A method for controlling the layer of hot dip tinning of superconducting fine diameter copper bus sectional annealing
By using segmented annealing and hot-dip tin plating processes, combined with the thickness characterization values of the copper-tin alloy transition layer and the free tin layer, the problem of uneven copper busbar plating was solved, achieving stability of the copper-tin interface reaction and uniformity of the plating, thus meeting the low-temperature conductivity and connection requirements of superconducting equipment.
Patent Information
- Application Number
- CN202611261815.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-24
AI Technical Summary
The existing annealing and hot-dip tin-plating processes for fine-diameter copper busbars used in superconducting applications do not fully consider cumulative work hardening and local deformation, resulting in unstable copper-tin interface reactions, uneven plating thickness, and a tendency to crack, peel, and increase resistance. This makes it difficult to meet the requirements for structural stability and conductivity of superconducting equipment.
By employing segmented annealing, graded cooling, drying, and hot-dip tin plating processes, combined with the thickness characterization values of the copper-tin alloy transition layer and the free tin layer, and utilizing annular airflow to adjust the circumferential uniformity of the tin plating layer, a suitable copper substrate structure and plating layer structure are formed.
It achieves stability of the copper-tin interface reaction and uniformity of the coating thickness, reduces interface stress during low-temperature cycling, reduces tin layer cracking and resistance increase, and meets the low-temperature conductivity and connection requirements of superconducting equipment.
Smart Images

Figure CN123152976A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of tin plating technology for thin-diameter copper busbars used in superconducting applications, and in particular to a method for controlling the layer of hot-dip tin plating in segmented annealing for thin-diameter copper busbars used in superconducting applications. Background Technology
[0002] Fine-diameter copper busbars used in superconducting cables, superconducting magnet leads, and cryogenic conductive connectors are typically made from larger-diameter copper wire through multiple fine drawing and micro-drawing processes, followed by continuous annealing and hot-dip tin plating. Current processes often set annealing conditions based on the finished wire diameter, experienced furnace temperature, and operating speed, without fully considering the cumulative work hardening and localized deformation concentration caused by different drawing passes, cross-sectional compression ratios, and drawing tensions. This easily leads to problems such as insufficient annealing, excessive recrystallization in certain areas, grain coarsening, or hot-dip tin plating. Furthermore, annealing, water cooling, drying, and hot-dip tin plating are usually controlled separately, resulting in a lack of coordination in the continuous thermal process of the copper wire from the annealing exit to the solidification of the tin layer, leading to unstable copper-tin interface reactions. Current tin plating controls are often based on the outer diameter or total plating thickness after tin plating, removing excess molten tin by using fixed molds or uniform airflow, without distinguishing between the copper-tin alloy transition layer that affects interfacial bonding and cryogenic brittleness, and the free tin layer that affects welding wetting and oxidation resistance. Therefore, even if the total coating thickness is qualified, there may still be problems such as excessively thick alloy layer, thin free tin layer, uneven circumferential coating, and cracking, peeling or increased resistance after low temperature cycling, which makes it difficult to meet the comprehensive requirements of superconducting equipment for the structural stability, conductivity and low temperature reliability of fine-diameter copper conductors. Summary of the Invention
[0003] This application provides a method for segmented annealing and hot-dip tin plating control layering of a thin-diameter copper busbar for superconducting applications, to solve the above-mentioned problems. The method includes: S1. The copper base material is subjected to fine drawing and micro-fine drawing in sequence to obtain a hardened fine-diameter copper busbar, and the cumulative deformation state is determined according to the cross-sectional area change of the copper base material and the hardened fine-diameter copper busbar and the deformation distribution of each drawing pass. S2. According to the cumulative deformation state, the hard-state thin-diameter copper busbar is subjected to segmented annealing by passing through the recovery section, the partial recrystallization section and the structure stabilization section in sequence, so as to reduce the residual stress after drawing, form a partial recrystallization structure and inhibit the continued growth of grains. S3. After annealing, the fine-diameter copper busbar is subjected to graded cooling, anti-oxidation treatment and drying treatment in sequence, and adjusted to the preset tin-entry temperature and flux is applied. S4. The thin-diameter copper busbar after applying flux is sent into the tin liquid for hot-dip tin plating. Based on the temperature-time history of the thin-diameter copper busbar from the annealing outlet to the tin removal and cooling stage, the thickness characterization value of the copper-tin alloy transition layer is determined, and at least one of the tin liquid temperature, tin immersion time and tin removal cooling intensity is adjusted according to the thickness characterization value. S5. Obtain the diameter of the copper wire before hot-dip tin plating and the outer diameter of the tin-plated wire after the tin layer solidifies, determine the total tin plating thickness, and determine the free tin layer thickness characterization value based on the total tin plating thickness and the copper-tin alloy transition layer thickness characterization value. S6. Adjust the annular airflow parameters at the tin melt outlet according to the free tin layer thickness characterization value, and adjust the airflow in the corresponding direction according to the circumferential thickness deviation of the tin plating line to control the free tin layer thickness and circumferential uniformity, and then perform take-up and winding.
[0004] Optionally, the cumulative deformation state includes cumulative true strain and deformation distribution across drawing passes, wherein the cumulative true strain is determined according to the following formula: ; In the formula, To accumulate true strain, and These are the cross-sectional areas of the copper base material and the hardened, thin-diameter copper busbar, respectively. and The diameters are those of the copper base material and the hardened fine-diameter copper busbar, respectively; the deformation distribution of each drawing pass is determined based on the cross-sectional compression ratio and drawing tension of each drawing pass.
[0005] Optionally, the heating temperature of the recovery section is 180–320°C, and the residence time is 0.3–3.0 s; The heating temperature of the recrystallization section is 300–500°C, and the residence time is 0.2–2.0 s; The heating temperature of the tissue stabilization section is 220–380°C, and the residence time is 0.2–2.0 s, and the heating temperature of the tissue stabilization section is lower than the heating temperature of the partial recrystallization section.
[0006] Optionally, the initial heating temperature and dwell time of each annealing section are determined based on the correspondence between the accumulated true strain and the pre-calibrated annealing parameters; The preset upper limit is determined by a drawing test of copper wire of the same material; when the maximum cross-sectional compression ratio or drawing tension in the drawing pass exceeds the corresponding preset upper limit, the dwell time of the recovery section is extended first, and then the heating temperature of the partial recrystallization section is adjusted so that the fine-diameter copper busbar forms a partially recrystallized structure in which the drawn fiber structure and the recrystallized structure coexist.
[0007] Optionally, the conveying path of the fine-diameter copper busbar can be divided into a tension zone before annealing, a tension zone after annealing, a tension zone after cooling and drying, a tension zone after tinning, and a tension zone after take-up. The corresponding tensile stress is determined based on the traction force of each tension zone and the diameter of the thin-diameter copper busbar. The tensile stress of the annealing tension zone is controlled to be 5% to 35% of the yield strength corresponding to the copper busbar temperature, and the traction force of the tin-immersion tension zone is lower than that of the tension zone before annealing.
[0008] Optionally, the graded cooling and anti-oxidation treatment includes a first cooling stage and a second anti-oxidation treatment stage; In the first cooling stage, the annealed fine-diameter copper busbar is cooled to 60-160°C to stop its continued recrystallization; In the second antioxidant treatment stage, the thin-diameter copper busbar is passed through an antioxidant solution with a mass percentage concentration of 0.05% to 2.0%. After drying, the temperature of the thin-diameter copper busbar before applying flux is adjusted to 30-100℃.
[0009] Optionally, the thickness characterization value of the copper-tin alloy transition layer is determined according to the following formula: ; In the formula, This represents the thickness of the copper-tin alloy transition layer. These are calibration constants obtained through copper-tin interface reaction experiments. R is the apparent activation energy of the copper-tin interface reaction, and R is the molar gas constant. and The first Absolute temperature and duration of the copper-tin interface within the specified temperature range. This refers to the number of temperature ranges where the copper-tin interface temperature is higher than the preset reaction termination temperature.
[0010] Optionally, the thickness characterization value of the free tin layer is determined according to the following formula: ; In the formula, This represents the thickness of the free tin layer. The diameter of the copper wire before hot-dip tin plating. This refers to the outer diameter of the tin-plated wire after the tin layer has solidified. The thickness of the copper-tin alloy transition layer is 0.1–2.0 μm, and the thickness of the free tin layer is 0.5–8.0 μm.
