Microalloyed AlSi 10 Mg alloy powder and its preparation method, 3D devices and their preparation methods

By doping AlSi10Mg alloy with Er and Zr elements to form a second phase with an L1₂ core-shell structure, the grains are refined and the microstructure is strengthened. This solves the problems of hot cracking and anisotropy of properties in aluminum microalloy powder, and realizes high-strength, high-elongation aluminum alloy powder suitable for 3D printing.

CN123152931APending Publication Date: 2026-11-24CHINALCO RES INST OF SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611476168.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing aluminum microalloyed AlSi10Mg alloy powder is prone to defects such as hot cracks and pores under rapid non-equilibrium cooling conditions, leading to deformation, cracking and anisotropy of properties. The types of materials are limited, and they rely on imports and are costly, making it difficult to meet the stringent requirements of engineering applications.

Method used

By doping the AlSi10Mg alloy matrix with Er and Zr elements, the grains are refined and the microstructure is improved by forming the L1₂ core-shell structure of the Al₃(Er,Zr) second phase. Combined with the phase transformation strengthening of Si and Mg, a high density of heterogeneous nucleation sites is formed, thereby improving the mechanical properties.

Benefits of technology

It achieves tensile strength of 500MPa and yield strength of 300MPa without heat treatment, with an elongation of 8.0-9.5%, exhibiting excellent strength-toughness balance and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152931A_ABST
    Figure CN123152931A_ABST
Patent Text Reader

Abstract

This application provides a microalloyed AlSi 10 Mg alloy powder and its preparation method, 3D devices and their preparation methods, and the micro-alloyed AlSi provided in this application 10 The Mg alloy powder comprises an alloy matrix and Er and Zr elements doped into the alloy matrix, wherein the mass content of Er element is 0.7-1.3% and the mass content of Zr element is 0.7-1.3%; the alloy matrix is ​​AlSi. 10 Mg alloys. This application utilizes specific microalloyed AlSi alloys. 10 The composition of Mg alloy powder utilizes the synergistic effect of Er and Zr elements to refine grains and improve the alloy microstructure, thereby significantly improving the microalloying of AlSi. 10 Mechanical properties of Mg alloy powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the fields of metallic materials and additive manufacturing technology, and more specifically, to a microalloyed AlSi... 10 Mg alloy powder and its preparation method, 3D devices and their preparation methods. Background Technology

[0002] Metal additive manufacturing technology (commonly known as 3D printing technology) has overcome traditional application limitations and expanded product design space due to its advantages such as optimized product structure, integrated molding of complex components, and shortened production processes. It has become a crucial national asset for meeting major national needs and supporting national economic development. Among various additive manufacturing technologies, laser powder bed fusion technology has become the mainstream technology in the field of metal additive manufacturing due to its high level of technological and industrial maturity. On the materials side, with the increasing standards for ultra-lightweight design in strategic emerging industries and the urgent need to reduce energy consumption and carbon footprint, aluminum microalloyed AlSi10Mg alloy powder for laser additive manufacturing has become a key engineering structural material.

[0003] Existing aluminum microalloyed AlSi10Mg alloy powders for additive manufacturing face the following bottlenecks: First, insufficient material specialization. Traditional aluminum microalloyed AlSi10Mg alloy powders are prone to hot cracking and porosity defects under rapid, non-equilibrium cooling conditions, leading to deformation, cracking, and anisotropy in properties, making them unsuitable for direct application. Second, limited material types. Fewer than 10 alloy types meet the application requirements, only 1 / 20th of the traditional grades, and only 3 are included in the national standard (GB / T 44239-2024), specifically AlSi... 10 Mg, AlSi7Mg, AlMgScZr; thirdly, some high-quality powders rely on imports and face technological blockades and patent barriers, lacking exclusive material standards and having high costs.

[0004] Among various aluminum alloy systems, the Al-Si alloy system has become one of the most widely studied aluminum alloy systems for laser additive manufacturing due to its advantages such as high fluidity, narrow solidification range, low hot cracking sensitivity, and excellent adaptability to additive manufacturing processes. AlSi is the primary alloy used. 10 Mg, AlSi7Mg and AlSi 12Al-Si alloys, primarily near-eutectic alloys, exhibit superior mechanical strength compared to traditionally manufactured Al-Si alloys due to the refined Si phase formation during the printing process. However, due to the inherent material properties of cast aluminum alloys, Al-Si alloys suffer from low strength, with a maximum tensile strength of 350 MPa and a maximum yield strength of 200 MPa, making them unsuitable for increasingly demanding engineering applications. Therefore, the mechanical properties of Al-Si alloys are typically controlled through stoichiometric alterations, the addition of reinforcing particles, or microalloying. While altering the Si and Mg content can enhance mechanical properties by inducing a refined eutectic network structure and utilizing solid solution strengthening, the controllability of these contents is limited; otherwise, high crack density may result. Adding ceramic or carbon-based reinforcing particles allows for the in-situ generation of heterogeneous nucleation sites, increasing the nucleation rate and pinning grain boundaries to limit α-Al growth. Precipitation strengthening based on high-density nano-precipitates, grain refinement, and grain boundary strengthening further inhibits cracking and reduces anisotropy, thereby improving mechanical strength. However, reinforcing particles are typically introduced through powder mixing. Besides considering dispersibility and uniformity, the secondary processing of composite powders can damage powder sphericity and particle size, affecting molding quality. Furthermore, density differences, wettability matching issues, and reactivity between reinforcing particles and the aluminum matrix can hinder atomization, lead to defect formation, and result in particle loss. Microalloying with the rare earth element Sc can avoid these problems and significantly improve mechanical strength; however, the high cost of Sc increases manufacturing costs, making large-scale industrial application difficult. In addition, the limited solid solubility of Sc restricts the maximum reinforcing effect, failing to meet the requirements of high-stress service scenarios.

[0005] Therefore, with the two core objectives of performance improvement and cost control, a 500MPa-grade AlSi steel with high strength, high elongation, and high molding quality was developed. 10 The microalloying of Mg into AlSi10Mg alloy powder is of great significance for expanding the engineering application scenarios of Al-Si additive alloys and breaking through the performance bottlenecks of existing materials. Summary of the Invention

[0006] The main objective of this application is to provide a microalloyed AlSi 10 Mg alloy powder and its preparation method, 3D devices and their preparation methods, to solve the problems of existing AlSi... 10 The problem of poor mechanical properties of Mg alloys.

