0.26% Mg,
[0045] 0.1% to 0.12% As,
[0046] P values ranged from 0.24% to 0.3%.
[0047] Pb content less than 0.1%,
[0048] Balance of Zn and
[0049] Unavoidable impurities.
[0050] According to another particularly advantageous improvement, the alloy contains
[0051] Cu content of 62.5% to 64.5%
[0052] 0.26% to 0.38% Mg,
[0053] 0.1% to 0.12% As,
[0054] P values ranged from 0.39% to 0.49%.
[0055] Pb content less than 0.1%,
[0056] Balance of Zn and
[0057] Unavoidable impurities.
[0058] According to another particularly advantageous improvement, the alloy contains
[0059] 64% Cu,
[0060] 0.26% Mg,
[0061] 0.11% As,
[0062] 0.22% P,
[0063] 0.08% Pb,
[0064] Balance of Zn and
[0065] Unavoidable impurities.
[0066] According to another particularly advantageous improvement, the alloy contains
[0067] 64% Cu,
[0068] 0.47% Mg,
[0069] 0.12% As,
[0070] 0.48% P,
[0071] 0.08% Pb,
[0072] Balance of Zn and
[0073] Unavoidable impurities.
[0074] For all the mentioned embodiments, according to the invention, the ratio of the sum of the weight parts of As and P to the weight parts of Mg is greater than or equal to 1.2. Preferably, the ratio of the sum of the weight parts of As and P to the weight parts of Mg can exceed 1.2, particularly between 1.2 and 9.0.
[0075] The lead-free brass alloy according to the present invention is resistant to dezincification, exhibits good machinability, and can achieve good machinability in continuous casting processes, while requiring a smaller proportion of valuable copper material.
[0076] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings. The drawings show:
[0077] Figure 1a Cross-sectional view of the first non-inventive alloy.
[0078] Figure 1b Chip diagram of the first non-inventive alloy after longitudinal turning.
[0079] Figure 2a Cross-sectional view of the second non-inventive alloy.
[0080] Figure 2b The second type of chip diagram after longitudinal turning of the alloy not of this invention.
[0081] Figure 3a A cross-sectional view of the third alloy of the present invention.
[0082] Figure 3b The third type of chip diagram after longitudinal turning of the alloy of the present invention.
[0083] Figure 4a A cross-sectional view of the fourth alloy of the present invention.
[0084] Figure 4b The fourth type of chip diagram of the alloy of the present invention after longitudinal turning.
[0085] Figure 1a , 2a Cross-sectional views 3a and 4a show longitudinal grinding discs of different alloy bar samples after undergoing the standard ISO 6509 dezincification test, with the top of each sample being the surface of the bolt. In both cases, Figure 1a and 2a The scales shown are all 200µm. Figure 3a and 4a The scale bars shown are all 20µm. Figure 1a and2a The pinkish areas on the surface can be identified as corrosive erosion in the form of zinc stripping. Figure 3a and 4a At a scale approximately five times smaller, only very small (pink) dezincification areas are directly visible on the material surface. Figure 1a and 2a The dezincification depth in the sample is much greater than 200µm. Figure 3a and 4a The dezincification depth ratio in Figure 1a and 2a The zinc removal depth of the alloy is more than 10 times lower (see Table 1 below).
[0086] Figure 1b , 2b The chip patterns in 3b and 4b were made by longitudinal turning of the alloys, respectively. Figure 1b , 2b The scale bars inserted in 3b and 4b are all 20 mm.
[0087] The respective alloy compositions can be found in the rows marked in the first column of Table 1.
[0088]
[0089] Table 1: Alloy composition of the experimental series (balance: Zn)
[0090] Table 1 lists the alloy compositions of the experimental series comprising 12 different brass alloys. The first column indicates whether and which figures are related to the corresponding alloy. The penultimate column lists the weight ratio of the sum of P and As to the weight of Mg. The last column gives the maximum dezincification depth as determined according to ISO 6509.
[0091] Brass alloys are generally considered to have resistance to dezincification if the dezincification depth is less than 100 µm in tests conducted according to ISO 6509. It can be clearly seen from the values in Table 1 that when the (P+As) / Mg value is below 1.2 (see also...) Figure 1a , 2a The dezincification depth is significantly higher than 100 µm. Starting from a (P+As) / Mg ratio of 1.2, the dezincification depth abruptly drops significantly below 100 µm. This is from... Figure 3a and 4a This can be clearly seen in the text.