[0011] Optionally, the annular airflow is formed by at least four independent airflow channels arranged circumferentially along the tin-plated line, and the circumferential thickness difference of the tin-plated line is obtained by combining at least two intersecting diameter measurement directions with circumferential sampling detection. When the tin layer thickness corresponding to any measuring direction exceeds the preset thickness limit, the airflow pressure of the airflow channel corresponding to the direction with the larger thickness is increased, or the airflow pressure of the airflow channel opposite to that direction is decreased.
[0012] Optionally, the tin-plated small-diameter copper busbar after the control layer is subjected to cyclic testing between room temperature and a preset low temperature: When the rate of change of resistance after the cycle exceeds the preset limit and the elongation of the thin-diameter copper busbar is lower than the preset elongation, the heating temperature of part of the recrystallization section is increased or its residence time is extended. When the number of cracks in the tin layer after the cycle exceeds the preset crack limit and the thickness characterization value of the copper-tin alloy transition layer is higher than the preset upper limit, the tin liquid temperature is reduced, the immersion time is shortened, or the tin removal cooling intensity is increased. When the number of cracks in the tin layer after the cycle exceeds the preset crack limit and the thickness characterization value of the copper-tin alloy transition layer is lower than the preset lower limit, the tin liquid temperature is increased, the immersion time is extended, or the tin removal cooling intensity is reduced.
[0013] Through the above technical solution, this application achieves the following beneficial effects: The cumulative deformation state is determined by the changes in cross-sectional area of the copper base material and the finished copper wire, as well as the deformation distribution of each drawing pass. This allows for the concentrated adjustment of annealing parameters to address overall work hardening and localized deformation, avoiding the need to set fixed annealing conditions solely based on the final wire diameter.
[0014] By performing residual stress reduction, controlled recrystallization, and grain stabilization in the recovery section, partial recrystallization section, and microstructure stabilization section respectively, a copper matrix in which recrystallized microstructure and drawn fiber microstructure coexist can be formed, reducing insufficient annealing, abnormal coarse grains, and excessive softening.
[0015] By combining zoned tension control, the annealed and softened fine-diameter copper busbars are kept in a controlled tensile stress state, reducing wire diameter reduction, tension fluctuations, and wire breakage during continuous tin plating and winding processes.
[0016] By creating a continuous temperature-time process involving segmented annealing, graded cooling, drying, tin immersion, and tin removal cooling, the temperature of the molten tin, the immersion time, and the cooling intensity can be adjusted accordingly to prevent the copper-tin alloy transition layer from being too thick or too thin.
[0017] The total tin plating thickness is determined based on the wire diameter before and after tin plating, and the thickness of the free tin layer is obtained by combining the thickness characterization value of the copper-tin alloy transition layer. The alloy transition layer and the free tin layer are adjusted by the tin immersion heat process and the annular airflow, respectively, to avoid the imbalance of the plating structure caused by only controlling the total outer diameter.
[0018] By using circumferential independent airflow channels to directionally adjust the tin layer thickness direction, tin layer eccentricity, tin beads, local copper exposure, and thickness fluctuations can be reduced, while maintaining a stable average plating thickness.
[0019] By rationally controlling the microstructure of the copper matrix and the thickness distribution of the alloy transition layer and free tin layer, the interfacial stress caused by thermal shrinkage differences during room temperature to low temperature cycling can be reduced, thereby reducing tin layer cracking, peeling and resistance increase, and meeting the low temperature conductivity and connection requirements of superconducting equipment. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 A flowchart illustrating a method for segmented annealing and hot-dip tin plating of a fine-diameter copper busbar for superconducting applications, provided in an embodiment of this application. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0023] Furthermore, the term "and / or" in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character " / " in this article, unless otherwise specified, generally indicates that the preceding and following related objects have an "or" relationship.
[0024] The embodiments of this application will now be described in further detail with reference to the accompanying drawings.
[0025] Example 1 This embodiment provides a method for segmented annealing and hot-dip tin plating of a fine-diameter copper busbar for superconducting applications. Using oxygen-free copper wire with a diameter of 1.02 mm as the copper base material, a tin-plated fine-diameter copper busbar with a diameter of 0.12 mm is prepared. The method specifically includes the following steps.
[0026] S1, Fine elongation and micro-elongation of copper base material Oxygen-free copper wire with a purity of not less than 99.95% and an initial diameter of 1.02 mm was selected as the copper base material. First, the copper base material was finely drawn by passing it through multiple drawing dies to draw it into a semi-finished copper wire with a diameter of 0.254 mm. Then, the semi-finished copper wire was micro-finely drawn to obtain a hardened fine-diameter copper busbar with a diameter of 0.12 mm.
[0027] The main drawing wire diameters used in this embodiment are as follows: 1.02mm, 0.91mm, 0.81mm, 0.72mm, 0.64mm, 0.57mm, 0.51mm, 0.455mm, 0.405mm, 0.361mm, 0.322mm , 0.287mm, 0.268mm, 0.254mm, 0.227mm, 0.203mm, 0.181mm, 0.162mm, 0.145mm, 0.130mm, 0.120mm.
[0028] The cross-sectional compression rate of each drawing pass was controlled between 10% and 22%, with a maximum cross-sectional compression rate of 20.7%. No abnormal concentration of cross-sectional compression rate was observed in any of the passes. The drawing speed during the fine stretching stage was 15–25 m / min, and the drawing speed during the micro-fine stretching stage was 30–45 m / min.
[0029] Based on the initial diameter of the copper base material and the final diameter of the hardened, thin-diameter copper busbar, the cumulative true strain is determined according to the following formula:
[0030] In the formula, The initial diameter of the copper base material. This refers to the final diameter of the hardened, narrow-diameter copper busbar.
[0031] Will , Substituting the values, the cumulative true strain of this batch of copper wires is 4.28. Combining the cross-sectional compression ratio and drawing tension of each drawing pass, this batch of hard-state small-diameter copper busbars is determined to be in a state of high cumulative deformation and no local deformation concentration.
[0032] The surface of the hardened, small-diameter copper busbar after micro-stretching showed no obvious scratches, folds, or oxide spots, and its measured average diameter was 0.1202 mm.
[0033] S2, Segmented Annealing The hardened, small-diameter copper busbar is continuously fed into a segmented annealing furnace with independent temperature control at a running speed of 40 m / min. The annealing furnace is sequentially set up with a recovery section, a partial recrystallization section, and a microstructure stabilization section along the running direction of the copper busbar. Nitrogen gas is introduced into the furnace to reduce surface oxidation of the copper busbar during the annealing process.
[0034] The process conditions for each annealing stage are shown in the table below.
[0035] Table 1 Process conditions for each annealing stage in Example 1
[0036] The recovery section is used to reduce the axial residual stress and dislocation entanglement formed by micro-drawing; the partial recrystallization section is used to enable controlled recrystallization of the copper busbar, forming a structure in which recrystallized grains and drawn fiber structures coexist; and the structure stabilization section is used to homogenize the radial temperature of the copper busbar and inhibit the continued growth of recrystallized grains.
[0037] A non-contact temperature detection unit is installed inside the annealing furnace to detect the surface temperature of the copper busbar at the exit of each annealing section. When the difference between the measured temperature and the target temperature of any annealing section exceeds 5°C, the heating power of the corresponding annealing section is adjusted.
[0038] To prevent secondary stretching of the copper busbar under high-temperature softening conditions, the conveying path is divided into a pre-annealing tension zone, an annealing tension zone, a cooling and drying tension zone, a tinning tension zone, and a take-up tension zone. The stable traction force in each zone is controlled at 0.35N, 0.06N, 0.10N, 0.08N, and 0.18N, respectively.
[0039] The tensile stress corresponding to the traction force in the annealing tension zone is approximately 5.3 MPa, which is 25% lower than the yield strength of the copper busbar at that temperature, thus preventing irreversible axial elongation of the copper busbar after annealing.
[0040] After annealing, the cross-sectional microstructure of the copper busbar was examined. The recrystallization area ratio was 61.8%, the average grain size was 8.4 μm, and no continuous coarse grain bands were observed, indicating that a partial recrystallization state was formed in which recrystallized structure and drawn fiber structure coexisted.