[0007] To achieve the above objectives, according to one aspect of this application, a microalloyed AlSi is provided. 10 Mg alloy powder includes an alloy matrix and Er and Zr elements doped in the alloy matrix, wherein the mass content of Er element is 0.7-1.3% and the mass content of Zr element is 0.7-1.3%; the alloy matrix is ​​AlSi10Mg alloy.

[0008] Furthermore, the mass ratio of Er to Zr is 1:(0.65-1).

[0009] Furthermore, AlSi 10 The Mg alloy contains the following components by mass fraction: Si: 9.5-10.5%, Mg: 0.35-0.55%, with the balance being Al and unavoidable impurities, and the total mass content of unavoidable impurities is ≤0.0815%.

[0010] Furthermore, unavoidable impurities include at least one of Fe, Cu, Ti, Zn, Mn, O, and N.

[0011] Furthermore, by mass fraction, microalloyed AlSi 10 In Mg alloy powder, Fe≤0.01%, Cu≤0.01%, Ti≤0.01%, Zn≤0.01%, Mn≤0.01%, O≤300ppm, and N≤15ppm.

[0012] A second aspect of this application provides a microalloyed AlSi 10 The preparation method of Mg alloy powder includes the following steps: according to the micro-alloying AlSi... 10 The mass fraction of Mg alloy powder components was determined by weighing and mixing raw materials, followed by sequential melting, refining, and atomization to obtain microalloyed AlSi. 10 Mg alloy powder.

[0013] Furthermore, the melting temperature is 850-950℃, and the melting time is 15-30 minutes.

[0014] Furthermore, the refining temperature is 850-950℃, and the refining time is 10-15 minutes.

[0015] Furthermore, atomization is achieved through a guide tube with a diameter of 4.5-5.0 mm, an atomization pressure of 2.3-2.8 MPa, and an atomization temperature of 850-900℃.

[0016] Furthermore, microalloyed AlSi 10 The Mg alloy powder has a particle size Dv10 of 20-27 μm, a particle size Dv50 of 35-40 μm, and a particle size Dv90 of 60-67 μm; and the microalloyed AlSi has a particle size Dv100 ≤ 75 μm. 10 The volume fraction of Mg alloy powder is ≥97%.

[0017] Furthermore, microalloyed AlSi 10 The sphericity of Mg alloy powder is ≥80%.

[0018] Furthermore, microalloyed AlSi 10The hollow powder ratio of Mg alloy powder is ≤0.43%.

[0019] The third aspect of this application provides a 3D device, the raw material of which is the microalloyed AlSi provided in the first aspect of this application. 10 Mg alloy powder or microalloyed AlSi obtained by the preparation method provided in the second aspect of this application 10 Mg alloy powder.

[0020] The fourth aspect of this application provides a method for fabricating a 3D device, the method comprising: microalloying AlSi 10 Mg alloy powder is added to a 3D printer to obtain 3D devices; micro-alloyed AlSi 10 The Mg alloy powder is the microalloyed AlSi provided in the first aspect of this application. 10 Mg alloy powder or microalloyed AlSi obtained by the preparation method provided in the second aspect of this application 10 Mg alloy powder.

[0021] Furthermore, the preparation method also includes an aging treatment after 3D printing, with the aging temperature being 165-170℃ and the aging time being 1-2 hours.

[0022] Applying the technical solution of this application, the microalloyed AlSi provided by this application 10 Mg alloy powder, in AlSi 10 Doping Mg alloys with Er and Zr elements is beneficial because Er is abundant and inexpensive in the Earth's crust, making microalloyed AlSi... 10 The preparation cost of Mg alloy powder is reduced. Simultaneously, the synergistic effect of Er and Zr elements refines the grains and improves the alloy microstructure, thereby significantly improving the microalloying of AlSi. 10 Mechanical properties of Mg alloy powder.

[0023] The 3D device provided in this application utilizes the aforementioned microalloyed AlSi. 10 Using Mg alloy powder as raw material, it can achieve tensile strength of over 500MPa, yield strength of over 300MPa, and elongation of 8.0-9.5% without heat treatment, exhibiting excellent strength-toughness balance characteristics. Attached Figure Description

[0024] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:

[0025] Figure 1The microalloyed AlSi prepared according to Example 1 of this application is shown. 10 Scanning electron microscope image of Mg alloy powder.

[0026] Figure 2 The microalloyed AlSi prepared according to Example 1 of this application is shown. 10 Schematic diagram of particle size distribution of Mg alloy powder.

[0027] Figure 3 The microalloyed AlSi prepared according to Example 1 of this application is shown. 10 The results of the sphericity test of Mg alloy powder are shown in the figure.

[0028] Figure 4(a) shows the microalloyed AlSi prepared according to Example 1 of this application. 10 Metallographic micrographs of the hollow powder ratio of Mg alloy powder in fields 1-6; Figure 4(b) shows the microalloyed AlSi prepared according to Example 1 of this application. 10 Metallurgical microscope images of the hollow powder content of Mg alloy powder in fields 7-10.

[0029] Figure 5 An optical microscope image of an unaged 3D device prepared according to Application Example 1 of this application is shown.

[0030] Figure 6 An optical microscope image of an unaged 3D device prepared according to Application Example 17 of this application is shown.

[0031] Figure 7 An EBSD image of an aged 3D device prepared according to Application Example 1 of this application is shown. Detailed Implementation

[0032] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.

[0033] As described in the background section of this application, conventional AlSi 10 Mg alloys have low strength, especially in AlSi alloys. 10 Adding rare earth element Sc to Mg alloys can improve the microalloying of AlSi. 10 The strength of Mg alloys, but leading to microalloying of AlSi 10 The preparation cost of Mg alloys increases significantly, making them unsuitable for large-scale industrial applications. To address this issue, traditional microalloyed AlSi alloys... 10 To address the issues of low strength and high preparation cost of Mg alloy powder, this application provides a microalloyed AlSi...10 Mg alloy powder and its preparation method, 3D devices and their preparation methods.

