Corrosion-resistant composite strengthening coating and preparation method and application thereof

By combining supersonic arc spraying technology with epoxy resin sealant, a composite reinforced coating with low porosity and high bonding strength is prepared, which solves the problem of insufficient wear resistance and corrosion resistance of existing coatings under coupled conditions of mud and sand erosion and electrochemical corrosion, and achieves efficient and low-cost local repair effect.

CN123152979APending Publication Date: 2026-11-24SANXIA JINSHAJIANG YUNCHUAN HYDROPOWER DEV CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611291580.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing protective coatings for flow-through components suffer from problems such as high porosity, low bonding strength, difficulty in achieving synergistic wear and corrosion resistance, complex or costly processes, and the risk of secondary damage to surrounding intact coatings during local repairs. These issues are particularly difficult to effectively address under conditions of coupled mud and sand erosion and electrochemical corrosion.

Method used

A double-layer composite reinforced coating is prepared using high-chromium iron-based core wire, chromium-nickel iron-based alloy wire, or nickel-aluminum alloy solid wire through supersonic arc spraying technology. The metal functional layer is combined with the epoxy resin sealing layer. The process parameters are optimized to achieve low porosity, high bonding strength, and excellent wear resistance and corrosion resistance, and localized precise repair avoids secondary damage.

Benefits of technology

The prepared composite reinforced coating has a porosity of no more than 3%, a bonding strength of no less than 50 MPa, significantly improved wear resistance and corrosion resistance, and a service life of 10 to 15 years. It is low in cost and suitable for on-site repair of large flow components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152979A_ABST
    Figure CN123152979A_ABST
Patent Text Reader

Abstract

This invention discloses a corrosion-resistant composite reinforced coating, its preparation method, and its application. By selecting spraying wires with specific components and optimizing supersonic arc spraying process parameters, combined with precise local pretreatment and sealant coating, a synergistic improvement in the corrosion resistance and mechanical properties of flow components is achieved. This method uses alloy wires as the coating material in conjunction with an epoxy resin sealant. Through precise adjustment of spraying parameters, a corrosion-resistant composite reinforced coating is prepared on the surface of commonly used structural steel or stainless steel, effectively solving the wear and corrosion damage problems of flow components such as turbines and extending their service life. This coating preparation method has fewer steps, high deposition efficiency, and no stringent requirements on the construction environment. This coating preparation method can be applied to engineering equipment such as flow components in hydropower stations that are subjected to long-term scouring and corrosive environments containing silt, as well as to the surface protection of components and engineering structures under severe abrasive conditions in various aquatic environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wear-resistant, corrosion-resistant and repair technology for metal surfaces, specifically to a corrosion-resistant composite reinforcing coating and its preparation method and application. Background Technology

[0002] As key basic components in core industrial fields such as hydropower, nuclear power, petrochemicals, and water supply and drainage, flow-through components are widely used in core equipment such as turbine guide vanes, runners, pump impellers, oil and gas pipelines, and chemical reactor linings. Their service condition directly determines the operational stability, safety, and economy of the entire system. These components are exposed to extremely complex working environments for extended periods, facing the combined effects of wear, corrosion, and cavitation damage mechanisms. On the one hand, sand and solid particles carried by water, air, or media flow continuously scour and wear the component surface. Especially under high-speed flow conditions, particle impact causes continuous peeling of surface material, forming erosion pits and grooves. On the other hand, corrosive media such as chloride ions, acid and alkali ions, and dissolved oxygen in the medium can trigger electrochemical corrosion, crevice corrosion, and even stress corrosion cracking, causing a rust layer to form on the component surface and gradually penetrate inward. In addition, alternating water vapor and sudden temperature changes can induce cavitation erosion. The instantaneous high-pressure shock wave generated by the bursting of bubbles continuously impacts the component surface, accelerating material fatigue and spalling.

[0003] The synergistic effects of wear, corrosion, and cavitation described above can lead to problems such as thinning of the walls, increased surface roughness, and deterioration of the mechanical properties of flow components. In severe cases, this can cause component deformation, leakage, or even breakage and failure. Statistics show that in the hydropower industry, downtime due to corrosion and wear of flow components accounts for more than 40% of all failures. The replacement cost of a single megawatt-class turbine runner can reach tens of millions of yuan, with downtime periods lasting 1 to 3 months, resulting in huge economic losses. In the chemical industry, leaks in flow pipelines caused by corrosive media can also lead to the spread of toxic and harmful media, causing environmental pollution and safety accidents. Therefore, solving the wear and corrosion problems of flow components and extending their service life has become a core technical requirement for ensuring the safe and efficient operation of industrial systems and reducing maintenance costs.