[0041] S3, staged cooling and antioxidant treatment After leaving the stable phase, the copper busbar first enters the first cooling zone. The first cooling zone uses a circumferential atomizing spray to rapidly cool the copper busbar, reducing its surface temperature from approximately 286°C at the annealing furnace exit to 103°C, thus stopping further recrystallization of the copper busbar.
[0042] The cooling medium in the first cooling zone is deionized water, and the spraying time is 0.35 seconds. The spray direction is evenly distributed around the circumference of the copper busbar to avoid lateral vibration of the thin-diameter copper busbar caused by unilateral impact.
[0043] Subsequently, the copper busbar enters the second anti-oxidation zone. This zone contains a water-soluble copper antioxidant with a mass percentage concentration of 0.30%, the antioxidant solution temperature is 45°C, and the copper busbar remains in the antioxidant solution for 0.40 seconds.
[0044] After leaving the second anti-oxidation zone, the copper busbar is subjected to an annular gas-liquid scraping device to remove large droplets from its surface, leaving a uniform thin liquid film on its surface. The scraping gas pressure is 3.0 kPa, and the scraping gas flow is uniformly distributed along the circumference of the copper busbar.
[0045] S4, Drying and Flux Treatment The copper busbars after anti-oxidation treatment are sent into a dual-temperature zone oven. The front of the oven is a drying zone, set at 130℃, used to remove moisture and volatile components from the surface of the copper busbars; the rear of the oven is a temperature homogenization zone, set at 70℃, used to regulate the temperature of the copper busbars before they enter the soldering station.
[0046] The total residence time of the copper busbar in the oven was 1.2 s, of which 0.7 s was spent in the drying zone and 0.5 s in the temperature homogenization zone. The measured surface temperature of the copper busbar at the oven outlet was 62 ℃.
[0047] Subsequently, a low-residue halogen-free flux was applied to the surface of the copper busbar using a dip-coating method. The effective solid content of the flux was 6.0%, and the dip-coating time was 0.20 s. After the copper busbar left the flux bath, excess flux was removed through a flexible scraper hole, allowing the flux to form a continuous and uniform thin layer on the surface of the copper busbar.
[0048] S5. Pre-calibration of copper-tin interface reaction parameters Before continuous hot-dip tin plating, a copper-tin interface reaction calibration test was conducted using a copper busbar of the same material and diameter as in this embodiment.
[0049] The copper busbar was immersed in high-purity tin at 245℃, 260℃, and 275℃, respectively, with immersion times of 0.3s, 0.6s, and 0.9s at each tin temperature. Cross-sectional samples of the obtained tin-plated copper busbars were prepared, and the thickness of the copper-tin alloy transition layer was measured using a scanning electron microscope.
[0050] Based on the temperature, immersion time, and measured alloy transition layer thickness for each group, the following formula is fitted:
[0051] In the formula, This represents the thickness of the copper-tin alloy transition layer. For calibration constants, R is the apparent activation energy of the copper-tin interface reaction, and R is the molar gas constant. For the first Absolute temperature of the copper-tin interface within the temperature range. This represents the duration of the corresponding temperature range.
[0052] Under the material and detection conditions of this embodiment, the fitting was obtained. It is 45.2 kJ / mol. for The model has a thickness of μm² / s and a coefficient of determination of 0.972. The average relative deviation between the model-calculated values and the measured values of the cross-section is 6.3%. Therefore, the model is used to characterize the thickness of the alloy transition layer in continuous production processes.
[0053] S6, Hot-dip tin plating and alloy transition layer control The copper busbar, after fluxing, is continuously fed into the tin furnace. The tin furnace uses high-purity tin with a purity of 99.95%, and the molten tin temperature is set to 260℃.
[0054] The effective operating path length of the copper busbar in the molten tin is 0.40m, and the production line speed is 40m / min, therefore the effective immersion time is 0.60s. The surface temperature of the copper busbar when it enters the molten tin is 60-64℃.
[0055] After leaving the molten tin, the copper busbar first passes through an 80mm long natural leveling zone before entering the annular airflow tin control assembly. Based on the temperature-time data of the copper busbar from the annealing outlet, staged cooling, drying, tin entry, tin immersion to the initial cooling stage after tin exit, the thickness of the copper-tin alloy transition layer is calculated to be 0.72μm, which is within the target range of 0.5 to 0.9μm set in this embodiment.
[0056] Therefore, the molten tin temperature, immersion path, and initial cooling parameters after tin removal were kept constant during this production process.
[0057] S7. Determination of total tin plating thickness and free tin layer thickness A first biaxial laser diameter measurement unit is set before the copper busbar enters the tin furnace, and a second biaxial laser diameter measurement unit is set after the tin layer solidifies.
[0058] The first biaxial laser diameter measurement unit detected the average diameter of the copper busbar before hot-dip tin plating. The average outer diameter of the tin-plated wire was 0.1202 mm, as measured by the second dual-axis laser diameter measuring unit. It is 0.1270mm.
[0059] The thickness of the free tin layer is determined according to the following formula:
[0060] The total tin plating thickness was calculated to be 3.40 μm, and the free tin layer thickness was 2.68 μm, which is within the target range of 2.0 to 4.0 μm.
[0061] S8, Annular airflow control layer and circumferential uniformity adjustment The annular airflow tin control assembly is located above the molten tin outlet and includes first to fourth airflow channels spaced 90° apart circumferentially along the copper busbar. Each airflow channel is connected to an independent pressure regulating valve. The distance from the nozzle to the surface of the copper busbar is 8 mm, and the airflow direction is inclined upward at 15° relative to the radial direction of the copper busbar.
[0062] In the initial stage of stable production, the airflow pressure of all four airflow channels was set to 8.0 kPa. Biaxial diameter measurement and circumferential sampling tests showed that the tin layer thickness on one side of the copper busbar in the first direction was 3.84 μm, and on the opposite side it was 3.12 μm; the tin layer thicknesses on both sides in the second direction were 3.46 μm and 3.31 μm, respectively, with a maximum circumferential thickness difference of 0.72 μm.
[0063] Based on the direction of tin layer thickness, the pressure of the corresponding first airflow channel is increased from 8.0 kPa to 9.4 kPa, and the pressure of the third airflow channel in the opposite direction is decreased from 8.0 kPa to 7.6 kPa; the pressure of the second and fourth airflow channels is maintained at 8.0 kPa.
[0064] After running continuously for 30 seconds, the tin layer thicknesses in the four circumferential directions were measured again. The thicknesses were 3.50 μm, 3.38 μm, 3.29 μm and 3.42 μm, respectively. The maximum thickness difference in the circumferential direction decreased to 0.21 μm. The average total tin plating thickness remained at 3.40 μm, and the average thickness of the free tin layer remained at 2.68 μm.
[0065] This demonstrates that by adjusting the airflow pressure in different circumferential directions, the circumferential uniformity of the free tin layer can be improved without significantly altering the average total tin plating thickness.
[0066] S9, take-up and take-up After the tin plating is controlled, the thin-diameter copper busbar enters the extraction device via a guide wheel. A solidification section with a length of 0.50m is set between the annular airflow tin control assembly and the first guide wheel, so that the tin layer solidifies before contacting the guide wheel.
[0067] The diameter of the first guide wheel is 20mm, and the copper busbar is not bent to a small radius before the tin layer is completely solidified. A tension swing arm is installed between the take-up device and the winding device to isolate the effect of changes in the reel diameter on the tension at the tin furnace outlet.
[0068] The winding device adjusts its rotation speed according to the real-time diameter of the reel, maintaining a winding speed of 40 m / min and a take-up tension of 0.18 N. No obvious solder balls, exposed copper, sudden changes in wire diameter, or wire breakage were observed during continuous production.
[0069] S10, Finished Product Inspection Five groups of samples were randomly selected from the tin-plated thin-diameter copper busbars obtained in this embodiment for testing. The average value of the test results is as follows: Table 2. Finished Product Testing Results of Example 1
[0070] The average thickness of the copper-tin alloy transition layer obtained by the actual cross-section measurement was 0.74 μm, which differed by 2.7% from the thickness characterization value of 0.72 μm obtained by the model.
[0071] After the sample was subjected to 20 low-temperature cycles between room temperature and 77K, the average resistance change rate of the sample was 0.42%, and no continuous interface peeling was found; the number of local microcracks observed under the microscope did not exceed 1 crack / cm, and the microcracks did not penetrate the free tin layer and the copper-tin alloy transition layer.