[0034] In a first typical embodiment of this application, a microalloyed AlSi is provided. 10 Mg alloy powder, comprising an alloy matrix and Er and Zr elements doped into the alloy matrix, wherein the mass content of Er element is 0.7-1.3% and the mass content of Zr element is 0.7-1.3%; the alloy matrix is ​​AlSi. 10 Mg alloy.

[0035] The microalloyed AlSi provided in this application 10 In Mg alloy powder, in AlSi 10 Doping Mg alloys with Er and Zr elements is beneficial because Er is abundant and inexpensive in the Earth's crust, making microalloyed AlSi... 10 The preparation cost of Mg alloy powder is reduced, and based on the characteristic that Er element has low solid solubility in Al matrix, micro-alloyed AlSi is made possible. 10 During the crystallization process of Mg alloy powder, Er elements are repelled to the front of the solid-liquid interface, resulting in enrichment and effectively inhibiting cell growth. This not only reduces the long and short axis dimensions of columnar crystals but also promotes the formation of equiaxed crystals, effectively improving the mechanical properties of the alloy. Simultaneously, the relatively low solid solubility of Er elements in the Al matrix provides a stronger precipitation driving force for Al3Er, leading to the precipitation of a larger volume fraction of the Al3Er phase. The precipitated Al3Er phase has a high melting point and will not completely melt during remelting at the relatively low temperature at the molten pool boundary. It can serve as a heterogeneous nucleation site, promoting the formation of equiaxed crystals, refining grains, and effectively inhibiting cell growth, thereby significantly improving mechanical properties.

[0036] Furthermore, Er and Zr elements in microalloyed AlSi 10 During the solidification of Mg alloy powder, a kinetically stable L12 core-shell structure of Al3(Er,Zr) second phase can be formed. This second phase can refine grains by providing high-density, low-potential-energy heterogeneous nucleation sites at the solidification front, reducing the total critical undercooling required to induce equiaxed grain growth. Consequently, high-mechanical-performance microalloyed AlSi can be obtained without heat treatment. 10Mg alloy powder; and the second phase is distributed inside the equiaxed crystals and at the grain boundaries. The second phase located inside the equiaxed crystals can act as heterogeneous nucleation sites to promote the formation of equiaxed crystals to refine the grains, thereby hindering the movement of dislocations and delaying crack propagation, and improving strength. The second phase located at the grain boundaries can effectively inhibit cell growth, reduce the short axis size of columnar crystals, and improve strength and resistance to hot cracking. In addition, equiaxed crystals will hinder the continuous growth of the front end of columnar crystals, reduce the long axis size of columnar crystals, improve plasticity, significantly reduce anisotropy, make crack propagation difficult, and provide additional strengthening based on the pinning effect.

[0037] In addition, microalloyed AlSi 10 Within Mg alloy powder, a eutectic Si network is distributed at the cell boundaries. Mg readily accumulates at triangular grain boundaries, forming the Mg2Si phase with Si. After heat treatment, nanoscale second phases or β phases (Mg5Si6 or Mg5Al2Si4) formed by the combination of Mg and Si precipitate from the matrix. These phases are dispersed in the matrix and generate internal stress, hindering dislocation movement and further propagation of the main crack, thus achieving a strengthening effect. Therefore, a 500MPa-level Er / Zr composite microalloyed AlSi is achieved based on grain refinement strengthening and precipitation strengthening, resulting in a synergistic effect of high strength and toughness. 10 Mg alloy powder has broad application prospects in the field of additive manufacturing and can meet higher service requirements.

[0038] In some specific embodiments, microalloyed AlSi 10 In Mg alloy powder, the mass contents of Er and Zr elements are each independently any value from 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3% or any range between the two.

[0039] In some embodiments, the mass ratio of Er to Zr is 1:(0.65-1), which is more conducive to the formation of a high-density, finely dispersed L12 Al3(Er,Zr) core-shell structure second phase during laser additive manufacturing and subsequent heat treatment. This more effectively hinders dislocation movement, further enhancing the strengthening effect and exhibiting superior strength-toughness balance. Specifically, the mass ratio of Er to Zr is any value from 1:0.65, 1:0.7, 1:0.8, 1:0.9, 1:1, or any value within a range of two.

[0040] In some embodiments, the alloy matrix (AlSi) 10The Mg alloy contains the following components by mass fraction: Si: 9.5-10.5%, Mg: 0.35-0.55%, with the balance being Al and unavoidable impurities, and the total mass content of unavoidable impurities ≤ 0.0815%. Specifically, the mass content of Si can be any value or a range between 9.5%, 9.6%, 9.7%, 9.8%, 9.9%, 10.0%, 10.1%, 10.2%, 10.3%, 10.4%, and 10.5%; the mass content of Mg can be any value or a range between 0.35%, 0.37%, 0.39%, 0.41%, 0.43%, 0.45%, 0.47%, 0.49%, 0.51%, 0.53%, and 0.55%. A total mass content of unavoidable impurities ≤ 0.0815% is more conducive to improving the overall performance of the alloy matrix.

[0041] In some embodiments, the alloy matrix (AlSi) 10 In Mg alloys, unavoidable impurities include at least one of Fe, Cu, Ti, Zn, Mn, O, and N. "At least one of the above" means that the impurity can be any one of Fe, Cu, Ti, Zn, Mn, O, and N; any two or three of Fe, Cu, Ti, Zn, Mn, O, and N; or any four, five, six, or all of Fe, Cu, Ti, Zn, Mn, O, and N.

[0042] In some embodiments, microalloyed AlSi 10 In Mg alloy powder, by mass fraction, Fe≤0.01%, Cu≤0.01%, Ti≤0.01%, Zn≤0.01%, Mn≤0.01%, O≤300ppm, and N (nitrogen)≤15ppm. By limiting the content of each impurity and the total impurity content within this range, it is possible to further avoid the formation of coarse and brittle phases due to the segregation of impurity elements and defects such as hot cracks, porosity, and lack of fusion caused by oxide / nitride inclusions during the additive manufacturing process, thus ensuring the reliability of high-performance additive manufacturing aluminum alloy components.

[0043] In a second typical embodiment of this application, a microalloyed AlSi is provided. 10 The preparation method of Mg alloy powder includes the following steps: according to the micro-alloying AlSi... 10 The mass fraction of Mg alloy powder components was determined by weighing and mixing raw materials, followed by sequential melting, refining, and atomization to obtain microalloyed AlSi. 10 Mg alloy powder. This application involves microalloyed AlSi. 10 The preparation of Mg alloy powder can be carried out using conventional metal smelting methods, which are mature and easy to operate.