[0004] To address the challenges of wear and corrosion in flow-through components, the industry has developed various protection and repair technologies, primarily through material upgrades and coating development. However, their effectiveness is limited. Directly manufacturing flow-through components using corrosion-resistant and wear-resistant materials such as stainless steel, titanium alloys, and Hastelloy can significantly improve component lifespan and extend replacement cycles. However, these materials are extremely expensive, typically more than five times the cost of ordinary carbon steel, and are difficult to process and weld, leading to a substantial increase in component production costs. Furthermore, even with high-end alloy materials, the surface of components still suffers varying degrees of damage under the intense impact of mud and water and the long-term effects of corrosive media, meaning that upgrading the material grade does not fundamentally solve the problem. In contrast, surface protection technologies can significantly improve the surface properties of materials without requiring replacement of the manufacturing materials. Epoxy coatings, the most common industrial protective system, are low-cost and simple to manufacture. The dense coating isolates the material from corrosive media, providing some corrosion protection. However, the core problem with epoxy resin coatings lies in their poor adhesion to the substrate, with a bonding strength often below 10 MPa. Under prolonged and intense erosion by mud and water, the coating is prone to peeling off, resulting in a protection lifespan of only 1-2 years. Arc spraying technology coats a metal surface with a layer of alloy coating of a certain thickness and special properties. Due to the metallurgical bond between the coating and the substrate, its bonding strength is far higher than that of epoxy organic coatings. However, ordinary arc spraying technology is limited by nozzle pressure, leading to uneven melting and oxidation of the metal material during spraying. This results in a porosity generally exceeding 5%, allowing corrosive media to easily penetrate the substrate-coating interface, causing interfacial corrosion and coating peeling. Furthermore, the coating's wear resistance is insufficient, making it difficult to resist the erosion of high-hardness particles. Its service life is only 3-5 years, longer than epoxy coatings, but still far below the designed service life of over 10 years for industrial equipment. While plasma spraying technology can produce high-density coatings and effectively solves the problem of excessive porosity in ordinary arc spraying coatings, this technology is expensive, energy-intensive, and complex, and is generally only suitable for laboratory research or the processing of small components, making it difficult to meet the on-site repair needs of large flow components. Furthermore, traditional coating repair techniques are prone to causing secondary damage to components: damage to flow components often exhibits localized characteristics, and traditional local repair methods, such as overall sandblasting or mechanical grinding of the corroded area, easily damage the density and bonding of the surrounding intact coating, leading to secondary damage. Moreover, the lack of targeted process parameter control during the repair process results in poor compatibility between the repaired coating and the original coating, easily causing interface peeling and affecting the overall protective effect.

[0005] A search revealed that the closest prior art to this invention is patent publication number CN103286516A, which also relates to arc spraying protection technology for hydraulic machinery flow components. However, the two technologies differ fundamentally. CN103286516A addresses single cavitation damage, requiring a welding process to fill cavitation pits deeper than 1 mm. While nominally employing high-speed arc spraying, it is actually a subsonic spraying process with compressed air pressure of only 0.6 MPa and a droplet velocity of approximately 220 m / s. The process parameters have an extremely wide range and lack criticality. The filament used is a common Fe-Ni-Cr-BC-Si-Re filament, and the coating's maximum hardness is 920 HV. The overall structure consists of a three-layer structure: a substrate, a welding layer, and a sprayed coating. An integral spraying method is used, combined with an organosilicon resin sealing agent containing nano-Al2O3 to enhance cavitation resistance. However, the welding process has a large heat-affected zone, easily damaging the surrounding intact coating. Furthermore, patent document CN102181813A addresses single cavitation erosion damage using a Cr-free FeNiBSiP amorphous powder-core wire. This wire has poor thermal stability and virtually no corrosion resistance. Its process parameters only have the gas pressure approaching the critical value, while the current parameter is insufficient, failing to achieve a true supersonic spraying effect through multi-parameter synergy. Patent document CN101191225B uses a single FeCrNiMoBSiCuRE general-purpose wire combined with a conventional arc spraying process, only vaguely mentioning pore sealing treatment, lacking quantitative data and local repair designs for the coupled conditions of silt erosion and electrochemical corrosion. All of the above-mentioned existing technologies share common limitations: a single damage mode, failure to overcome the bottleneck of subsonic spraying performance, reliance on a single general-purpose wire system, and a lack of specific design for the most common and severe coupled damage caused by silt erosion and electrochemical corrosion in the hydropower industry.

[0006] In summary, to address the problems existing in current wear and corrosion protection coating technologies for flow-through components, this paper proposes a composite reinforced coating technology suitable for on-site repair of flow-through components. This technology involves optimizing the supersonic spraying process parameters, applying a high-alloy coating, and combining it with an epoxy resin sealant. This results in a composite reinforced coating with low porosity, high bonding strength, high hardness, and synergistic wear and corrosion resistance. Summary of the Invention

[0007] The technical problem to be solved by this invention is: addressing the common problems of existing protective coatings on the surface of flow components, such as high porosity, low bonding strength, difficulty in achieving synergistic wear resistance and corrosion resistance, complex or high cost processes, and the tendency for local repairs to cause secondary damage to the surrounding intact coatings. This invention provides a corrosion-resistant composite reinforced coating, its preparation method, and its application. This coating, which combines low porosity, high bonding strength, and excellent wear resistance and corrosion resistance, can be prepared on the surface of commonly used structural steel and stainless steel substrates. It enables precise, efficient, and low-cost repair of localized wear and corrosion damage areas in flow components such as turbine guide vanes, runners, and pump impellers, extending their service life in environments with silt-laden water flow and corrosion.

[0008] To achieve the above objectives, the present invention provides the following technical solutions for corrosion-resistant composite reinforced coatings, their preparation methods, and applications: I. Overall Structure of the Coating The corrosion-resistant composite reinforced coating provided by this invention has a two-layer composite structure, consisting of a bottom metal functional layer and a top epoxy resin sealing layer. The metal functional layer is prepared using any one of the following: high-chromium iron-based flux-cored wire, chromium-nickel iron-based alloy wire, or nickel-aluminum alloy solid wire, through supersonic arc spraying technology. It primarily provides high hardness and wear resistance. The epoxy resin sealing layer is coated on the surface of the metal functional layer to seal residual pores within the metal functional layer and block the penetration path of corrosive media to the substrate-coating interface, primarily enhancing corrosion resistance. These three wire materials are independent optional technical solutions. The technical effect of this invention can be achieved by selecting one based on the actual operating performance requirements of the component to be protected, rather than requiring a combination or composite use. In other words, when preparing the metal functional layer, it is not necessary to use multiple wire materials simultaneously to form a multi-layer or gradient layer structure. Simply selecting any one of the wire materials and combining it with the supersonic arc spraying process parameters specified in this invention can produce a metal functional layer with a porosity of no more than 3% and a bonding strength of no less than 50 MPa.

