A process for obtaining nickel-based cast equiaxed crystal high-temperature alloy with curved grain boundaries and an alloy with curved grain boundaries
By employing a bent grain boundary heat treatment process in nickel-based cast equiaxed superalloys, bent grain boundaries are formed through the interaction of γ' phase and secondary carbides, thus solving the problem of insufficient grain boundary strength in cast equiaxed superalloys and improving high-temperature creep life and mid-temperature plasticity.
Patent Information
- Application Number
- CN202611616495.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are insufficient to improve the grain boundary strength of cast equiaxed superalloys, leading to grain boundary slip and intergranular brittle fracture at high temperatures, which affects the high-temperature creep life and mid-temperature plasticity of the alloy.
A bent grain boundary heat treatment process is adopted, which forms bent grain boundaries by performing subsolution treatment and intermediate temperature holding treatment in nickel-based cast equiaxed superalloys. The interaction between γ' phase and secondary carbides at the grain boundaries enhances the grain boundary strength.
It significantly improves the high-temperature creep life and mid-temperature plasticity of cast equiaxed superalloys, enhances their resistance to deformation and damage, and does not change the alloy composition or manufacturing process.
Smart Images

Figure CN123152971A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature alloy heat treatment, and more specifically, relates to a heat treatment process for obtaining bent grain boundaries in nickel-based cast equiaxed high-temperature alloys and alloys with bent grain boundaries. Background Technology
[0002] Nickel-based superalloys possess high high-temperature strength, good plasticity and fracture toughness, as well as excellent comprehensive properties such as oxidation resistance and hot corrosion resistance, and are now widely used in aero engines and industrial gas turbines.
[0003] Cast equiaxed superalloys exhibit high intragranular strength but low grain boundary strength at high temperatures. Grain boundaries become weak points in the load-bearing capacity of cast equiaxed superalloys at high temperatures, directly determining their critical properties such as high-temperature durability, creep resistance, and mid-temperature plasticity. Therefore, it is crucial to improve grain boundary strength to enhance the high-temperature strength of cast equiaxed superalloys. Conventional grain boundary strengthening methods rely on trace elements and precipitates for regulation, which are insufficient to address grain boundary failure at the grain boundary itself. Traditional straight-grain-boundary superalloys are prone to grain boundary slip and intergranular brittle fracture in the high-temperature service range, resulting in insufficient component life and low plasticity, failing to meet requirements. Simultaneously, it is necessary to improve the coordinated deformation capability between alloy grain boundaries and the grain interior to avoid excessive strength within the grains, which could reduce plasticity and affect the alloy's usability.
[0004] To address the aforementioned issues, bent grain boundaries are one optimized option. Bent grain boundary treatment induces wavy or serrated bending morphology transformations in grain boundaries, forming a bent grain boundary structure. This is a low-cost, industrially scalable grain boundary engineering technique. Bent grain boundaries can significantly increase grain boundary length, alter interfacial stress distribution, and optimize grain boundary morphology and precipitates. On one hand, it coordinates intragranular and grain boundary deformation; on the other hand, it delays crack propagation in alloys under high-temperature loading conditions, breaking through the performance bottleneck of high-temperature alloys at the microstructural level, thereby improving the alloy's resistance to deformation and damage.
[0005] Bending grain boundary treatment can significantly improve the high-temperature creep life of high-temperature alloys, enhance their mid-temperature plasticity, and even strengthen their fatigue and thermal cycling resistance, without altering the alloy composition or manufacturing process. This technology is of great significance in overcoming the performance limitations of hot-end components in high-end equipment and ensuring the independent control and safe service of current high-temperature alloy components.