[0044] In some specific embodiments, microalloyed AlSi 10 The raw materials used in the Mg alloy composition are aluminum source, silicon source, magnesium source, erbium source and zirconium source. The aluminum source can be pure aluminum with a purity of ≥99.5%, the magnesium source can be pure magnesium with a purity of ≥99.5%, the silicon source can be an aluminum-silicon master alloy with a silicon mass percentage of 20% (purity ≥99%), the erbium source can be an aluminum-erbium master alloy with a erbium mass percentage of 5% (purity ≥99%), and the zirconium source can be an aluminum-zirconium master alloy with a zirconium mass percentage of 10% (purity ≥99%).

[0045] In some specific embodiments, before the raw materials are heated and melted, the melting chamber is evacuated to a vacuum level of about 50 Pa, and then replaced with a protective gas (the protective gas can be at least one of nitrogen and inert gas) before melting and refining operations are carried out.

[0046] In some embodiments, the melting temperature is 850-950℃, and the melting time is 15-30 min. Suitable melting temperature and time are more conducive to promoting the uniform diffusion of Er and Zr elements into the molten aluminum, avoiding segregation, and simultaneously inhibiting excessive Mg loss and oxidation absorption of the molten aluminum, preventing grain coarsening, and ensuring a uniform and pure melt composition, thus providing a high-quality melt for subsequent gas atomization powder production. Specifically, the melting temperature can be any value from 850℃, 860℃, 870℃, 880℃, 890℃, 900℃, 910℃, 920℃, 930℃, 940℃, and 950℃, or any range between two values; the melting time can be any value from 15 min, 20 min, 25 min, and 30 min, or any range between two values.

[0047] In some embodiments, the refining temperature is 850-950℃ and the refining time is 10-15 minutes. Suitable refining temperature and time are more conducive to efficient degassing and slag removal, reducing the microalloying of AlSi. 10 The impurity content in the Mg alloy powder and the porosity of the powder after atomization. The specific refining temperature can be any value or a range between 850℃, 860℃, 870℃, 880℃, 890℃, 900℃, 910℃, 920℃, 930℃, 940℃, and 950℃; the refining time can be any value or a range between 10 min and 15 min.

[0048] In some embodiments, a guide tube is used for atomization. The diameter of the guide tube is 4.5-5.0 mm, the atomization pressure is 2.3-2.8 MPa, and the atomization temperature is 850-900 °C. A suitable guide tube diameter is more conducive to obtaining powder with a narrower particle size distribution, effectively improving the powder yield. Combined with the atomization pressure and atomization temperature, it ensures that the gas can effectively act on the metal jet, achieving efficient crushing, improving sphericity, and reducing the rate of irregular and hollow powders, so as to obtain a powder morphology with superior physical properties. Specifically, the diameter of the guide tube can be any value or a range between 4.5mm, 4.6mm, 4.7mm, 4.8mm, 4.9mm, and 5.0mm; the atomization pressure can be any value or a range between 2.3MPa, 2.4MPa, 2.5MPa, 2.6MPa, 2.7MPa, and 2.8MPa; and the atomization temperature can be any value or a range between 850℃, 860℃, 870℃, 880℃, 890℃, and 900℃.

[0049] In some embodiments, microalloyed AlSi 10 The particle size of the Mg alloy powder is Dv10 of 20-27 μm, Dv50 of 35-40 μm, and Dv90 of 60-67 μm; and the particle size of the microalloyed AlSi10Mg alloy powder is ≤75 μm. 10 The volume fraction of Mg alloy powder is ≥97%, and microalloyed AlSi containing the above particle size distribution is used. 10 When Mg alloy powder is used in additive manufacturing, it not only possesses excellent gradation, flowability, and spreading properties, but also improves the uniformity and consistency of the powder during laser powder spreading, resulting in 3D devices with high density, fewer defects, and more precise interlayer bonding. This, in turn, enhances the mechanical strength, print quality, and reliability of the printed parts. Specifically, the particle size Dv10 can be any value or a range between 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, and 27μm; the particle size Dv50 can be any value or a range between 35μm, 36μm, 37μm, 38μm, 39μm, and 40μm; and the particle size Dv90 can be any value or a range between 60μm, 61μm, 62μm, 63μm, 64μm, 65μm, 66μm, and 67μm.

[0050] In some embodiments, microalloyed AlSi 10The sphericity of the Mg alloy powder is ≥80%, and / or the hollow powder ratio is ≤0.43%. Sphericity typically refers to the circularity under two-dimensional projection, calculated as the ratio of the area equivalent diameter of the particle's projection to its perimeter equivalent diameter. Hollow powder ratio refers to the percentage of powder particles containing closed cavities (hollow / pores) out of the total number of particles. Higher sphericity helps improve flowability during printing, ensuring tight bonding between layers. Furthermore, microalloyed AlSi10Mg alloy powder has the advantages of low hollow powder ratio and controllable particle size distribution, avoiding porosity during printing and thus better adapting to laser additive printing.

[0051] In a third typical embodiment of this application, a 3D device is provided, the raw material of which is the microalloyed AlSi provided in the first typical embodiment of this application. 10 Mg alloy powder or microalloyed AlSi prepared in the second typical embodiment of this application 10 Mg alloy powder. The 3D devices prepared using the two typical implementation methods described above exhibit high density, high strength, and high plasticity.

[0052] In a fourth typical embodiment of this application, a method for fabricating a 3D device is provided, comprising adding micro-alloyed AlSi10Mg alloy powder into a 3D printer and obtaining a 3D device by 3D printing; micro-alloyed AlSi 10 The Mg alloy powder is the microalloyed AlSi provided in the first typical embodiment of this application. 10 Mg alloy powder or microalloyed AlSi prepared in the second typical embodiment of this application 10 Mg alloy powder.

[0053] Using the above-mentioned microalloyed AlSi 10 When Mg alloy powder is used in 3D printing, microalloying of AlSi 10 During the solidification process of Mg alloy powder, Er and Zr elements form a kinetically stable L12 core-shell structure Al3(Er,Zr) second phase. The second phase can refine the grains by providing high-density, low-potential-energy heterogeneous nucleation sites at the solidification front, reducing the total critical undercooling required to induce equiaxed grain growth. As a result, 3D devices with tensile strength above 500 MPa, yield strength above 300 MPa, and elongation of 8.0-9.5% can be obtained without heat treatment.