[0009] II. Selection of Substrate Currently, flow-through components in hydroelectric power plants operating in silt-flushing water environments, such as turbine guide vanes, runners, and pump impellers, are generally made of stainless steel, including 0Cr13Ni4Mo martensitic stainless steel, 304 austenitic stainless steel, 316L austenitic stainless steel, and 20SiMn high-strength alloy steel. In pressure-bearing flow-through components, such as volutes and pressure pipes, high-strength structural steel is typically used, including Q235B and Q345R. Therefore, the substrate selected for supersonic arc spraying in this invention is at least one of stainless steel and structural steel, preferably 316L austenitic stainless steel. The substrate is preferably a 100mm × 100mm × 10mm block to facilitate coating performance testing and evaluation; in practical engineering applications, the size and shape of the substrate can be determined according to the actual structure of the flow-through component to be protected.

[0010] III. Local Pretreatment Before preparing a corrosion-resistant composite reinforced coating using supersonic arc spraying technology, it is necessary to first identify the local wear and corrosion damage areas on the surface of the component to be protected. High-temperature resistant tape is then used to cover the intact, undamaged areas around the damaged areas, exposing only the local wear and corrosion damage areas of the component to be treated. This avoids secondary damage to the surrounding intact coating caused by the sandblasting and spraying process.

[0011] After exposing the damaged area, the substrate surface in that area needs to be roughened and derusted, preferably by surface sandblasting. Specifically, quartz sand with a particle size of 0.8–1.2 mm is used as the sandblasting medium, and the sandblasting pressure is 0.5–0.6 MPa. After derusting, the surface roughness Ra of the substrate is controlled at 5–8 μm, and the pretreated surface is free of visible rust and oil, thus providing a good bonding foundation for the subsequent supersonic arc spraying of the metal functional layer.

[0012] IV. Selection of Spray Coating Wire This invention allows for the selection of wires with different compositions to prepare the metal functional layer based on the actual operating performance requirements of the flow-through components. Specifically, it includes the following five optional wires: High-chromium iron-based core wire A has the following chemical composition by mass fraction: Cr 30%–40%, Ni < 0.1%, Mn < 1%, B 3%–5%, Si < 1%, C ≤ 2%, with the balance being Fe. When this wire is used for spraying, the coating hardness can reach up to 1375 HV, and the porosity is approximately 2.0%.

[0013] The high-chromium iron-based flux-cored wire B has the following chemical composition by mass fraction: Cr 18%–22%, Ni 9%–11%, Mn 1%–2%, B 3%–6%, Si 1%–2%, with the balance being Fe. When this wire is used for spraying, the coating hardness can reach up to 1113.2 HV, and the porosity is approximately 1.9%.

[0014] The chromium-nickel-iron-based alloy wire C has the following chemical composition by mass fraction: Cr 17%–19%, Ni 8%–11%, Mn 2%, Si 1%, C 0.07%, with the balance being Fe. When this wire is used for spraying, the coating hardness can reach up to 284.0 HV, and the porosity is approximately 1.2%.

[0015] Chromium-nickel-iron based alloy wire D has the following chemical composition by mass fraction: Cr 12.5%, Ni 4.7%, Mn 0.7%, Si 0.4%, C 0.03%, Mo 0.8%, with the balance being Fe. When this wire is used for spraying, the coating hardness can reach up to 360.0 HV, and the porosity is approximately 0.5%.

[0016] The solid nickel-aluminum alloy wire E has the following chemical composition by mass fraction: Ni 94.5%–95.5%, Al 4.5%–5.5%, Mn < 0.3%, Si < 0.5%, Fe < 0.3%. When this wire is used for spraying, the coating hardness can reach up to 320.3 HV, and the porosity is approximately 0.4%.

[0017] The high-chromium iron-based flux-cored wire A and high-chromium iron-based flux-cored wire B mentioned above both belong to the high-chromium iron-based flux-cored wires described in this invention, while chromium nickel iron-based alloy wire C and chromium nickel iron-based alloy wire D can both be classified into the chromium nickel iron-based alloy wire category described in this invention. The diameter of the wire is preferably 1.0–2.0 mm, more preferably 2.0 mm; the length of the wire is not less than 1500 mm. The five wires A to E mentioned above are all independent alternative technical solutions. The technical effect of this invention does not depend on the combination or composite use of multiple wires; the corresponding technical effect can be achieved by selecting one according to the actual working condition and performance requirements of the component to be protected.

[0018] It should be noted that the high-chromium iron-based flux-cored wire used in this invention has significant differences in composition design compared with the conventional FeCrBSi or FeNiBSiP arc spraying wires that have been disclosed. The coating performance achieved by the two under the supersonic arc spraying process is also fundamentally different. Conventional FeCrBSi wires are typically designed for ordinary arc spraying processes. Their composition optimization aims to achieve better spreadability of the molten droplets at lower droplet velocities, resulting in coatings with a hardness of 600–800 HV. In contrast, the high-chromium iron-based flux-cored wire A in this invention, with its extremely low Ni content combined with high Cr and B content, forms a large number of high-hardness CrB and Fe2B phases within the coating under the intense impact of supersonic droplets, increasing the coating hardness to 1375 HV, far exceeding the hardness level of conventional FeCrBSi coatings. The high-chromium iron-based flux-cored wire B, by increasing the Ni content to 9%–11% and the B content to 3%–6%, achieves a balance between hardness and toughness while maintaining high hardness, and simultaneously improves the corrosion resistance of the coating. This gives the coating a comprehensive performance advantage of both wear resistance and corrosion resistance, which is difficult to achieve simultaneously with conventional FeCrBSi or FeNiBSiP arc spraying wires.

[0019] Furthermore, the composition of the high-chromium iron-based flux-cored wire B has a synergistic strengthening effect with the supersonic arc spraying process parameters defined in this invention. The two work together to reduce the porosity of the coating by more than 60% and increase the bonding strength by more than 80%. The reason is that the composition of high-chromium iron-based flux-cored wire B gives it optimal melting characteristics under process conditions of arc working voltage of 34-40V and arc working current of 210-240A. Combined with compressed air pressure of 0.7-1.0MPa, the droplet velocity can reach the optimal supersonic range of 400-450m / s. Under this parameter range, when the droplets of high-chromium iron-based flux-cored wire B impact the substrate, they can undergo sufficient plastic deformation to form a dense layered stacked structure, reducing the coating porosity to 1.9%, which is far lower than the porosity level of more than 5% under conventional process conditions. This dense layered structure not only improves the bonding strength of the coating, but also allows the Cr element in the coating to be evenly distributed, forming a continuous chromium oxide protective film, thereby greatly improving the corrosion resistance of the coating.