[0092] Experimental series showed that when the (P+As) / Mg value started from 1.2, especially between 1.2 and 9.0, the dezincification depth was less than 100 µm, while when the value was less than 1.2, the dezincification resistance according to ISO 6509 was not achieved.
[0093] Figure 3b and4b Although the chip diagram is more Figure 1b and 2b It exhibits a high proportion of longer chips, but the chips are short enough that the dezincification-resistant alloy according to the invention has good machinability.
[0094] Alloys with the compositions shown in Table 2 have also been shown to be equally resistant to dezincification and at the same time have good machinability.
[0095]
[0096] Table 2: Alloy composition of preferred embodiments of the present invention
[0097] All the alloys mentioned may also have up to 0.1% Al and / or up to 0.1% Sn and / or up to 0.1% Si and / or up to 0.1% Fe added. Al and Sn improve the adhesion of the coating, Si improves machinability, and Fe improves the fineness of the grain structure.
[0098] Due to its resistance to dezincification and its good machinability, the lead-free brass alloy according to the present invention is particularly suitable as a material for components that come into contact with drinking water. It meets common preconditions regarding resistance to dezincification and maximum lead content, has good machinability, and requires a relatively low copper content.
Claims
1. Lead-free brass alloy, each containing, by weight % 60 to 65% Cu, 0.09% to 0.45% Mg 0.03% to 0.2% As, P from 0.03% to 0.5% 0 to 0.1% Pb, Optionally, an additional 0 to 0.1% Al, Optionally, an additional 0 to 0.1% Sn, Optionally, an additional 0 to 0.1% Si, Optionally, an additional 0 to 0.1% Fe, Balance of Zn and Unavoidable impurities The ratio of the sum of the weight parts of As and P to the weight parts of magnesium is at least 1.
2.
2. The lead-free brass alloy according to claim 1, It contains 62.5% to 64.5%, 63% to 64%, and especially 63.2% to 63.9% Cu.
3. The lead-free brass alloy according to any one of the preceding claims, It contains 0.18 to 0.38%, preferably 0.18 to 0.26%, and especially 0.18 to 0.21% Mg.
4. The lead-free brass alloy according to any one of the preceding claims, It contains 0.10 to 0.12%, preferably 0.11% As.
5. The lead-free brass alloy according to any one of the preceding claims, It contains 0.22% to 0.48% P.
6. The lead-free brass alloy according to any one of the preceding claims, It contains less than 0.1%, preferably 0.05 to 0.09%, and especially 0.08% Pb.
7. The lead-free brass alloy according to any one of the preceding claims, It contains less than 0.1% Al and / or less than 0.1% Sn and / or less than 0.1% Si and / or less than 0.1% Fe.
8. The lead-free brass alloy according to claim 1, comprising... Cu content of 62.5% to 64.5% 0.09% to 0.14% Mg 0.1% to 0.12% As, P values ranged from 0.08% to 0.1%. Pb content less than 0.1%, Balance of Zn and Unavoidable impurities.
9. The lead-free brass alloy according to claim 1, comprising... Cu content of 62.5% to 64.5% 0.18 to 0.26% Mg, 0.1% to 0.12% As, P values ranged from 0.24% to 0.3%. Pb content less than 0.1%, Balance of Zn and Unavoidable impurities.
10. The lead-free brass alloy according to claim 1, comprising... Cu content of 62.5% to 64.5% 0.26% to 0.38% Mg, 0.1% to 0.12% As, P values ranged from 0.39% to 0.49%. Pb content less than 0.1%, Balance of Zn and Unavoidable impurities.
11. The lead-free brass alloy according to claim 1, comprising... 64% Cu, 0.26% Mg, 0.11% As, 0.22% P, 0.08% Pb, Balance of Zn and Unavoidable impurities.
12. The lead-free brass alloy according to claim 1, comprising... 64% Cu, 0.47% Mg, 0.12% As, 0.48% P, 0.08% Pb, Balance of Zn and Unavoidable impurities.
13. The lead-free brass alloy according to any one of the preceding claims, in, The ratio of the sum of the weight parts of As and P to the weight parts of magnesium exceeds 1.2, especially between 1.2 and 9.
0.
14. Use of the lead-free brass alloy according to any one of the preceding claims as a material for components in contact with drinking water.
Citation Information
Patent Citations
Copper / zinc / silicon alloy, use and production thereof
EP1812612B1
Tin-free lead-free free-cutting magnesium brass alloy and its manufacturing method
EP2133437A1
Lead and antimony-free brass alloy
EP4124667A1