[0006] Currently, research on bent grain boundaries in high-temperature alloys mainly focuses on wrought high-temperature alloys. This is because wrought high-temperature alloys have small grain sizes, relatively straight grain boundaries, and low γ' phase content. Due to the low γ' phase content, the precipitation strengthening ability of wrought high-temperature alloys is insufficient. Therefore, using bent grain boundaries to improve the mechanical properties of wrought high-temperature alloys and avoid straight grain boundaries is particularly important. However, research on bent grain boundaries in cast equiaxed high-temperature alloys is relatively limited. Cast equiaxed high-temperature alloys have a high γ' phase content, and mechanical properties are generally improved by controlling the γ' phase content, size, and distribution. However, as mentioned earlier, while γ' phase optimization improves intragranular strength, it does not improve grain boundary strength. The incoordination between grain boundary and intragranular deformation is detrimental to the overall performance of the alloy. Therefore, it is necessary to improve the grain boundary strength of cast equiaxed high-temperature alloys to enhance their high-temperature creep life. Summary of the Invention
[0007] The purpose of this invention is to address the shortcomings of existing technologies by proposing a heat treatment process for obtaining bent grain boundaries in nickel-based cast equiaxed superalloys and producing alloys with bent grain boundaries. This invention achieves bent grain boundaries between the grains of nickel-based cast equiaxed superalloys.
[0008] To achieve the above objectives, the present invention provides a heat treatment process for obtaining bent grain boundaries in nickel-based cast equiaxed superalloys, the heat treatment process comprising the following steps: S1: Heat the nickel-based cast equiaxed superalloy to a first temperature below its solution temperature, hold it at that temperature for a first preset time, and then cool it to room temperature to achieve subsolution treatment and obtain the alloy after subsolution treatment. S2: The alloy after subsolution treatment is kept at the temperature range in which the γ′ phase and secondary carbides precipitate for a second preset time, and then cooled to room temperature to achieve intermediate temperature holding treatment, thereby obtaining a nickel-based cast equiaxed high-temperature alloy with bent grain boundaries.
[0009] According to the present invention, preferably, in step S1: The first temperature is a temperature 5-30°C lower than the solution temperature of the nickel-based cast equiaxed superalloy. The first preset duration is 1 to 5 hours.
[0010] According to the present invention, preferably, in step S1: the cooling method is air cooling or furnace cooling; the cooling rate of the furnace cooling is 2~20℃ / min.
[0011] According to the present invention, preferably, in step S2: the second preset duration is 5~200h.
[0012] According to the present invention, preferably, in step S2, the cooling method is air cooling.
[0013] According to the present invention, preferably, in steps S1 and S2, the room temperature is 15-35°C.
[0014] According to the present invention, preferably, the nickel-based cast equiaxed superalloy comprises, by weight: Cr: 10.0~13.0%, Co: 8.0~11.0%, Mo: 1.0~2.5%, W: 3.0~5.0%, Ta: 3.0~6.0%, Al: 3.0~6.0%, Ti: 3.0~4.0%, C: 0~0.2%, B: 0~0.05%.
[0015] According to the present invention, preferably, the nickel-based cast equiaxed superalloy is cast nickel-based superalloy K466, and further, the creep rupture life of the nickel-based cast equiaxed superalloy with bent grain boundaries is ≥69h under the conditions of 900℃ and 314MPa.
[0016] Another aspect of the present invention provides a nickel-based cast equiaxed superalloy with bent grain boundaries obtained by the aforementioned heat treatment process.
[0017] The beneficial effects of the technical solution of the present invention are as follows: This invention targets cast equiaxed superalloys: (1) First, a subsolution treatment is performed at 5~30℃ below the solid solution temperature of the cast equiaxed superalloy for 1~5h to dissolve most of the irregularly shaped γ' phase; then, air cooling or furnace cooling is performed to room temperature. At this time, a uniform γ' phase will precipitate in most areas. Meanwhile, the subsolution treatment retains the coarse γ' phase and the γ / γ' eutectic phase, and dissolves less of the initial MC carbide. These coarse γ' phases, the initial MC carbide and the γ / γ' eutectic phase will hinder grain boundary migration during the grain boundary migration process of the subsolution, thereby forming the first stage of bent grain boundaries. (2) Then, the intermediate temperature holding treatment is carried out for 5~200h within the temperature range of γ' phase and secondary carbide precipitation, and then air-cooled to room temperature; during the second holding time stage, the precipitated secondary carbide will interact with the grain boundary, further promoting the grain boundary bending, and finally obtaining the bent grain boundary of nickel-based cast equiaxed superalloy; at the same time, the present invention regulates the precipitation of γ' phase and grain boundary carbide through intermediate temperature holding treatment, and while obtaining the bent grain boundary, the size of the intragranular strengthening phase γ' phase and the grain boundary carbide phase are both moderate, thereby effectively controlling the size of the alloy precipitated phase, strengthening the grain boundary, improving the high temperature creep life of nickel-based cast equiaxed superalloy, and also helping to improve its comprehensive mechanical properties.