[0020] Furthermore, nickel-aluminum alloy solid wire E possesses characteristics of low porosity and high bonding strength, and the porosity of the prepared metal functional layer can be as low as 0.4%, exhibiting excellent corrosion resistance. It is particularly suitable for operating conditions where high corrosion resistance of the coating is required, while the requirements for hardness and wear resistance are relatively low. The metal functional layers prepared from chromium-nickel-iron based alloy wires C and D have hardness and corrosion resistance properties between those of high-chromium-iron based flux-cored wires and nickel-aluminum alloy solid wires, exhibiting good comprehensive performance and suitable for operating conditions where wear resistance and corrosion resistance requirements are relatively balanced. In this invention, the high-chromium-iron based flux-cored wire, chromium-nickel-iron based alloy wire, and nickel-aluminum alloy solid wire are all independent metal functional layer material solutions. They can be used individually to meet the differentiated protection requirements of different flow components under different service conditions, without the need for combination in a stacked or gradient layer manner.

[0021] V. Supersonic Arc Spraying Process Parameters This invention, through numerous single-factor and multi-factor orthogonal experiments, determined the optimal process parameter window for preparing corrosion-resistant composite reinforced coatings by supersonic arc spraying: arc working voltage of 34–40V, arc working current of 210–240A, spraying distance of 10–20cm, compressed air pressure of 0.7–1.0MPa, wire feed speed of 8–15m / min, 2–3 spraying passes, and controlling the thickness of the resulting metallic functional layer to be 200–280μm.

[0022] Experiments have shown that when any of the above process parameters deviates from the range defined by this invention, the coating performance will significantly deteriorate; only when all process parameters fall within the range defined by this invention can the synergistic effect of low porosity, high bonding strength, and excellent corrosion resistance be achieved simultaneously. This indicates that there is a critical relationship of mutual constraint and synergistic effect among the parameters, rather than conventional process parameters that are independent and arbitrarily adjustable. Specifically: Firstly, when the arc working voltage is below 34V, the wire is not fully melted, and the coating porosity rises sharply to over 5%; when the arc working voltage is above 40V, the molten droplets are severely oxidized, and the coating's corrosion resistance decreases significantly.

[0023] Secondly, when the arc working current is below 210A, the melting rate of the wire is insufficient and the deposition efficiency is low; when the arc working current is above 240A, the molten droplets overheat, the internal stress of the coating is too large, and cracking is likely to occur.

[0024] Third, when the spraying working distance is less than 10cm, the molten droplets splash severely; when the spraying working distance is greater than 20cm, the kinetic energy of the molten droplets when they reach the substrate surface is insufficient, resulting in a decrease in bonding strength.

[0025] Fourth, when the compressed air pressure is below 0.7 MPa, the molten droplets cannot reach supersonic speed, and the bonding strength of the resulting coating is below 40 MPa; when the compressed air pressure is above 1.0 MPa, the molten droplet splashing rate and the internal stress of the coating increase sharply.

[0026] Fifth, when the wire feeding speed is below 8 m / min, the coating grains are coarse; when the wire feeding speed is above 15 m / min, the wire is not fully melted, and a large number of unmelted particles appear in the coating.

[0027] After the aforementioned metal wire is melted at the high temperature of an electric arc, it is accelerated by compressed air at 0.7–1.0 MPa to form supersonic atomized droplets with an average velocity of 350–550 m / s. This velocity range is determined based on the jet acceleration capability of the supersonic electric arc spraying equipment under corresponding compressed air pressure conditions and the measured flight velocity of the wire droplets. When these supersonic droplets impact the substrate surface, they undergo intense plastic deformation, fully filling the micro-anchor patterns on the substrate surface. Subsequently, they rapidly solidify to form a dense, functional metal layer with a porosity of no more than 3%, a bonding strength of no less than 50 MPa, high hardness, and excellent corrosion resistance.

[0028] In addition, during the supersonic arc spraying process, the moving speed of the spray gun is 5 to 15 mm / s, the single spraying time is 5 to 15 s, and the angle between the spray gun and the substrate surface is kept at 90° to ensure that the molten droplets are uniformly deposited on the substrate surface to form a metal functional layer of uniform thickness.

[0029] VI. Preparation of Epoxy Resin Sealing Layer After the metal functional layer cools to room temperature, an epoxy resin sealant is applied to the surface of the metal functional layer by brushing, spreading it evenly over the entire coating surface. Then, it is cured at 25-30°C for 24-36 hours until fully cured, resulting in an epoxy resin sealant layer covering the surface of the metal functional layer.

[0030] Preferably, the epoxy resin sealant is a two-component epoxy resin sealant, composed of an epoxy resin matrix and an amine curing agent, wherein the mass ratio of the amine curing agent to the epoxy resin matrix is ​​60:100 to 80:100, that is, the curing agent content is not less than 60% of the mass of the epoxy resin matrix; the coating thickness of the sealant is 30 to 40 μm. The epoxy resin sealant layer blocks the permeation path of corrosive media to the substrate-coating interface by sealing the interconnected pores on the surface and inside the metal functional layer. It works synergistically with the underlying metal functional layer to solve the problem of coupled damage from mud and sand erosion and electrochemical corrosion, further improving the overall corrosion resistance of the composite coating.