[0072] The above results show that, in this embodiment, segmented annealing driven by cumulative deformation state enables the small-diameter copper busbar to obtain suitable strength and elongation; the copper-tin alloy transition layer is controlled by continuous temperature-time history, and the thickness of the free tin layer is determined according to the characteristic values of the wire diameter and alloy transition layer thickness before and after tin plating. Then, the circumferential distribution of the free tin layer is adjusted by using annular partitioned airflow, thereby obtaining a tin-plated small-diameter copper busbar with stable plating thickness, uniform circumferential distribution, and suitable for low-temperature cycling.
[0073] Example 2 This embodiment provides a method for controlling the tin plating layer in segmented annealing of fine-diameter copper busbars for superconducting applications with concentrated deformation during drawing passes. This embodiment uses the same initial diameter of the copper base material and the diameter of the finished copper substrate as in Embodiment 1, but changes the deformation distribution during the micro-drawing stage to illustrate the specific process of adjusting the segmented annealing parameters based on the cumulative deformation state.
[0074] Except for the drawing passes and annealing parameters that are explicitly adjusted in this embodiment, the graded cooling, anti-oxidation, drying, fluxing, hot-dip tin plating, annular airflow control layer, take-up and winding methods are the same as in Embodiment 1.
[0075] S1, Fine elongation and micro-elongation of copper base material Oxygen-free copper wire with a purity of not less than 99.95% and an initial diameter of 1.02 mm was selected as the copper base material. First, it was processed into a semi-finished copper wire with a diameter of 0.254 mm through multiple fine drawing processes. Then, the semi-finished copper wire was further processed into a hardened fine-diameter copper busbar with a diameter of 0.12 mm.
[0076] In this embodiment, the same drawing path as in Embodiment 1 is used during the fine drawing stage; the wire diameters during the micro-fine drawing stage are as follows: 0.254mm, 0.227mm, 0.203mm, 0.181mm, 0.165mm, 0.150mm, 0.129mm and 0.120mm.
[0077] Among them, the cross-sectional compression ratio of the 0.150mm to 0.129mm drawing passes was 26.0%, which was significantly higher than that of the other micro-drawing passes. The measured drawing tension of this pass was 1.48N, and the average drawing tension of the adjacent micro-drawing passes was 1.08N. The ratio of the drawing tension of this pass to the average drawing tension of the adjacent passes was 1.37.
[0078] In this embodiment, based on a pull-out test of copper wire of the same material, the pull-out state that meets any of the following conditions is determined to be a state of localized deformation concentration: (1) The cross-sectional compression ratio of any drawing pass is greater than 23%; (2) The ratio of the pulling tension of any pulling pass to the average pulling tension of the three adjacent pulling passes is greater than 1.25. Therefore, it is determined that the hard-state thin-diameter copper busbar in this embodiment belongs to a state of high cumulative deformation and localized deformation concentration.
[0079] Based on the initial diameter of the copper base material and the final diameter of the hardened, thin-diameter copper busbar, the cumulative true strain of this batch of copper wires is also 4.28. The average diameter of the copper busbar after micro-elongation is 0.1201 mm, the hardened tensile strength is 472 MPa, and the elongation is 2.3%.
[0080] S2. Determine the segmented annealing parameters based on the deformation concentration state. Since this embodiment has the same initial diameter, final diameter and cumulative true strain as Embodiment 1, the overall work hardening degree of the two is similar; however, this embodiment has a single-pass cross-sectional compression ratio and concentrated drawing tension, and the local dislocation density and axial residual stress inside the copper wire are relatively high.
[0081] To avoid causing localized abnormal coarse crystals by directly increasing the temperature of part of the recrystallization section, this embodiment adopts an adjustment method of "prioritizing the increase of heat input in the recovery section and limiting the maximum temperature of part of the recrystallization section".
[0082] Compared to Example 1, the dwell time in the recovery section was extended by 0.3 s, the temperature in part of the recrystallization section was reduced by 5 °C, and the dwell time in the tissue stabilization section was extended by 0.1 s. The adjusted parameters are shown in the table below.
[0083] Table 3 Process conditions for each annealing stage in Example 2
[0084] The production line speed is maintained at 40m / min.
[0085] The increased dwell time in the recovery section is used to preferentially reduce residual stress and dislocation entanglement caused by localized concentrated drawing; the temperature in the partial recrystallization section is slightly lower than that in Example 1 to limit rapid grain growth in local high-energy storage regions; the increased dwell time in the microstructure stabilization section is used to reduce the radial and axial microstructure differences of the copper wire.
[0086] Nitrogen gas continues to flow into the annealing furnace, and non-contact temperature detection units are installed at the outlet of each annealing section. When the measured temperature of each section deviates from the set temperature by more than 5°C, the heating power of the corresponding section is adjusted.
[0087] S3, Zoned Tension Control In this embodiment, tension zones are set up along the copper busbar conveying direction, including a pre-annealing tension zone, an annealing tension zone, a cooling and drying tension zone, a tinning tension zone, and a take-up tension zone.
[0088] Considering that the copper wire in this embodiment has high axial residual stress after localized concentrated drawing and that the dwell time in the recovery section is extended, the traction force in the annealing tension zone is reduced from 0.06N in Example 1 to 0.05N to reduce secondary stretching of the copper wire during the recovery softening stage.
[0089] The stable traction force in each zone is as follows: Table 4 Stable traction force in each zone of Example 2
[0090] The tensile stress of the copper wire in the annealing tension zone is approximately 4.4 MPa, which is 25% lower than the yield strength of the copper wire at this temperature. During continuous operation, the average diameter change of the copper wire before and after annealing is less than 0.0003 mm, and no detectable hot thinning phenomenon occurred.
[0091] S4. Microstructure and property testing after annealing Samples were taken from the segmented annealed copper busbar, and the cross-sectional microstructure of the copper wire was observed using electron backscatter diffraction and metallographic microscopy.
[0092] The test results show that: (1) The recrystallization area ratio is 58.9%; (2) The average grain size is 7.9 μm; (3) The copper wire retains some of the fibrous structure that extends along the drawing direction; (4) No continuous coarse grain zone caused by concentrated drawing passes from 0.150 mm to 0.129 mm was observed; (5) The axial residual stress value decreased from 171 MPa in the hard copper wire to 46 MPa.
[0093] The annealed copper wire exhibited a tensile strength of 257 MPa, an elongation of 17.4%, and an average diameter of 0.1200 mm. These results indicate that extending the recovery section without increasing the maximum temperature of the partial recrystallization section can reduce residual stress caused by localized deformation concentration, while simultaneously preventing excessive recrystallization in high-energy-storage regions.
[0094] S5, staged cooling, anti-oxidation and drying After annealing, the copper busbar first enters the first cooling zone, where a circumferential atomizing spray method is used to reduce the surface temperature of the copper busbar from about 284°C at the annealing furnace outlet to 101°C, in order to stop further recrystallization.
[0095] The first cooling zone uses deionized water, with a spraying time of 0.38 s. Subsequently, the copper busbar is immersed in a water-soluble copper antioxidant solution with a mass percentage concentration of 0.30%, the antioxidant solution temperature is 45℃, and the residence time is 0.40 s.
[0096] After the copper busbar leaves the antioxidant solution, it is subjected to an annular gas-liquid scraper to remove large droplets from its surface before being sent to a dual-temperature zone oven. The oven drying zone has a temperature of 130℃ and a dwell time of 0.7s; the temperature homogenization zone has a temperature of 70℃ and a dwell time of 0.5s.
[0097] The measured temperature of the copper busbar at the oven outlet was 61°C. Subsequently, a low-residue halogen-free flux was used for dip coating, the same as in Example 1, with an effective solid content of 6.0% and a dipping time of 0.20s.
[0098] S6, hot-dip tin plating and double-layer thickness control The copper busbar, after fluxing, is immersed in molten high-purity tin with a purity of 99.95%. The molten tin temperature is 260℃, the effective running path length of the copper busbar in the molten tin is 0.40m, the production line speed is 40m / min, and the effective immersion time is 0.60s.
[0099] Using the copper-tin interface reaction parameters calibrated in Example 1, and based on the temperature-time data of the copper busbar in this example from the annealing exit, staged cooling, drying, tin immersion to the initial cooling stage after tin removal, the thickness of the copper-tin alloy transition layer was calculated to be 0.70 μm.