[0018] The heat treatment process of this invention is simple and easy to implement.
[0019] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0020] The above and other objects, features and advantages of the present invention will become more apparent from the more detailed description of exemplary embodiments of the invention in conjunction with the accompanying drawings.
[0021] Figure 1 A scanning electron microscope image (scale bar 10 μm) of the flat grain boundary blocky sample obtained in Comparative Example 1 of the present invention is shown.
[0022] Figure 2 A scanning electron microscope image (scale bar 10 μm) of the bent grain boundary block sample obtained in Example 1 of the present invention is shown.
[0023] Figure 3 A scanning electron microscope image (scale bar 20 μm) of the bent grain boundary block sample obtained in Example 1 of the present invention is shown. Detailed Implementation
[0024] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided so that the invention will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0025] Example 1
[0026] This embodiment provides a heat treatment process for obtaining bent grain boundaries in nickel-based cast equiaxed superalloys, the heat treatment process including the following steps: S1: The nickel-based cast equiaxed superalloy is heated to a first temperature of 1220°C, which is lower than its solution temperature, and held at that temperature for 2 hours before being air-cooled to room temperature of 25°C to achieve subsolution treatment and obtain the alloy after subsolution treatment. In this embodiment, two types of nickel-based cast equiaxed superalloys were used: a 15mm×10mm×10mm block sample and a 68mm×15mm×15mm strip sample cut from cast nickel-based superalloy K466 by wire cutting. The heat treatment process of this embodiment was carried out. S2: The alloy after the subsolution treatment is kept at 900°C, the temperature at which the γ′ phase and secondary carbides precipitate, for 160 hours and then air-cooled to room temperature of 25°C to achieve intermediate temperature holding treatment, thereby obtaining blocky samples with bent grain boundaries and strip-shaped samples with bent grain boundaries respectively.
[0027] In this embodiment, a metallographic preparation procedure was performed on a blocky sample with curved grain boundaries to obtain an alloy sample with the microstructure to be tested. The microstructure of the alloy sample in the heat-treated state was observed using a scanning electron microscope, and the results are as follows: like Figure 2As shown, after heat treatment using the process described in this embodiment, coarse γ' phase, γ / γ' eutectic phase, and initial MC carbides exist near the grain boundaries. These coarse γ' phase, initial MC carbides, and γ / γ' eutectic phases hinder grain boundary migration during the subsolid solution grain boundary migration process. Therefore, curved grain boundaries are formed inside the test sample, such as... Figure 2 As indicated by the arrow; like Figure 3 As shown, further microscopic observation reveals that many secondary carbides precipitate on the grain boundaries. These secondary carbides interact with the grain boundaries, further promoting grain boundary bending.
[0028] In this embodiment, a strip-shaped sample with bent grain boundaries was processed into a long-term sample (working section diameter 5 mm, working section length 25 mm), and a high-temperature long-term test was conducted at 900℃ and 314 MPa. The test result showed that the long-term life of the nickel-based cast equiaxed superalloy with bent grain boundaries obtained in this embodiment was 75 h.
[0029] Example 2
[0030] The only difference between this embodiment and Embodiment 1 is that: The first temperature is 1200℃; The second preset duration is 50 hours.
[0031] After heat treatment using the heat treatment process described in this embodiment, more coarse γ' phase, γ / γ' eutectic phase, and initial MC carbides exist near the grain boundaries, causing the formation of curved grain boundaries inside the test sample. At the same time, the secondary carbides on the grain boundaries interact with the grain boundaries, further promoting the bending of the grain boundaries.