[0031] VII. Preparation method and performance testing of corrosion-resistant composite reinforced coatings In summary, the method for preparing the corrosion-resistant composite reinforced coating provided by this invention includes the following steps: fixing the filament using a roller feeding device, setting the corresponding spraying parameters on a supersonic arc spraying control device, and then spraying to form a metallic functional layer on the damaged area of ​​the component to be protected. Subsequently, an epoxy resin sealant is coated onto the surface of the metallic functional layer and cured to obtain a double-layer composite corrosion-resistant reinforced coating consisting of the metallic functional layer and the epoxy resin sealant. This method can prepare a composite coating with high hardness, wear resistance, and corrosion resistance, and allows for precise control of coating thickness and performance. The spraying method is simple, suitable for on-site repair of large flow components, and can complete the preparation of the corrosion-resistant reinforced coating with high deposition efficiency and low equipment cost.

[0032] The performance testing of the prepared corrosion-resistant composite reinforced coating preferably includes coating porosity determination, microhardness testing, bonding strength testing, neutral salt spray testing, and electrochemical testing. The bonding strength test is conducted according to GB / T8642-2022 standard, with a tensile rate of 2 mm / min; the neutral salt spray test is conducted according to GB / T 10125-2021 standard. The tests show that the composite coating prepared by this invention has a porosity of no more than 3%, a bonding strength of no less than 50 MPa, and shows no rust after 240 hours of neutral salt spray testing.

[0033] Based on the above scheme, this invention prepares a functional metal layer using supersonic arc spraying technology, combined with localized precise sandblasting pretreatment and epoxy resin sealing treatment, achieving a synergistic improvement in the coating's mechanical properties and corrosion resistance. Compared with commonly used industrial arc-sprayed coatings, the coating obtained by this invention exhibits a 43%–100% increase in bonding strength and a 50%–63% reduction in porosity. This method is simple, requires no complex equipment, and has a construction cost that is only about one-quarter of that of plasma spraying. Furthermore, it has no stringent requirements for the construction environment and can complete the repair of large flow components on-site. Based on accelerated testing data, the coating obtained by this invention has a service life of 10–15 years in a water environment containing silt and sediment, which is 2–3 times that of ordinary arc-sprayed coatings and 5–10 times that of epoxy organic coatings. It is particularly suitable for surface strengthening and repair of flow components such as turbine runners and guide vanes in hydroelectric power stations.

[0034] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. This invention selects any one of the following as the spraying wire on the pre-treated damaged area: high-chromium iron-based flux-cored wire, chromium-nickel iron-based alloy wire, or nickel-aluminum alloy solid wire. The arc working voltage, arc working current, spraying distance, compressed air pressure, and wire feeding speed of the supersonic arc spraying process are limited to a specific synergistic range. The metal wire melts at the high temperature of the arc and is accelerated by compressed air to form supersonic atomized droplets with an average speed of 350–550 m / s. When the droplets impact the substrate surface, they undergo intense plastic deformation and fully fill the microscopic anchor patterns on the substrate surface. Subsequently, they rapidly solidify to form a dense metal functional layer. The resulting metal functional layer has a porosity of no more than 3% and a bonding strength of no less than 50 MPa. It shows no rust after a 240-hour neutral salt spray test. Compared to ordinary arc-sprayed coatings, the bonding strength is increased by 43%–100%, and the porosity is reduced by 50%–63%, achieving a synergistic improvement in wear resistance and corrosion resistance. When high-chromium iron-based flux-cored wire is used as the spraying wire, the microhardness of the metal functional layer can reach up to 1375 HV, which is a significant improvement compared to the 600-800 HV hardness of coatings prepared by conventional FeCrBSi arc spraying wire. This is because the wire used in this invention has extremely low Ni content and high Cr and B content. Under the intense impact of supersonic droplets, a large number of high-hardness CrB phase and Fe2B phase are formed inside the coating. In contrast, the composition design goal of conventional FeCrBSi wire is to obtain good spreadability at a lower droplet velocity. The strengthening mechanisms of the two are fundamentally different.

[0035] 2. Under the conditions of an arc working voltage of 34-40V and an arc working current of 210-240A, and with a compressed air pressure of 0.7-1.0MPa, this invention creates a synergistic strengthening effect between the wire composition and the supersonic arc spraying process parameters. Within this parameter range, the droplet velocity is in the optimal range of 400-450m / s. When the droplets impact the substrate, they undergo sufficient plastic deformation, forming a dense layered stacked structure. The coating porosity can be reduced by more than 60%, and the bonding strength can be increased by more than 80%. At the same time, the Cr element in the coating is uniformly distributed, forming a continuous chromium oxide protective film, which greatly improves the corrosion resistance. When any process parameter deviates from the range defined by this invention, the coating performance will deteriorate significantly. This indicates that there is a critical relationship of mutual constraint and synergistic effect among the process parameters, rather than a simple superposition optimization of conventional process parameters.

[0036] 3. In this invention, an epoxy resin sealant is brushed onto the surface of the metal functional layer to form an epoxy resin sealing layer covering the surface of the metal functional layer. Through the sealing effect of the sealant on the residual pores of the metal functional layer, the penetration path of the corrosive medium to the interface between the substrate and the coating is further blocked. Together with the metal functional layer, a double-layer composite protective structure is formed, which further improves the overall corrosion resistance of the composite coating compared with the single metal functional layer without sealing, and increases the electrochemical impedance by 1 to 2 orders of magnitude.

[0037] 4. This invention adopts a localized and precise repair method. It uses high-temperature resistant tape to cover the undamaged area around the damaged area on the surface of the component to be protected. Only the exposed damaged area is subjected to sandblasting and rust removal pretreatment and supersonic arc spraying repair. This avoids secondary damage to the surrounding intact coating caused by traditional overall sandblasting or mechanical grinding methods. At the same time, it can directly repair localized shallow wear and corrosion areas without the need for welding. The heat-affected zone is small and the repair efficiency is high.