[0100] The average diameter of the copper busbar was measured to be 0.1200 mm before the tin bath; the average outer diameter of the tin-plated wire was measured to be 0.1268 mm after the tin layer solidified. Therefore, the total tin plating thickness was 3.40 μm, and the free tin layer thickness was 2.70 μm.
[0101] The thickness characterization values of the copper-tin alloy transition layer and the free tin layer are both within the corresponding target range, so the tin liquid temperature, immersion time and average annular gas flow pressure are kept constant.
[0102] S7, Circumferential airflow adjustment This embodiment uses the same four-channel annular airflow control assembly as in Embodiment 1. During the initial production phase, the pressure in all four airflow channels was set to 8.0 kPa.
[0103] Initial testing revealed that the tin layer thicknesses in the four circumferential directions of the tin-plated line were 3.61 μm, 3.44 μm, 3.16 μm, and 3.39 μm, respectively, with a maximum circumferential thickness difference of 0.45 μm.
[0104] Based on the detection results of the thicker tin layer in the first direction, the pressure of the airflow channel corresponding to the first direction is increased from 8.0 kPa to 8.8 kPa, and the pressure of the airflow channel in the opposite direction is decreased from 8.0 kPa to 7.8 kPa.
[0105] After 30 seconds of continuous operation, the tin layer thicknesses in the four circumferential directions were 3.46 μm, 3.39 μm, 3.28 μm and 3.43 μm, respectively. The maximum circumferential thickness difference decreased to 0.18 μm, while the average total tin plating thickness remained at 3.40 μm.
[0106] S8. Extraction, winding, and finished product inspection After the control layer is applied, the tin-plated fine-diameter copper busbar enters the take-up device through a 0.50m long solidification section. The take-up speed is maintained at 40m / min, and the take-up tension is 0.18N. No wire breakage occurred during the continuous production of 1000m, and no obvious solder beads, exposed copper, or abrupt changes in wire diameter were observed.
[0107] Five samples were randomly selected from the obtained tin-plated thin-diameter copper busbars for testing, and the results are shown in the table below.
[0108] Table 5. Sample test results of Example 2
[0109] After the sample was subjected to 20 low-temperature cycles between room temperature and 77K, the average resistance change rate was 0.47%, no continuous peeling was observed at the copper-tin interface, and the number of local microcracks observed under microscopy did not exceed 1 crack / cm.
[0110] This embodiment demonstrates that, with the same initial diameter, final diameter, and cumulative true strain, the deformation distribution during each drawing pass still affects the residual stress and recrystallization behavior of the copper wire. For situations with concentrated local deformation, prioritizing increased heat input in the recovery section and limiting the maximum temperature in some recrystallization sections can reduce local residual stress, prevent abnormal coarse grains, and simultaneously maintain the tensile strength and elongation of the copper busbar to meet the requirements for subsequent hot-dip tinning and low-temperature use.
[0111] Example 3 This embodiment provides a method for controlling the tin plating layer of a thin-diameter copper busbar for superconducting applications by segmented annealing and hot-dip tin plating, based on the decoupling adjustment of the copper-tin alloy transition layer and the free tin layer. It illustrates that, under the condition that the total tin plating thickness is basically the same, the thickness distribution of the copper-tin alloy transition layer and the free tin layer can be changed by adjusting the tin plating thermal history and the annular airflow parameters respectively, and the subsequent production parameters can be corrected based on the low-temperature cycle test results.
[0112] In this embodiment, oxygen-free copper wire with a diameter of 1.02 mm is used as the copper base material, and it is processed to a diameter of 0.12 mm through fine drawing and micro-fine drawing. The drawing passes, segmented annealing, graded cooling, anti-oxidation treatment and flux treatment are the same as in Example 1. The main difference is that the hot-dip tinning and tin exit control parameters are adjusted.
[0113] S1. Preparation and segmented annealing of fine-diameter copper busbars Oxygen-free copper wire with a diameter of 1.02 mm and a purity of not less than 99.95% is processed to 0.254 mm through multiple fine drawing processes, and then further processed to 0.12 mm through micro-fine drawing processes to obtain a hard-state fine-diameter copper busbar.
[0114] The cumulative true strain of this batch of copper wire was 4.28, and the cross-sectional compression ratio of each drawing pass did not exceed 22%. No local deformation concentration was detected. Therefore, the same segmented annealing parameters as in Example 1 were used. Table 6 Process conditions for each annealing stage in Example 3
[0115] The production line speed is 40m / min, and the traction force in the annealing tension zone is 0.06N.
[0116] The recrystallization area of the annealed copper busbar is 60.7%, the average grain size is 8.2μm, the tensile strength is 250MPa, and the elongation is 18.1%, which meets the requirements for subsequent continuous hot-dip tin plating.
[0117] S2, graded cooling, drying and fluxing treatment After the copper busbar leaves the annealing furnace, it undergoes the first stage of cooling using a circumferential atomizing spray method, reducing its surface temperature to 105°C. Subsequently, the copper busbar is passed through a water-soluble copper antioxidant solution with a mass percentage concentration of 0.30% for a residence time of 0.40 seconds.
[0118] After oxidation treatment, the copper busbar is subjected to an annular gas-liquid scraping device to remove large droplets from its surface before entering a dual-temperature zone oven. The oven drying zone has a temperature of 130℃ and a dwell time of 0.7s, while the temperature homogenization zone has a temperature of 70℃ and a dwell time of 0.5s.
[0119] The surface temperature of the copper busbar when it leaves the oven is 63°C. It is then dip-coated with a low-residue halogen-free flux with an effective solid content of 6.0% for 0.20 seconds.
[0120] S3, Hot-dip tin plating in the first production stage In the first production stage, the fluxed copper busbar is fed into molten high-purity tin with a purity of 99.95%, using the following initial process parameters: Table 7 Initial process parameters for Example 3
[0121] After the tin layer solidifies, the first biaxial laser diameter measuring unit detects that the average diameter of the copper busbar before tin plating is 0.1201 mm, and the second biaxial laser diameter measuring unit detects that the average outer diameter of the tin-plated wire is 0.1269 mm. Thus, the total tin plating thickness is determined to be 3.40 μm.
[0122] Using the copper-tin interface reaction parameters calibrated in Example 1, and based on the temperature-time data of the copper busbar immersion temperature, tin liquid temperature, immersion time, and the initial cooling stage after tin removal, the thickness of the copper-tin alloy transition layer in the first production stage was calculated to be 1.16 μm.
[0123] The thickness of the free tin layer is 2.24 μm, obtained by subtracting the thickness of the copper-tin alloy transition layer from the total tin plating thickness.
[0124] Cross-sectional testing was performed on the samples from the first production stage, and the actual average thickness of the copper-tin alloy transition layer was measured to be 1.20 μm, with a relative deviation of 3.3% from the model characterization value.
[0125] Although the total tin plating thickness of the first production stage is within the target range of 2.0 to 6.0 μm, the thickness of its copper-tin alloy transition layer is higher than the target range of 0.5 to 0.9 μm set in this embodiment. This indicates that the qualified total tin plating thickness does not necessarily mean that the internal structure of the plating layer meets the requirements for low-temperature use.
[0126] S4, Low-temperature cycle testing in the first production section Five samples with a length of 300 mm were randomly cut from the tin-plated fine-diameter copper busbars obtained from the first production section and subjected to 30 low-temperature cycles between room temperature and 77 K.
[0127] Each loop includes: (1) Cool the sample from room temperature to 77K and hold for 10 min; (2) Allow the sample to return to room temperature and maintain this temperature for 15 minutes; (3) After checking the surface condition of the sample, proceed to the next cycle.
[0128] After 30 cycles, the sample was tested for resistance, cross-sectional area, and bending. The results are as follows: Table 8. Detection results of low-temperature cycling samples in Example 3
[0129] Cross-sectional observations revealed that some cracks originated in the thicker copper-tin alloy transition layer and extended outwards into the free tin layer. This indicates that the alloy transition layer in the first production stage was too thick, increasing the overall brittleness of the coating and making it prone to interfacial stress concentration when the copper substrate and tin layer experienced inconsistent low-temperature shrinkage.