[0032] In this embodiment, a strip-shaped sample with bent grain boundaries was processed into a creep test sample (working section diameter 5 mm, working section length 25 mm), and a high-temperature creep test was conducted at 900℃ and 314 MPa. The test result showed that the creep life of the nickel-based cast equiaxed superalloy with bent grain boundaries obtained in this embodiment was 69.4 h.
[0033] Comparative Example 1
[0034] This comparative example provides a conventional heat treatment process for nickel-based cast equiaxed superalloys, the conventional heat treatment process including the following steps: Nickel-based cast equiaxed superalloys were subjected to heat treatment at 1230℃ / 2h / AC+1120℃ / 4h / AC+850℃ / 24h / AC (AC being air-cooled) to obtain blocky samples with straight grain boundaries and strip-shaped samples with straight grain boundaries, respectively. The nickel-based cast equiaxed superalloy used in this comparative example is the same as that used in Example 1.
[0035] This comparative example demonstrates the metallographic preparation process performed on a blocky sample with straight grain boundaries to obtain the alloy sample to be tested. The microstructure of the alloy sample in the heat-treated state was observed using a scanning electron microscope, and the results are as follows: Figure 1 As shown, after conventional heat treatment in this comparative example, lamellar precipitates formed at the grain boundaries and were embedded in the grain boundaries, while the interior of the sample was dominated by straight grain boundaries.
[0036] In this comparative example, a strip-shaped specimen with straight grain boundaries was processed into two long-term specimens with the same working section size (working section diameter 5 mm, working section length 25 mm). Both specimens were subjected to high-temperature long-term tests at 900℃ and 314 MPa. The test results showed that the long-term life of the two long-term specimens with the same working section size was 57 h and 61 h, respectively.
[0037] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A bend grain boundary heat treatment process for obtaining a nickel-based cast equiaxed high temperature alloy, characterized in that, The heat treatment process includes the following steps: S1: Heat the nickel-based cast equiaxed superalloy to a first temperature below its solution temperature, hold it at that temperature for a first preset time, and then cool it to room temperature to achieve subsolution treatment and obtain the alloy after subsolution treatment. S2: The alloy after subsolution treatment is kept at the temperature range in which the γ′ phase and secondary carbides precipitate for a second preset time, and then cooled to room temperature to achieve intermediate temperature holding treatment, thereby obtaining a nickel-based cast equiaxed high-temperature alloy with bent grain boundaries.
2. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a nickel-base cast single crystal high-temperature alloy. In step S1: The first temperature is a temperature 5-30°C lower than the solution temperature of the nickel-based cast equiaxed superalloy. The first preset duration is 1 to 5 hours.
3. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. In step S1: the cooling method is air cooling or furnace cooling; the cooling rate of furnace cooling is 2~20℃ / min.
4. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. In step S2: the second preset duration is 5~200h.
5. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. In step S2, the cooling method is air cooling.
6. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. In steps S1 and S2: the room temperature is 15-35℃.
7. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. Based on the total weight of the nickel-based cast equiaxed superalloy, the nickel-based cast equiaxed superalloy comprises: Cr: 10.0~13.0%, Co: 8.0~11.0%, Mo: 1.0~2.5%, W: 3.0~5.0%, Ta: 3.0~6.0%, Al: 3.0~6.0%, Ti: 3.0~4.0%, C: 0~0.2%, B: 0~0.05%.
8. The process of claim 1, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1484 alloy. The nickel-based cast equiaxed superalloy is cast nickel-based superalloy K466.
9. The process of claim 8, wherein the nickel-base cast equiaxed high-temperature alloy is a PWA1480 alloy. The creep rupture life of nickel-based cast equiaxed superalloys with bent grain boundaries is ≥69h under conditions of 900℃ and 314MPa.
10. A nickel-based cast equiaxed superalloy with bent grain boundaries obtained by the heat treatment process according to any one of claims 1-9.