[0038] 5. This invention can select appropriate wires from high-chromium iron-based flux-cored wires, chromium-nickel iron-based alloy wires, and nickel-aluminum alloy solid wires to prepare metal functional layers according to the actual operating performance requirements of the flow-through components. Each wire can independently achieve the technical effects of this invention and form differentiated performance gradients: among them, the coating prepared by high-chromium iron-based flux-cored wires has the highest hardness and is suitable for operating conditions with high wear resistance requirements; the coating prepared by chromium-nickel iron-based alloy wires has the best comprehensive performance of hardness and corrosion resistance and is suitable for operating conditions with both high wear resistance and corrosion resistance requirements; the coating prepared by nickel-aluminum alloy solid wires has the lowest porosity and the best corrosion resistance and is suitable for operating conditions with high corrosion resistance requirements, thereby meeting the differentiated protection needs of different flow-through components under different service environments.

[0039] 6. The preparation method of this invention is simple and requires no complex equipment. The construction cost is only about 1 / 4 of that of plasma spraying, and it has no harsh requirements on the construction environment. Large flow components can be repaired on-site. According to accelerated test data, the service life of the composite reinforced coating prepared by this invention in a water environment with silt and sand can reach 10 to 15 years, which is 2 to 3 times that of ordinary arc spraying coatings and 5 to 10 times that of epoxy organic coatings. It is particularly suitable for surface strengthening and repair of flow components such as turbine runners, guide vanes, and pump impellers in hydropower stations. Attached Figure Description

[0040] Figure 1 This is a diagram showing the friction coefficient of the coating in an embodiment of the present invention; Figure 2 This is a topographic image of the coating wear marks in an embodiment of the present invention; Figure 3 This is a diagram showing the bonding strength of coatings with different film thicknesses in an embodiment of the present invention; Figure 4The impedance diagram and Tafel curve of the uncoated sealant coating in this embodiment of the invention are shown. In the figure, (a) is the impedance diagram of the uncoated coating and (b) is the corresponding Tafel curve. Figure 5 The impedance diagram and Tafel curve of the coating after applying the sealant are shown in the embodiments of the present invention. In the figure, (a) is the impedance diagram of the coating after the sealant is applied, and (b) is the corresponding Tafel curve. Figure 6 This is a neutral salt spray corrosion image of an embodiment of the present invention without a sealant coating. Figure 7 This is a neutral salt spray corrosion image of the coating after applying a sealant in an embodiment of the present invention. Detailed Implementation

[0041] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that the following embodiments are only used to explain the present invention and are not intended to limit the scope of protection of the present invention.

[0042] Example 1 In this embodiment, the coating performance testing method is as follows: Friction and wear performance testing was conducted using an RTEC friction and wear testing machine. Under a load of 15 N and a friction time of 20 min, the friction performance of multiple groups of different coatings was evaluated. The wear resistance of each coating was assessed by comparing the friction coefficients and three-dimensional morphology of the friction surfaces. The relevant friction coefficients and wear track morphologies are shown below. Figure 1 , Figure 2 As shown.

[0043] The coating bond strength was tested using the tensile method: A substrate of the same material (e.g., 316L stainless steel) with a diameter of φ25mm × 10mm was used. After spraying a coating of a certain thickness onto the surface to be coated according to the corresponding process, a high-strength epoxy structural adhesive with a tensile strength of not less than 70MPa was used to coaxially bond it to a blank dual specimen of the same size. The specimen was cured at 25℃ for 24 hours, and then subjected to tensile testing at a constant rate of 2mm / min on a universal testing machine. Three parallel samples were tested in each group, and only the specimen where fracture occurred at the coating interface was taken. The bond strength of the corresponding coating was calculated based on the ratio of the maximum fracture load to the bonded area. The bond strength of coatings with different film thicknesses is shown below. Figure 3 As shown.

[0044] The electrochemical test used a standard three-electrode system, with the following key parameters: the working electrode was the coating to be tested, with an exposed area of ​​1 cm². 2The reference electrode was a saturated calomel electrode; the auxiliary electrode was a platinum sheet; the electrolyte was a 3.5% NaCl aqueous solution; the sample was immersed in the electrolyte for 30 minutes before testing until the open circuit potential (OCP) stabilized; the electrochemical impedance spectroscopy (EIS) test frequency range was 10... -2 ~10 5 The frequency was Hz, the AC amplitude was 10mV; the Tafel polarization curve test scan range was ±250mV relative to OCP, the scan rate was 1mV / s; the test environment temperature was 25±2℃.

[0045] In this embodiment, a high-chromium iron-based flux-cored wire A with a diameter of 2.0 mm and a length of 4000 mm was selected as the coating raw material. Before spraying, the intact area around the damaged area was covered with high-temperature resistant silicone rubber tape. Quartz sand with a particle size of 1.0 mm was used for sandblasting to remove rust at a pressure of 0.55 MPa. After rust removal, the surface roughness Ra of the substrate was 6.5 μm, and there was no oil or rust. Subsequently, the wire and substrate material were respectively mounted on the wire feeding rollers and spraying fixtures at both ends of the spray gun for the next step of supersonic arc spraying.

[0046] In this embodiment, a turbine guide vane (316L stainless steel) with an area of ​​approximately 0.5 m² was selected as the substrate. A corrosion-resistant composite reinforced coating was prepared using an SX-1000 supersonic arc spraying device. The main parameters of the spraying process were: arc working voltage 37V, arc working current 240A, spraying distance 10cm, compressed air pressure 0.8MPa, spray gun moving speed 7mm / s, wire feed speed 15m / min, and continuous spraying for 15s without interruption. After spraying and allowing the metal functional layer to cool to room temperature, an epoxy resin sealant was applied and cured using the aforementioned method to form an epoxy resin sealing layer. In this embodiment, the mass ratio of amine curing agent to epoxy resin matrix in the epoxy resin sealant was 70:100. Curing was performed at 25°C for 24 hours, and the thickness of the cured epoxy resin sealing layer was approximately 35μm.