[0130] S5. Correct the tin-immersion thermal process based on the low-temperature test results. To address the issue of an excessively thick copper-tin alloy transition layer in the first production stage, while maintaining the same copper material, annealing parameters, flux type, and target total tin plating thickness, the following adjustments will be made to the second production stage: (1) Reduce the temperature of the molten tin from 272℃ to 258℃; (2) The effective tin-dipping path length is shortened from 0.46m to 0.36m; (3) Maintain the production line speed at 40m / min to shorten the effective tin immersion time from 0.69s to 0.54s; (4) The length of the tin-out natural leveling section is shortened from 100mm to 70mm, so that the copper busbar can enter the initial cooling and airflow tin control area earlier; (5) Reduce the initial cooling airflow temperature after tinning from 35°C to 25°C; (6) Appropriately reduce the average pressure of the annular airflow to compensate for the reduced amount of free tin adhesion due to the decrease in tin liquid temperature and immersion time.
[0131] Of the above adjustments, the tin bath temperature, immersion time, and initial cooling after tin removal are mainly used to reduce the degree of reaction at the copper-tin interface; the annular airflow pressure is used to adjust the thickness of the free tin layer, and the two are applied to different plating structures respectively.
[0132] S6, Two-layer decoupling control of the second production section The second production stage proceeded with continuous production according to the revised parameters. The average diameter of the copper busbar before tin plating was 0.1201 mm.
[0133] In the initial stage of production, the pressure of all four channels of the annular airflow was set to 7.6 kPa, the average outer diameter of the tin-plating wire was 0.1273 mm, and the corresponding total tin plating thickness was 3.60 μm, which is higher than the set control range of 3.2 to 3.5 μm.
[0134] Based on continuous temperature-time data, the calculated thickness of the copper-tin alloy transition layer is 0.69 μm, which falls within the target range of 0.5–0.9 μm. Since the alloy transition layer thickness is normal but the total tin plating thickness is too large, the controller no longer adjusts the tin bath temperature and immersion time, but instead increases the average pressure of the four airflow channels from 7.6 kPa to 8.2 kPa.
[0135] After adjustment, the average outer diameter of the tin-plated wire stabilized at 0.1269 mm, the total tin plating thickness was 3.40 μm, and the free tin layer thickness was 2.71 μm.
[0136] This achieves the following: (1) First production stage: alloy transition layer 1.16μm, free tin layer 2.24μm; (2) Second production stage: alloy transition layer 0.69μm, free tin layer 2.71μm; (3) The total tin plating thickness of both production sections is about 3.40 μm.
[0137] This indicates that by adjusting the immersion tin heat process and the annular airflow, the thickness distribution of the alloy transition layer and the free tin layer can be changed while keeping the total tin plating thickness essentially constant.
[0138] S7, Circumferential thickness adjustment in the second production section After the second production section stabilized, the tin layer thickness in the four circumferential directions of the tin-plated wire was obtained through four-directional diameter measurement and cross-sectional sampling inspection as follows: The thicknesses are 3.62 μm, 3.42 μm, 3.19 μm and 3.37 μm, with a maximum circumferential thickness difference of 0.43 μm.
[0139] The tin layer thickness is greatest in the first direction. The pressure of the airflow channel corresponding to the first direction is increased from 8.2 kPa to 8.9 kPa, and the pressure of the airflow channel in the opposite direction is decreased from 8.2 kPa to 7.9 kPa, while the pressure in the other two directions remains at 8.2 kPa.
[0140] After 30 seconds of continuous operation, the tin layer thicknesses in the four circumferential directions were 3.46 μm, 3.39 μm, 3.31 μm and 3.43 μm, respectively. The maximum circumferential thickness difference decreased to 0.15 μm, while the average total tin plating thickness remained at 3.40 μm.
[0141] Therefore, circumferentially partitioned airflow can correct the circumferential distribution of the free tin layer without changing the thickness of the alloy transition layer.
[0142] S8, Cross-section and ambient temperature performance testing of the second production section Five sets of samples were randomly selected from the tin-plated small-diameter copper busbars obtained from the second production section. The test results are as follows: Table 9. Room temperature performance test of sample from Example 3
[0143] The relative deviation between the alloy transition layer model characterization value and the measured cross-sectional value is 2.8%, indicating that the thickness characterization value determined based on the continuous temperature-time history can be used for production process adjustment.
[0144] S9, Low-temperature cycle detection in the second production section Using the same method as the first production stage, the samples from the second production stage were cycled 30 times between room temperature and 77K. The test results are as follows: Table 10. Results of Low Temperature Cycling Test in Example 3
[0145] No continuous interface delamination was observed in the samples from the second production stage after low-temperature cycling; only short microcracks that did not penetrate the free tin layer appeared in a few locations. Compared with the first production stage, the resistivity change rate, the number of cracks, and the interface delamination area were all significantly reduced after low-temperature cycling.
[0146] S10, Feedback confirmation of production parameters Based on the test results of the second production stage, the preferred control conditions corresponding to the 0.12mm fine-diameter copper busbar used in this embodiment are determined as follows: (1) The thickness of the copper-tin alloy transition layer is controlled at 0.6–0.8 μm; (2) The thickness of the free tin layer is controlled between 2.5 and 3.0 μm; (3) The total tin plating thickness is controlled between 3.2 and 3.6 μm; (4) The temperature of the molten tin is controlled at 255-262℃; (5) The effective tin immersion time should be controlled within 0.50 to 0.58 seconds; (6) The average pressure of the annular airflow is controlled at 8.0 to 8.5 kPa, and the corresponding airflow channels are adjusted according to the circumferential thickness deviation.
[0147] The above parameters were used as the initial production parameters for the next coil of copper busbar of the same specification. During the continuous production of the next coil for 1000m, the cross-sectional thickness of the alloy transition layer was maintained at 0.67-0.75μm, the thickness of the free tin layer was maintained at 2.61-2.78μm, the maximum circumferential thickness difference did not exceed 0.22μm, and no wire breakage, continuous copper exposure or obvious tin beads occurred.
[0148] This embodiment demonstrates that simply controlling the total tin plating thickness cannot accurately reflect the low-temperature performance of the coating. Under the condition of essentially the same total tin plating thickness, reducing the thickness of the copper-tin alloy transition layer and correspondingly increasing the thickness of the free tin layer can reduce coating brittleness and interfacial stress during low-temperature cycling. By controlling the alloy transition layer through the immersion tin thermal process and controlling the free tin layer through annular airflow, decoupled adjustment of the two types of coatings can be achieved, and subsequent production parameters can be corrected based on the results of low-temperature cycling.
[0149] Comparative Example 1: Single-zone continuous annealing This comparative example illustrates that, under conditions of similar total annealing time, it is difficult to simultaneously achieve residual stress reduction, partial recrystallization, and grain stability control using single-temperature annealing.
[0150] Except for the annealing method, the copper base material, drawing route, graded cooling, anti-oxidation treatment, drying, fluxing, hot-dip tinning, annular airflow tin control, and take-up conditions used in this comparative example are all the same as in Example 1.
[0151] 1. Pulling treatment Oxygen-free copper wire with a purity of not less than 99.95% and an initial diameter of 1.02mm is selected, and it is processed to 0.254mm through multiple fine drawing processes, and then further processed to 0.12mm through micro-fine drawing.
[0152] The drawing passes and drawing speeds were the same as in Example 1. The calculated cumulative true strain of the copper wire was 4.28, and the cross-sectional compression ratio of each drawing pass did not exceed 22%, indicating a state of high cumulative deformation without localized deformation concentration.
[0153] The average diameter of the hardened copper wire after micro-stretching is 0.1202 mm, the tensile strength is 468 MPa, and the elongation is 2.5%.
[0154] 2. Single-zone annealing treatment The recovery section, partial recrystallization section, and structure stabilization section in Example 1 were replaced with a single-temperature annealing zone.
[0155] The single-zone annealing temperature was set to 380℃, and the total residence time of the copper wire in the annealing zone was set to 2.2s, which is the same as the total residence time of the three annealing zones in Example 1; the production line speed was maintained at 40m / min, and the traction force in the annealing zone was 0.06N.
[0156] During continuous annealing, the heating power is adjusted only according to the outlet temperature of the annealing zone, without separately controlling the recovery, recrystallization and stabilization stages.
[0157] 3. Follow-up processing The copper wires after single-temperature annealing are processed sequentially as follows: (1) The temperature of the copper wire was reduced to 102℃ by circumferential atomizing spray; (2) Through a water-soluble copper antioxidant solution with a mass percentage concentration of 0.30%; (3) Drying is carried out in a 130℃ drying zone and a 70℃ temperature homogenization zone; (4) Use a low-residue halogen-free flux with an effective solid content of 6.0% for dip coating; (5) Immerse in molten high-purity tin at 260℃ for 0.60s; (6) The total tin plating thickness is controlled by a four-channel annular airflow. (7) Take in and wind up the wire at a speed of 40 m / min.