[0054] In some embodiments, the preparation method further includes an aging treatment following 3D printing, i.e., aging the 3D-printed device at a temperature of 165-170°C for 1-2 hours. Due to the non-equilibrium solidification characteristics and uneven thermal cycling of laser forming during 3D printing, large residual stresses exist in the laser-added samples. These residual stresses severely affect mechanical properties. Therefore, performing a certain heat treatment on the 3D-printed sample can further eliminate defects and residual stresses and form a strengthening phase, thereby further improving its mechanical properties. Specifically, the aging treatment temperature can be any value from 165°C, 166°C, 167°C, 168°C, 169°C, and 170°C, or any value within a range of both. The aging treatment time can be any value from 1 hour, 1.5 hours, and 2 hours, or any value within a range of both.

[0055] In some embodiments, a scanning power of 350-370W and a scanning speed of 1300-2400mm / s in 3D printing are more conducive to improving the tensile strength and yield strength of 3D devices and to eliminating internal porosity. In some specific embodiments, the scanning power can be any value among 350W, 360W, and 370W or any value between two of these; the scanning speed can be any value among 1300mm / s, 1500mm / s, 1700mm / s, 1900mm / s, 2100mm / s, 2300mm / s, and 2400mm / s or any value between two of these.

[0056] In some embodiments, the 3D printer includes a printing chamber, a substrate for supporting the device, and a protective gas (nitrogen, argon, or helium, etc.) is introduced during the printing process. The oxygen content of the printing chamber is 0.00-0.05%, the pressure of the printing chamber is 23-27 mbar, the substrate preheating temperature is 80-100°C, the flow rate of the protective gas is 2.3-2.7 m / s, the interlayer thickness is 30 μm, the scanning pitch is 100 μm, the interlayer rotation angle is 67°, the scanning power is 350-370 W, the scanning speed is 1300-2400 mm / s, and the infill type during printing is a long straight line or a checkerboard pattern. In 3D printing, microalloyed AlSi with different compositions... 10 Different scanning power and scanning speed are used for Mg alloy powder, so appropriate process parameters can make the density of the printed parts no less than 99.8%, and the resulting devices are free of cracks and have few defects, which helps to improve the strength of 3D devices.

[0057] In some specific embodiments, the oxygen content of the printing chamber can be any value or a range between any two of 0.00%, 0.001%, 0.002%, 0.003%, 0.004%, and 0.005%; the pressure of the printing chamber can be any value or a range between any two of 23 mbar, 24 mbar, 25 mbar, 26 mbar, and 27 mbar; the substrate preheating temperature can be any value or a range between any two of 80°C, 85°C, 90°C, 95°C, and 100°C; and the flow rate of the protective gas can be any value or a range between any two of 2.3 m / s, 2.4 m / s, 2.5 m / s, 2.6 m / s, and 2.7 m / s.

[0058] The beneficial effects of this application will be further illustrated below with reference to embodiments and comparative examples.

[0059] Example 1

[0060] A microalloyed AlSi 10 Mg alloy powder is prepared according to the following method:

[0061] S1. Weigh out the raw materials as follows: pure aluminum (purity ≥99.5%), pure magnesium (purity ≥99.5%), aluminum-silicon master alloy (silicon mass percentage 20%, purity ≥99%), aluminum-erbium master alloy (erbium mass percentage 5%, purity ≥99%), and aluminum-zirconium master alloy (zirconium mass percentage 10%, purity ≥99%) to obtain a mixed raw material. The raw materials in the following examples are the same as those in Example 1 and will not be repeated.

[0062] S2. Place the mixed raw materials in the melting chamber and evacuate the melting chamber to a vacuum degree of about 50 Pa. Replace the gas with high-purity argon (purity ≥99%). After the replacement is completed, perform alloy melting and refining. The temperature and time during the melting process are 850℃ and 20 min, respectively, and the temperature and time during the refining process are 850℃ and 15 min, respectively, to obtain aluminum alloy melt.

[0063] S3. The molten aluminum alloy is poured into an intermediate ladle in stages and subjected to gas atomization powder production.

[0064] The atomization conditions are as follows: argon is used as the atomizing gas, the diameter of the atomizing guide tube is 4.5 mm, the atomizing gas pressure is 2.5 MPa, the atomization temperature is 850℃, and the atomization speed is 10 kg / min, to obtain atomized alloy powder;

[0065] S4. After cooling the atomized alloy powder to room temperature, the alloy powder is first passed through an air jet for classification, and then passed through an ultrasonic vibrating screen for particle size separation. The screen mesh size is 150 mesh, to obtain micro-alloyed AlSi. 10 Mg alloy powder.

[0066] Example 2-10

[0067] The difference between Examples 2-10 and Example 1 lies in the microalloying of AlSi. 10 The composition of Mg alloy powder varies, as shown in Table 1.

[0068] Example 11

[0069] The difference between Example 11 and Example 1 lies in the different preparation conditions in each step, as detailed below:

[0070] In step S2, the melting temperature is 950℃ and the melting time is 15min; the refining temperature is 950℃ and the refining time is 15min.

[0071] In step S3, the diameter of the atomizing guide tube is 5.0 mm, the atomizing gas pressure is 2.8 MPa, and the atomizing temperature is 900℃.

[0072] Example 12

[0073] The difference between Example 12 and Example 1 is that in step S2, the melting temperature is 800°C, the melting time is 20 min, the refining temperature is 800°C, and the refining time is 15 min.

[0074] Example 13

[0075] The difference between Example 13 and Example 1 is that in step S3, the atomization pressure is 2.0 MPa and the atomization temperature is 950°C.

[0076] Example 14

[0077] The difference between Example 14 and Example 1 is that in step S3, the atomization pressure is 3.0 MPa and the atomization temperature is 800°C.

[0078] Example 15

[0079] The difference between Example 15 and Example 1 is that in step S2, the melting temperature is 1050°C, the melting time is 20 min, the refining temperature is 1050°C, and the refining time is 10 min.