[0047] The metal functional layer prepared in this embodiment has a thickness of approximately 280 μm, a bluish-gray surface, a dense surface structure, a porosity of approximately 2.0%, a microhardness of 1375.0 HV, and a bonding strength of 58 MPa. Electrochemical testing results show that coating A without the sealing agent has a low impedance in the EIS Nyquist plot (impedance diagram); after applying the sealing agent, the impedance of coating A increases to 10. 4 Ω·cm 2This indicates a significant improvement in its corrosion resistance. The Tafel curve of coating A shows a lower corrosion potential and a higher corrosion current, reflecting that coating A has generally lower corrosion resistance. However, after brushing with the sealant, its corrosion rate is significantly reduced. Similarly, the 240-hour neutral salt spray corrosion test results show that the corrosion resistance of coating A is significantly improved after brushing with the sealant. The electrochemical test results before and after sealing of different coatings are as follows: Figure 4 , Figure 5 As shown, the results of neutral salt spray corrosion are as follows: Figure 6 , Figure 7 As shown.

[0048] The results of this embodiment show that coating A has extremely high hardness but average corrosion resistance, making it suitable for working conditions requiring high hardness and wear resistance, but where corrosion resistance requirements are not particularly high.

[0049] Example 2 In this embodiment, a high-chromium iron-based flux-cored wire B with a diameter of 2.0 mm and a length of 2000 mm was selected as the coating raw material. Before spraying, the intact area around the damaged area was covered with high-temperature resistant silicone rubber tape. Quartz sand with a particle size of 1.0 mm was used for sandblasting to remove rust at a pressure of 0.55 MPa. After rust removal, the surface roughness Ra of the substrate was 6.5 μm, and there was no oil or rust. Subsequently, the wire and substrate material were respectively mounted on the wire feeding rollers and spraying fixtures at both ends of the spray gun for the next step of supersonic arc spraying.

[0050] In this embodiment, a turbine guide vane (316L stainless steel) with an area of ​​approximately 0.5 m² was selected as the substrate. A corrosion-resistant composite reinforced coating was prepared using an SX-1000 supersonic arc spraying device. The main parameters of the spraying process were: arc working voltage 40V, arc working current 240A, spraying distance 20cm, compressed air pressure 0.8MPa, spray gun moving speed 8.5mm / s, wire feed speed 10m / min, and continuous spraying for 10 seconds without interruption. After spraying and allowing the metal functional layer to cool to room temperature, an epoxy resin sealant was brushed on and cured according to the aforementioned method to form an epoxy resin sealing layer. In this embodiment, the mass ratio of amine curing agent to epoxy resin matrix in the epoxy resin sealant was 70:100. Curing was performed at 25°C for 24 hours, and the thickness of the cured epoxy resin sealing layer was approximately 35μm.

[0051] The metallic functional layer prepared in this embodiment has a thickness of approximately 250 μm, a white-gray surface, a dense surface structure, a porosity of approximately 1.9%, a microhardness of 1113.2 HV, and a bonding strength of 55 MPa. Electrochemical testing results show that the uncoated coating B has a relatively large radius of curvature (semicircle) in the EIS Nyquist plot (impedance diagram), approximately 10. 2 Ω·cm 2This indicates that coating B has a high impedance; after applying the sealant, the impedance of coating B further increases to 10. 5 Ω·cm 2 The corresponding charge transfer resistance is relatively large, indirectly reflecting a significant improvement in its corrosion resistance. The Tafel curve of coating B shows that it has a high corrosion potential and extremely low corrosion current (10⁻⁶). -9 A) directly reflects that the corrosion rate of coating B is lower, and the corrosion rate is further reduced after brushing with a sealant. Similarly, the results of the 240h neutral salt spray corrosion test show that the corrosion resistance of coating B is significantly improved after brushing with a sealant.

[0052] The results of this embodiment show that coating B has excellent hardness and corrosion resistance, and its overall performance is optimal, which can meet the dual requirements of wear resistance and corrosion resistance.

[0053] Example 3 In this embodiment, a solid nickel-aluminum alloy wire E with a diameter of 1.5 mm and a length of 2000 mm was selected as the coating raw material. Before spraying, the intact area around the damaged area was covered with high-temperature resistant silicone rubber tape. Quartz sand with a particle size of 1.0 mm was used for sandblasting to remove rust at a pressure of 0.55 MPa. After rust removal, the surface roughness Ra of the substrate was 6.5 μm, and there was no oil or rust. Subsequently, the wire and substrate material were respectively mounted on the wire feeding rollers and spraying fixtures at both ends of the spray gun for the next step of supersonic arc spraying.

[0054] In this embodiment, a turbine guide vane (316L stainless steel) with an area of ​​approximately 0.5 m² was selected as the substrate. A corrosion-resistant composite reinforced coating was prepared using an SX-1000 supersonic arc spraying device. The main parameters of the spraying process were: arc working voltage 34V, arc working current 210A, spraying distance 10cm, compressed air pressure 0.8MPa, spray gun moving speed 9mm / s, wire feed speed 8m / min, and continuous spraying for 8 seconds without interruption. After spraying and allowing the metal functional layer to cool to room temperature, an epoxy resin sealant was applied and cured using the aforementioned method to form an epoxy resin sealing layer. In this embodiment, the mass ratio of amine curing agent to epoxy resin matrix in the epoxy resin sealant was 70:100. Curing was performed at 25°C for 24 hours, resulting in a epoxy resin sealing layer thickness of approximately 35 μm after curing.