[0158] The target thickness and annular airflow adjustment method of the copper-tin alloy transition layer and the free tin layer are the same as those in Example 1.
[0159] 4. Test Results Five samples were randomly selected from the obtained tin-plated thin-diameter copper busbars, and the test results are as follows: Table 11 Test results of Comparative Example 1
[0160] Microstructural analysis showed that single-temperature annealing caused recrystallization in most areas of the copper wire, with significantly larger grains forming in some localized areas. Because a low-temperature recovery stage and a post-recrystallization stabilization stage were not included, the grains in the localized high-energy-storage regions continued to grow, leading to a decrease in the strength of the copper wire.
[0161] During the subsequent tin plating and winding process, the copper wire underwent a certain degree of secondary stretching in the annealed and softened state, with an average diameter reduction greater than that in Example 1, and two wire breaks occurred during the continuous production of 1000m.
[0162] After 20 low-temperature cycles between room temperature and 77K, the average resistivity change rate of the sample was 0.73%, and the number of surface microcracks was 1.9 lines / cm. Although the coating thickness basically met the requirements, the stability of the copper substrate structure and the continuous processing performance were lower than those of Example 1.
[0163] This shows that simply extending the heating time of copper wire at a certain temperature cannot replace the microstructure regulation functions undertaken by the recovery section, the partial recrystallization section, and the microstructure stabilization section, respectively.
[0164] Comparative Example 2: Copper wires with concentrated local deformation were subjected to fixed segmented annealing parameters. This comparative example illustrates that, even with the same initial diameter, final wire diameter, and cumulative true strain of the copper base material, if the segmented annealing parameters are not adjusted according to the deformation distribution of the drawing passes, problems such as excessive residual stress and abnormal local grain growth may still occur.
[0165] Except for the annealing parameters, this comparative example uses the same drawing path, tension control, cooling, anti-oxidation, drying, fluxing, tin dipping and take-up conditions as Example 2.
[0166] 1. Pull-out treatment for concentrated local deformation Oxygen-free copper wire with a diameter of 1.02mm is used, which is then drawn to a fineness of 0.254mm, and then drawn according to the following main micro-drawing diameters: 0.254mm, 0.227mm, 0.203mm, 0.181mm, 0.165mm, 0.150mm, 0.129mm and 0.120mm.
[0167] Among them, the cross-sectional compression rate of the 0.150mm to 0.129mm drawing pass is 26.0%, the drawing tension of this pass is 1.48N, and the average drawing tension of adjacent micro-drawing passes is 1.08N.
[0168] The cumulative true strain of this batch of copper wires is 4.28, which is a state of high cumulative deformation and localized deformation concentration.
[0169] 2. Fixed segmented annealing process This comparative example does not extend the recovery segment according to the local deformation concentration state, but directly adopts the fixed annealing parameters set in Example 1 for copper wires without local deformation concentration: Table 12 Comparative Example 2 Fixed Annealing Parameters
[0170] The production line speed is 40m / min, and the traction force in the annealing tension zone is 0.06N.
[0171] Compared to Example 2, this comparative example did not extend the dwell time of the recovery segment to 1.3s, did not reduce the temperature of the partial recrystallization segment, and did not extend the dwell time of the tissue stabilization segment.
[0172] 3. Follow-up processing The annealed copper wire is processed using the same process as in Example 2: (1) First stage atomization cooling; (2) Antioxidant treatment; (3) Dual-temperature zone drying; (4) Flux dipping; (5) Hot-dip tin plating in 260℃ high-purity tin liquid; (6) Four-channel annular airflow control layer; (7) Leading and taking up the wire.
[0173] The total tin plating thickness is controlled at 3.2–3.6 μm.
[0174] 4. Test Results The test results are as follows: Table 13 Detection results of Comparative Example 2
[0175] In the cross-section of the copper wire in Comparative Example 2, larger recrystallized grains were formed in the high-energy storage region corresponding to the local concentrated drawing passes, while the adjacent region still had a lot of drawing fiber structure, showing obvious structural inhomogeneity.
[0176] This is because the dwell time of the fixed recovery section is insufficient to fully release the residual stress formed by local concentrated deformation, while the partial recrystallization treatment at 405℃ causes rapid recrystallization and grain growth to preferentially occur in the high energy storage region.
[0177] Tests conducted after tin plating revealed: Table 14 Test results after tin plating in Comparative Example 2
[0178] It can be seen that the coating of Comparative Example 2 can meet the basic thickness requirements, but due to the unstable structure and mechanical properties of the copper substrate, wire breakage and hot drawing still occur during continuous production.
[0179] After 20 low-temperature cycles between room temperature and 77K, the average resistance change rate of the sample was 0.69%, which was higher than 0.47% in Example 2; the number of local cracks after low-temperature bending was 2.4 per sample, while that in Example 2 was 1.0 per sample.
[0180] The above results show that having the same final wire diameter and cumulative true strain does not mean that the same annealing parameters can be used. It is also necessary to adjust the heat input of the recovery section, partial recrystallization section and microstructure stabilization section according to the degree of deformation concentration of the drawing pass.
[0181] Comparative Example 3: Fixed air blowing for tinning based solely on the total outer diameter of the tin plating This comparative example is for illustration purposes only. It only measures the total outer diameter of the tin-plated wire and adjusts the air volume accordingly. It cannot identify the thickness distribution of the copper-tin alloy transition layer and the free tin layer, nor can it improve the circumferential deviation of the plating layer and the low-temperature cycling performance.
[0182] Except for hot-dip tin plating and blower control, this comparative example uses the same copper material, drawing, annealing, cooling, anti-oxidation, drying and fluxing conditions as Example 3.
[0183] 1. Copper wire preparation and annealing treatment Oxygen-free copper wire with a diameter of 1.02mm is used, which is then stretched to 0.254mm and then further stretched to 0.12mm.
[0184] The parameters for segmented annealing are: Table 15 Comparative Example 3: Segmented Annealing Parameters
[0185] The production line speed is 40 m / min. After annealing, the tensile strength of the copper wire is 251 MPa, and the elongation is 18.0%.
[0186] 2. Hot-dip tin plating The copper wire after soldering is immersed in high-purity tin liquid at 272℃, with an effective immersion path length of 0.46m and an effective immersion time of 0.69s.
[0187] This comparative example does not collect continuous temperature-time data of the copper wire from the annealing exit to the initial cooling stage after tinning, does not calculate the characterization value of the copper-tin alloy transition layer thickness, and does not adjust the tin liquid temperature, immersion time or initial cooling intensity according to the alloy layer thickness.
[0188] 3. Fixed airflow control for soldering An integrated annular blower is installed at the molten tin outlet, with all directions sharing the same air supply chamber, making it impossible to adjust the airflow pressure in different circumferential directions separately.
[0189] The operator adjusts the overall blowing pressure based solely on the diameter of the copper wire before tinning and the total outer diameter after tinning. When the outer diameter of the tinned wire is higher than the target value, the overall blowing pressure is increased; when the outer diameter of the tinned wire is lower than the target value, the overall blowing pressure is decreased.
[0190] After adjustment, the overall blowing pressure was set to 9.0 kPa, which stabilized the average outer diameter of the tin-plating wire at 0.1269 mm. The average diameter of the copper substrate was 0.1201 mm, corresponding to a total tin plating thickness of 3.40 μm, which is the same as the total tin plating thickness in the second production stage of Example 3.
[0191] 4. Coating cross-section inspection Since this comparative example only controls the overall outer diameter, although the total tin plating thickness meets the target requirements, the cross-sectional inspection results are as follows: Table 16 Test results of section 3 in Comparative Example 3
[0192] The thickness of the copper-tin alloy transition layer is significantly higher than that of the second production stage in Example 3 (0.71 μm). However, the overall blowing can only remove the unsolidified free tin on the outside and cannot thin the already formed copper-tin alloy transition layer.
[0193] Meanwhile, since the integral annular blower cannot adjust the airflow in each direction according to the circumferential thickness deviation, the maximum circumferential thickness difference of Comparative Example 3 is 0.74 μm, which is significantly greater than the 0.17 μm of the second production section of Example 3.