[0080] Comparative Examples 1-8

[0081] The difference between Comparative Examples 1-8 and Example 1 is that the contents of Er and Zr in the alloy powder are different, as shown in Table 1.

[0082] Table 1. Composition of microalloyed AlSi10Mg alloy (wt%)

[0083]

[0084] Performance testing

[0085] The microalloyed AlSi obtained in the above embodiments and comparative examples 10 The particle size, sphericity, and hollow powder ratio of Mg alloy powder were tested, and the powder yield was calculated. The results are shown in Table 2.

[0086] Among them, (1) the particle size test method is: use a laser particle size analyzer to detect and read directly.

[0087] (2) The test method for sphericity is as follows: The test method refers to JY / T0584-2020, and the characterization and determination are carried out by scanning electron microscope. Specifically, the sphericity is calculated according to the standard operating procedure for particle characteristics of ASTM F1877-16.

[0088] (3) The test method for hollow powder rate is as follows: The test method refers to GB / T41978-2022. After the sample is mounted, ground and polished, 10 fields of view are randomly selected under a 200× metallographic microscope for shooting and statistics. The formula for calculating hollow powder rate is: hollow powder rate = (number of hollow particles / total number of particles detected) × 100%.

[0089] Table 2 Microalloyed AlSi 10 Mg Alloy Powder Performance Test Table

[0090]

[0091] Figure 1 The microalloyed AlSi obtained in Example 1 of this application 10 Scanning electron microscope images of Mg alloy powder, from Figure 1 As can be seen from this, microalloyed AlSi 10 Most of the Mg alloy powder has a round, approximately spherical surface.

[0092] Figure 2 The microalloyed AlSi obtained in Example 1 of this application 10 The particle size distribution of Mg alloy powder shows that the particle size Dv10 is between 20-27 μm, the particle size Dv50 is between 35-40 μm, and the particle size Dv90 is between 60-67 μm.

[0093] Figure 3The microalloyed AlSi obtained in Example 1 of this application 10 The image shows the sphericity test results of Mg alloy powder. Figure 3 It can be seen that microalloyed AlSi 10 Mg alloy powder has a high sphericity, which helps to improve the flowability of the printing process.

[0094] Figure 4(a) shows the microalloyed AlSi obtained in Example 1 of this application. 10 Metallurgical micrographs of the hollow powder ratio of Mg alloy powder under fields of view 1-6. Figure 4(b) shows the microalloyed AlSi obtained in Example 1 of this application. 10 Metallographic micrographs of Mg alloy powder under the 7th to 10th fields of view regarding the hollow powder ratio. As can be seen from Figure 4 (a) and (b), the number of hollow powder particles under each field of view is small, and the overall hollow powder ratio is low.

[0095] As can be seen from the test results in Table 1, the microalloyed AlSi obtained in Examples 1-11 of this application... 10 The Mg alloy powder has an oxygen content of <200ppm and a nitrogen content of <15ppm, and exhibits good particle size consistency. The particle size Dv10 is between 20-27μm, the particle size Dv50 is between 35-40μm, and the particle size Dv90 is between 60-67μm. The sphericity is >80%, indicating high sphericity. The hollow powder rate is ≤0.43%, and the powder yield of this preparation method is between 39-45%, indicating that the preparation method has stable process and strong controllability.

[0096] Compared to Example 1, Examples 12 and 15 show improvements when the melting and refining temperatures are lower or higher than those of Example 1. The resulting microalloyed AlSi... 10 The hollow powder ratio of the Mg alloy powder was >0.43%, and the sphericity was <80%. This is likely because melting and refining temperatures are key parameters determining the surface tension and viscosity of droplets. Excessively high or low melting and refining temperatures can disrupt the stability of droplets during atomization, increasing the hollow powder ratio and decreasing the sphericity. Furthermore, in Example 15, the excessively high temperature caused Mg element burn-off, thus affecting the microalloyed AlSi. 10 The magnesium content in Mg alloy powder is reduced.

[0097] Compared to Example 1, Examples 13-14 show that when the atomization pressure and temperature are higher or lower than the limits specified in this application, the microalloyed AlSi obtained is... 10 The hollow powder ratio of the Mg alloy powder is all >0.43%, and the sphericity is all <80%.

[0098] Microalloyed AlSi obtained from Comparative Examples 1-8 10The particle sizes of the Mg alloy powders are all between 20-27 μm (Dv10), 35-40 μm (Dv50), and 60-67 μm (Dv90), with sphericity >80% and hollow powder ratio ≤0.43%.

[0099] Application Example 1

[0100] A 3D device is obtained using the following fabrication method:

[0101] The microalloyed AlSi obtained in Example 1 10 Mg alloy powder is added to a 3D printer for device printing. The specific process parameters of the 3D printer are as follows: oxygen content in the printing chamber is 0.00%, pressure in the printing chamber is 25 mbar, substrate preheating temperature is 100℃, protective gas flow rate is 2.5 m / s, interlayer thickness is 30 μm, scanning spacing is 100 μm, interlayer rotation angle is 67°, printing strategy fill type is long straight line, scanning power is 350W, and scanning speed is 1500 mm / s, to obtain the 3D printed device.

[0102] The above-mentioned 3D device was subjected to aging treatment at 165℃ for 2 hours to obtain the heat-treated 3D device.

[0103] Application Example 2

[0104] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 2. 10 Mg alloy powder was used for printing, with a scanning power of 350W and a scanning speed of 1300mm / s, to obtain a 3D printed device. All other conditions were the same as in Application Example 1.

[0105] Application Example 3

[0106] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 3. 10 Mg alloy powder was used for printing, with a scanning power of 370W and a scanning speed of 1800mm / s, to obtain a 3D printed device. All other conditions were the same as in Application Example 1.

[0107] Application Example 4

[0108] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 4. 10 Mg alloy powder was used for printing, with a scanning power of 350W and a scanning speed of 1300mm / s, to obtain a 3D printed device. All other conditions were the same as in Application Example 1.

[0109] Application Example 5

[0110] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 5. 10 Mg alloy powder was used for printing, with a scanning power of 370W and a scanning speed of 1800mm / s, to obtain a 3D printed device. All other conditions were the same as in Application Example 1.