[0055] The metallic functional layer prepared in this embodiment has a thickness of approximately 200 μm, a yellowish-gray surface, a dense surface structure, a porosity of approximately 0.4%, a microhardness of 320 HV, and a bonding strength of 52 MPa. Electrochemical testing results show that the coating E without the sealing agent exhibits the largest radius of curvature (semicircle) in the EIS Nyquist plot (impedance plot), approximately 10. 3 Ω·cm 2This indicates that coating E has the highest impedance; after applying the sealant, the impedance of coating E further increases to 10. 6 Ω·cm 2 The corresponding charge transfer resistance is extremely high, indirectly reflecting its optimal anti-corrosion effect. The Tafel curve of coating E also shows that it has the highest corrosion potential (-0.41V) and the lowest corrosion current (10V). -7 A) directly reflects the slow corrosion rate of coating E; after brushing with a sealant, the corrosion potential becomes -0.32V, and the corrosion current is as low as 10. -9 A. The corrosion rate further decreased. Similarly, the results of the 240h neutral salt spray corrosion test showed that coating E had no obvious rust areas on its surface, regardless of whether a sealant was applied.

[0056] The results of this embodiment show that coating E has the best corrosion resistance, but its hardness is low and its wear resistance is average. It is suitable for working environments with high requirements for corrosion resistance.

[0057] Based on the above scheme, this invention forms a double-layer composite coating in the locally damaged area of ​​the flow-through component through local sandblasting pretreatment, supersonic arc spraying, and epoxy resin sealing treatment. The porosity of the metal functional layers obtained in Examples 1-3 is 0.4%–2.0%, and the bonding strength is 52 MPa–58 MPa. The electrochemical impedance after sealing treatment is higher than that of the unsealed coating. The results of the 240-hour neutral salt spray test are shown in […]. Figure 6 and Figure 7 The sealing agent parameters in Examples 1 to 3 above are the same, and the pore-sealing improvement of the sealing layer itself is consistent. However, due to the essential differences in the intrinsic corrosion resistance and porosity of the underlying metal functional layer, the total impedance of the final composite reinforced coating shows the phenomenon of Example 3 > Example 2 > Example 1. The aforementioned differences are not related to the sealing agent itself, but are determined by the material properties of the metal functional layer.

[0058] This invention can select different types of wire materials and corresponding supersonic arc spraying process parameters according to the actual working conditions of the flow-through components, and prepare a corrosion-resistant composite reinforced coating that has both excellent wear resistance and corrosion resistance.

Claims

1. A method for preparing a corrosion-resistant composite reinforced coating, characterized in that: Includes the following steps: The undamaged area surrounding the locally damaged area of ​​the protective component is shielded, and the locally damaged area is pre-treated by sandblasting to remove rust. Choose any one of the following as the coating wire: high chromium iron-based core wire, chromium nickel iron-based alloy wire, and nickel aluminum alloy solid wire; and use supersonic arc spraying process to prepare a metal functional layer in the localized damaged area. After the metal functional layer cools down, an epoxy resin sealant is brushed onto the surface of the metal functional layer and cured to form an epoxy resin sealing layer, resulting in a double-layer composite coating consisting of the metal functional layer and the epoxy resin sealing layer.

2. The preparation method according to claim 1, characterized in that: The roughness Ra of the pretreated surface obtained after the sandblasting rust removal pretreatment is 5μm to 8μm, and there is no visible rust or oil on the pretreated surface.

3. The preparation method according to claim 2, characterized in that: The chemical composition of the high-chromium iron-based core wire, by mass fraction, is: Cr 30%–40%, Ni < 0.1%, Mn < 1%, B 3%–5%, Si < 1%, C ≤ 2%, with the balance being Fe; or, Cr 18%–22%, Ni 9%–11%, Mn 1%–2%, B 3%–6%, Si 1%–2%, with the balance being Fe; The chemical composition of the chromium-nickel-iron-based alloy wire, by mass fraction, is: Cr 17%–19%, Ni 8%–11%, Mn 2%, Si 1%, C 0.07%, with the balance being Fe; or, Cr 12.5%, Ni 4.7%, Mn 0.7%, Si 0.4%, C 0.03%, Mo 0.8%, with the balance being Fe. The chemical composition of the nickel-aluminum alloy solid wire, by mass fraction, is: Ni 94.5%~95.5%, Al 4.5%~5.5%, Mn<0.3%, Si<0.5%, Fe<0.3%.

4. The preparation method according to claim 3, characterized in that: The process parameters for preparing the functional metal layer using supersonic arc spraying include: arc working voltage of 34V to 40V, arc working current of 210A to 240A, spraying distance of 10cm to 20cm, compressed air pressure of 0.7MPa to 1.0MPa, and wire feeding speed of 8m / min to 15m / min.

5. The preparation method according to claim 4, characterized in that: In the process of preparing the metal functional layer using supersonic arc spraying, the moving speed of the spray gun is 5 mm / s to 15 mm / s, the spraying time is 5 s to 15 s, and the angle between the spray gun and the surface of the locally damaged area is 90°.

6. The preparation method according to claim 5, characterized in that: The thickness of the metal functional layer is 200μm to 280μm.

7. The preparation method according to claim 6, characterized in that: The epoxy resin sealant is a two-component epoxy resin sealant composed of an epoxy resin matrix and an amine curing agent, wherein the mass ratio of the amine curing agent to the epoxy resin matrix is ​​(60-80):100; and the thickness of the epoxy resin sealing layer is 30μm-40μm.

8. The preparation method according to claim 7, characterized in that: The porosity of the prepared double-layer composite coating is not greater than 3%, the bonding strength between the metal functional layer and the substrate is not less than 50 MPa, and the double-layer composite coating shows no rust after 240 h of neutral salt spray test.

9. A corrosion-resistant composite reinforced coating, characterized in that: The corrosion-resistant composite reinforced coating is prepared using the preparation method described in any one of claims 1 to 8.

10. The application of the corrosion-resistant composite reinforced coating of claim 9 in the surface protection of flow-through components, characterized in that: The flow-through components are turbine runners, turbine guide vanes, or pump impellers.

Citation Information

Patent Citations

  • Antiseptic wearable coat and coating method thereof

    CN101191225B

  • Cored wire for electric arc spraying of amorphous and nano-crystalline anti-cavitation coating layer

    CN102181813A

  • Composite repair covering for cavitation of flow passage part of hydraulic machine, and preparation method thereof