[0194] 5. Low-temperature cycling test Five groups of samples were randomly selected from the tin-plated narrow-diameter copper busbars obtained in this comparative example. The samples were cycled 30 times between room temperature and 77K. The test results are as follows: Table 17 Low-temperature cycling test results of Comparative Example 3
[0195] After low-temperature cycling, some cracks in Comparative Example 3 started from the thicker copper-tin alloy transition layer and extended outward along the circumferentially thinner free tin layer region. Localized peeling and increased contact resistance occurred in some areas where the tin layer was thinner.
[0196] The above results indicate that even with the same total tin plating thickness, different thickness distributions of the copper-tin alloy transition layer and the free tin layer can lead to significantly different low-temperature cycling performance. Simply adjusting the airflow rate based on the total outer diameter cannot correct for an excessively thick alloy transition layer, nor can it effectively eliminate circumferential thickness unevenness.
[0197] Explanation of Comparative Results The three comparisons illustrate the following: (1) Comparative Example 1 shows that single-temperature annealing cannot replace segmented annealing with different microstructure regulation effects; (2) Comparative Example 2 shows that setting fixed segmented annealing parameters only based on the final wire diameter cannot adapt to the drawing state with concentrated local deformation; (3) Comparative Example 3 shows that controlling the total thickness of tin plating alone cannot replace the dual-layer decoupling control of the alloy transition layer and the free tin layer.
[0198] Therefore, the technical effect of this application is not produced by a single annealing, tinning, or blowing parameter, but rather by the synergistic effect between "drawing deformation state identification - segmented annealing microstructure adjustment - continuous thermal process control of alloy transition layer - annular zoned airflow control of free tin layer".
[0199] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of this application.
Claims
1. A method for segmented annealing and hot-dip tin plating control layering of a thin-diameter copper busbar for superconducting applications, characterized in that, include: S1. The copper base material is subjected to fine drawing and micro-fine drawing in sequence to obtain a hardened fine-diameter copper busbar, and the cumulative deformation state is determined according to the cross-sectional area change of the copper base material and the hardened fine-diameter copper busbar and the deformation distribution of each drawing pass. S2. According to the cumulative deformation state, the hard-state thin-diameter copper busbar is subjected to segmented annealing by passing through the recovery section, the partial recrystallization section and the structure stabilization section in sequence, so as to reduce the residual stress after drawing, form a partial recrystallization structure and inhibit the continued growth of grains. S3. After annealing, the fine-diameter copper busbar is subjected to graded cooling, anti-oxidation treatment and drying treatment in sequence, and adjusted to the preset tin-entry temperature and flux is applied. S4. The thin-diameter copper busbar after applying flux is sent into the tin liquid for hot-dip tin plating. Based on the temperature-time history of the thin-diameter copper busbar from the annealing outlet to the tin removal and cooling stage, the thickness characterization value of the copper-tin alloy transition layer is determined, and at least one of the tin liquid temperature, tin immersion time and tin removal cooling intensity is adjusted according to the thickness characterization value. S5. Obtain the diameter of the copper wire before hot-dip tin plating and the outer diameter of the tin-plated wire after the tin layer solidifies, determine the total tin plating thickness, and determine the free tin layer thickness characterization value based on the total tin plating thickness and the copper-tin alloy transition layer thickness characterization value. S6. Adjust the annular airflow parameters at the tin melt outlet according to the free tin layer thickness characterization value, and adjust the airflow in the corresponding direction according to the circumferential thickness deviation of the tin plating line to control the free tin layer thickness and circumferential uniformity, and then perform take-up and winding.
2. The method according to claim 1, characterized in that, The cumulative deformation state includes the cumulative true strain and the deformation distribution of each drawing pass, and the cumulative true strain is determined according to the following formula: ; In the formula, To accumulate true strain, and These are the cross-sectional areas of the copper base material and the hardened, thin-diameter copper busbar, respectively. and The diameters are those of the copper base material and the hardened fine-diameter copper busbar, respectively; the deformation distribution of each drawing pass is determined based on the cross-sectional compression ratio and drawing tension of each drawing pass.
3. The method according to claim 2, characterized in that, The heating temperature of the recovery section is 180–320°C, and the residence time is 0.3–3.0 s; The heating temperature of the recrystallization section is 300–500°C, and the residence time is 0.2–2.0 s; The heating temperature of the tissue stabilization section is 220–380°C, and the residence time is 0.2–2.0 s, and the heating temperature of the tissue stabilization section is lower than the heating temperature of the partial recrystallization section.
4. The method according to claim 3, characterized in that, The initial heating temperature and dwell time of each annealing section are determined based on the correspondence between the accumulated true strain and the pre-calibrated annealing parameters. The preset upper limit is determined by a drawing test of copper wire of the same material; when the maximum cross-sectional compression ratio or drawing tension in the drawing pass exceeds the corresponding preset upper limit, the dwell time of the recovery section is extended first, and then the heating temperature of the partial recrystallization section is adjusted so that the fine-diameter copper busbar forms a partially recrystallized structure in which the drawn fiber structure and the recrystallized structure coexist.
5. The method according to claim 1, characterized in that, The conveying path of the fine-diameter copper busbar is divided into the tension zone before annealing, the tension zone after annealing, the tension zone after cooling and drying, the tension zone after tinning, and the tension zone after take-up. The corresponding tensile stress is determined based on the traction force of each tension zone and the diameter of the thin-diameter copper busbar. The tensile stress of the annealing tension zone is controlled to be 5% to 35% of the yield strength corresponding to the copper busbar temperature, and the traction force of the tin-immersion tension zone is lower than that of the tension zone before annealing.
6. The method according to claim 1, characterized in that, The graded cooling and antioxidant treatment includes a first cooling stage and a second antioxidant treatment stage; In the first cooling stage, the annealed fine-diameter copper busbar is cooled to 60-160°C to stop its continued recrystallization; In the second antioxidant treatment stage, the thin-diameter copper busbar is passed through an antioxidant solution with a mass percentage concentration of 0.05% to 2.0%. After drying, the temperature of the thin-diameter copper busbar before applying flux is adjusted to 30-100℃.
7. The method according to claim 6, characterized in that, The thickness of the copper-tin alloy transition layer is determined according to the following formula: ; In the formula, This represents the thickness of the copper-tin alloy transition layer. These are calibration constants obtained through copper-tin interface reaction experiments. R is the apparent activation energy of the copper-tin interface reaction, and R is the molar gas constant. and The first Absolute temperature and duration of the copper-tin interface within the specified temperature range. This refers to the number of temperature ranges where the copper-tin interface temperature is higher than the preset reaction termination temperature.
8. The method according to claim 7, characterized in that, The thickness of the free tin layer is determined according to the following formula: ; In the formula, This represents the thickness of the free tin layer. The diameter of the copper wire before hot-dip tin plating. This refers to the outer diameter of the tin-plated wire after the tin layer has solidified. The thickness of the copper-tin alloy transition layer is 0.1–2.0 μm, and the thickness of the free tin layer is 0.5–8.0 μm.
9. The method according to claim 8, characterized in that, The annular airflow is formed by at least four independent airflow channels arranged circumferentially along the tin-plated line, and the circumferential thickness difference of the tin-plated line is obtained by combining at least two intersecting diameter measurement directions with circumferential sampling detection. When the tin layer thickness corresponding to any measuring direction exceeds the preset thickness limit, the airflow pressure of the airflow channel corresponding to the direction with the larger thickness is increased, or the airflow pressure of the airflow channel opposite to that direction is decreased.
10. The method according to claim 9, characterized in that, Cyclic testing was performed on the tin-plated small-diameter copper busbar after the control layer was applied, between room temperature and a preset low temperature. When the rate of change of resistance after the cycle exceeds the preset limit and the elongation of the thin-diameter copper busbar is lower than the preset elongation, the heating temperature of part of the recrystallization section is increased or its residence time is extended. When the number of cracks in the tin layer after the cycle exceeds the preset crack limit and the thickness characterization value of the copper-tin alloy transition layer is higher than the preset upper limit, the tin liquid temperature is reduced, the immersion time is shortened, or the tin removal cooling intensity is increased. When the number of cracks in the tin layer after the cycle exceeds the preset crack limit and the thickness characterization value of the copper-tin alloy transition layer is lower than the preset lower limit, the tin liquid temperature is increased, the immersion time is extended, or the tin removal cooling intensity is reduced.