[0111] Application Example 6

[0112] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 6. 10 Mg alloy powder was used for printing, and the above 3D device was subjected to aging treatment at 165°C for 1.5 hours to obtain the heat-treated 3D device. All other conditions were the same as in Application Example 1.

[0113] Application Example 7

[0114] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 7. 10 Mg alloy powder was used for printing, with a scanning power of 360W and a scanning speed of 1500mm / s, to obtain 3D printed devices.

[0115] Application Example 8

[0116] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Example 8. 10 Mg alloy powder was used for printing, with a scanning power of 360W and a scanning speed of 1600mm / s, to obtain 3D printed devices.

[0117] Application Example 9-15

[0118] A 3D device, differing from Application Example 1, uses microalloyed AlSi obtained in Examples 9-15. 10 Mg alloy powder was used as the raw material for printing, and all other conditions were the same as in Application Example 1.

[0119] Application Example 16

[0120] A 3D device differs from Application Example 1 in that the printing strategy fill type is checkerboard, the scanning speed is 2300mm / s, the aging treatment temperature is 170℃, the aging treatment time is 2h, and all other conditions are the same as in Application Example 1.

[0121] Application Example 17

[0122] A 3D device differs from Application Example 1 in that it has a scanning power of 320W and a scanning speed of 1400mm / s, while all other conditions are the same as in Application Example 1.

[0123] Application Example 18

[0124] A 3D device differs from Application Example 1 in that the 3D printed device is subjected to aging treatment at 280°C for 2 hours to obtain a heat-treated 3D device, while all other conditions are the same as in Application Example 1.

[0125] Comparative Application Example 1

[0126] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 1. 10 The Mg alloy powder was scanned at a power of 260W and a scanning speed of 1600mm / s, with all other conditions being the same as in Application Example 1.

[0127] Comparative Application Example 2

[0128] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 2. 10 The Mg alloy powder was scanned at a power of 300W and a scanning speed of 1800mm / s, with all other conditions being the same as in Application Example 1.

[0129] Comparative Application Example 3

[0130] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 3. 10 The Mg alloy powder was scanned at a power of 280W and a scanning speed of 1700mm / s, with all other conditions being the same as in Application Example 1.

[0131] Comparative Application Example 4

[0132] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 4. 10 The Mg alloy powder was scanned at a power of 250W and a scanning speed of 1400mm / s, with all other conditions being the same as in Application Example 1.

[0133] Comparative Application Example 5

[0134] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 5. 10 The Mg alloy powder was scanned at a power of 250W and a scanning speed of 1300mm / s, with all other conditions being the same as in Application Example 1.

[0135] Comparative Application Example 6

[0136] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 6. 10The Mg alloy powder was scanned at a power of 340W and a scanning speed of 1600mm / s, with all other conditions being the same as in Application Example 1.

[0137] Comparative Application Example 7

[0138] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 7. 10 The Mg alloy powder was scanned at a power of 260W and a scanning speed of 1800mm / s, with all other conditions being the same as in Application Example 1.

[0139] Comparative Application Example 8

[0140] A 3D device, differing from Application Example 1, employs the microalloyed AlSi obtained in Comparative Example 7. 10 Mg alloy powder was used, with a scanning power of 430W and a scanning speed of 1400mm / s. The 3D printed device was then subjected to aging treatment at 280℃ for 2 hours, with all other conditions being the same as in Application Example 1.

[0141] Performance testing

[0142] The tensile strength, yield strength, and elongation of the 3D devices prepared in the above application examples and comparative application examples without aging treatment and the 3D devices prepared with aging treatment were tested respectively. At the same time, the internal structure of the 3D devices without aging treatment and the 3D devices prepared with aging treatment were detected by scanning electron microscopy. The density of the 3D devices prepared in the above application examples and comparative application examples without aging treatment was also detected. The test results are shown in Table 3.

[0143] Among them, (1) density detection involves characterizing the sample under a metallographic microscope after it has been inlaid, ground and polished, and the porosity module in the image analysis system is used to directly read the value.

[0144] (2) The tensile strength, yield strength and elongation of the 3D device were measured by a universal testing machine, and the testing method was carried out in accordance with the relevant provisions in GB / T 228.1-2021.

[0145] Table 3 Performance Test Results of 3D Devices

[0146]

[0147] Continued from Table 3

[0148]

[0149] Note: The average grain size after aging treatment is the total average of the sizes of equiaxed and columnar crystals.

[0150] Figure 5 The image shows an optical microscope image of the 3D device without aging treatment in Example 1. The optical microscope image shows that there are no cracks and few defects in the tissue.

[0151] Figure 6 The image shows an optical microscope image of the 3D device without aging treatment, as described in Example 17. It can be seen from the image that there are obvious pores inside the 3D device, with the largest pore size reaching 66.13 μm.

[0152] Figure 7 The image shows the EBSD diagram of the 3D device after aging treatment in Application Example 1. As can be seen from the EBSD diagram, the structure is a bimodal structure with alternating columnar and equiaxed crystals, and the boundary forms equiaxed crystals while the interior is columnar crystals.

[0153] Based on the test results in Table 3, it can be seen that:

[0154] The 3D devices obtained in Examples 1-11 of this application all have a density of over 99.9%. Without aging treatment, their tensile strength is >500MPa, yield strength is >300MPa, and elongation is ≥8.0%, demonstrating high strength and toughness. This achieves a performance leap from "printable structural components" to "load-bearing structural components." After a simple and short-term aging treatment, composite precipitation of Si-rich phase and β'-Mg2Si phase can be induced on the basis of the printed supersaturated solid solution, further improving its tensile strength and yield strength. The average grain size of its equiaxed and columnar crystals is in the range of 1.71-1.75μm, opening up a new application space for traditional Al-Si materials in 500MPa-level load-bearing structural components. This forms a dual advantage of performance and cost, namely cost reduction, simplified process, and high strength and toughness. It can be applied to the requirements of 500MPa-level lightweight new design-level key load-bearing structural components in aerospace, defense, new energy vehicles and other fields, providing a disruptive material solution for expanding the engineering application boundaries of Al-Si additive manufacturing alloys.

[0155] Compared with Application Example 1, Application Examples 12-15 show that when microalloyed AlSi 10 When the particle size distribution of Mg alloy powder is large and / or the hollow powder ratio is high and the sphericity is low, it is not conducive to improving the loose density of the powder, which reduces the powder spreading quality and uniformity. At the same time, more pores are introduced during the printing process, resulting in the tensile strength of the unaged 3D devices being below 500MPa, the yield strength being significantly lower than the yield strength in Application Example 1, and the elongation being below 8%. Heat treatment is required to reach the 500MPa level.

[0156] Compared to Application Example 1, when the fill type is adjusted to checkerboard, this strategy reduces stress during the printing process. When the scanning speed is increased to 2300 mm / s, the tensile strength of the unaged 3D devices obtained is all >500 MPa, the yield strength is all >300 MPa, and the elongation is ≥8.0%, which has a high strength and toughness effect.

[0157] Compared to Application Example 1, Application Example 17 shows that when the printed microalloyed AlSi... 10 The Mg alloy powder is the same, but when using an inappropriate printing process: scanning power of 350W and scanning speed of 1400mm / s, combined with... Figure 6 The unaged 3D device not only showed obvious pores, but also had significantly lower tensile strength, yield strength, and elongation than Application Example 1. Furthermore, even after aging treatment, the tensile strength did not reach 500 MPa. This further illustrates that a suitable printing process can help improve the strength of 3D devices.

[0158] Compared to Application Example 1, Application Example 18, after the same 3D device was subjected to aging treatment at a higher temperature, resulted in coarsening of the eutectic Si skeleton and an average grain size of 3.19 μm, which significantly reduced the strength of the 3D device.

[0159] Compared with Application Example 1, Comparative Examples 1-6 show that the microalloyed AlSi obtained using Comparative Examples 1-6... 10 After 3D printing with Mg alloy powder, the tensile strength of the 3D devices obtained by comparative application examples 1-6 after aging treatment did not reach 500MPa, and the yield strength, except for comparative application example 4, did not reach 300MPa. It can be seen that the synergy between the Er and Zr elements in this application ensures that the 3D device can be obtained as a load-bearing structural component with a strength of 500MPa even without aging treatment.

[0160] Compared with Application Example 1, when Zr element is missing or Er and Zr elements are not added, the average grain size of the 3D device after aging treatment obtained in Application Example 7-8 is above 3μm. The tensile strength of the 3D device after aging treatment is much lower than 500MPa and the yield strength is much lower than 300MPa. It can be seen that the combined use of Er and Zr elements improves the strength of the 3D device.

[0161] As can be seen from the above description, the embodiments of this application achieve the following technical effects:

[0162] This application selects specific microalloyed AlSi 10 The composition of Mg alloy powder utilizes the synergistic effect of Er and Zr elements to refine grains and improve the alloy microstructure, thereby significantly improving the microalloying of AlSi.10 Mechanical properties of Mg alloy powder.

[0163] The 3D device provided in this application utilizes the aforementioned microalloyed AlSi. 10 Using Mg alloy powder as raw material, it can achieve tensile strength of over 500MPa, yield strength of over 300MPa, and elongation of 8.0-9.5% without heat treatment, exhibiting excellent strength-toughness balance characteristics.

[0164] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A microalloyed AlSi 10 Mg alloy powder, characterized in that, The alloy comprises an alloy matrix and Er and Zr doped in the alloy matrix, wherein the mass content of the Er is 0.7-1.3%, the content of the Zr is 0.7-1.3%; the alloy matrix is AlSi 10 Mg alloy.

2. The microalloyed AlSi according to claim 1 10 Mg alloy powder, characterized in that, The mass ratio of Er to Zr is 1:(0.65-1).

3. The microalloyed AlSi according to claim 1 or 2 10 Mg alloy powder, characterized in that, The AlSi 10 The Mg alloy comprises the following mass fractions of components: Si: 9.5-10.5%, Mg: 0.35-0.55%, the balance being Al and inevitable impurities, and the total mass content of the inevitable impurities is ≤0.0815%. Preferably, the unavoidable impurities include at least one of Fe, Cu, Ti, Zn, Mn, O, and N; Preferably, the micro-alloyed AlSi 10 In the Mg alloy powder, Fe ≤ 0.01 %, Cu ≤ 0.01 %, Ti ≤ 0.01 %, Zn ≤ 0.01 %, Mn ≤ 0.01 %, O ≤ 300 ppm, N ≤ 15 ppm.

4. A method for preparing microalloyed AlSi10Mg alloy powder according to any one of claims 1 to 3, characterized in that, It comprises the following steps: weighing raw materials according to the micro-alloyed AlSi 10 The micro-alloyed AlSi 10 Mg alloy powder component.

5. The preparation method according to claim 4, characterized in that, The melting temperature is 850-950℃, and the melting time is 15-30 minutes; And / or, the refining temperature is 850-950℃, and the refining time is 10-15 min; And / or, the atomization is performed through a guide tube with a diameter of 4.5-5.0 mm, the atomization pressure is 2.3-2.8 MPa, and the atomization temperature is 850-900 °C.

6. The preparation method according to claim 4, characterized in that, The micro-alloyed AlSi 10 The micro-alloyed AlSi 10 The volume fraction of the Mg alloy powder is ≥ 97%.

7. The preparation method according to any one of claims 4 to 6, characterized in that, The micro-alloyed AlSi 10 The sphericity of the Mg alloy powder is ≥ 80%; and / or, the micro-alloyed AlSi 10 The hollow powder rate of the Mg alloy powder is ≤ 0.43%.

8. A 3D device, characterized in that, The raw material for the 3D device is the microalloyed AlSi as described in any one of claims 1 to 3. 10 Mg alloy powder or microalloyed AlSi obtained by the preparation method according to any one of claims 4 to 7 10 Mg alloy powder.

9. A method for fabricating a 3D device according to claim 8, characterized in that, The preparation method includes: microalloying AlSi 10 Mg alloy powder is added to a 3D printer, and 3D devices are obtained through 3D printing; wherein, the microalloyed AlSi 10 The Mg alloy powder is the microalloyed AlSi as described in any one of claims 1 to 3. 10 Mg alloy powder or microalloyed AlSi obtained by the preparation method according to any one of claims 4 to 7 10 Mg alloy powder.

10. The preparation method according to claim 9, characterized in that, The preparation method further includes an aging treatment performed after the 3D printing, wherein the aging treatment temperature is 165-170℃ and the aging treatment time is 1-2 hours.