Long-life h13 die-casting mold plasma nitriding process and die prepared thereby
By performing nitriding in a vacuum environment using plasma nitriding technology, the problems of long cycle and uneven nitriding in traditional gas nitriding treatment are solved, thereby extending mold life and improving production efficiency. It is suitable for efficient nitriding treatment of molds with complex shapes.
Patent Information
- Application Number
- CN202611231738.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing gas nitriding processes have long cycles, uneven nitriding in complex cavities and deep holes, and the nitrided layer is prone to loosening or oxidation, resulting in short mold life and low production efficiency.
The plasma nitriding process is adopted, including pretreatment, ion etching, nitriding and cooling steps. Argon ion bombardment and nitrogen atmosphere nitriding are used in a vacuum environment to form a dense nitriding layer. The uniformity of nitriding is ensured by combining cathode turntable rotation and active screen ion nitriding.
It significantly shortens nitriding time, improves nitriding efficiency, forms a dense nitrided layer, significantly extends mold life, reduces production costs, is suitable for high-precision and complex-shaped molds, and improves the quality of die-cast products.
Smart Images

Figure CN123152984A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of plasma nitriding technology for H13 type die casting molds, and particularly to a long-life plasma nitriding process for H13 type die casting molds and the molds prepared therefrom. Background Technology
[0002] H13 die steel (also known as 4Cr5MoSiV1) is a hot work die steel that conforms to national standards. It is mainly used to manufacture hot forging dies, hot extrusion dies, and aluminum-copper alloy die casting dies that withstand high impact loads. This steel uses chromium, molybdenum, and vanadium as the main alloying elements, with a carbon content of 0.32%~0.45%. The purity is improved through electroslag remelting technology, resulting in high hardenability, resistance to hot cracking, and wear resistance.
[0003] During the die casting process, the mold cavity surface is repeatedly subjected to the scouring of high-temperature molten aluminum alloy and the cyclic load of rapid cooling and heating, which easily leads to thermal fatigue cracks, sticking and erosion wear, resulting in a short service life of the mold.
[0004] To improve mold life, gas nitriding is commonly used in industry for surface strengthening. However, this process takes 20-50 hours, and the concentration of active nitrogen atoms produced by ammonia decomposition is greatly affected by the uniformity of atmosphere flow. In particular, the nitriding effect is significantly worsened in complex cavities, deep holes, and narrow gaps, which can easily lead to problems such as uneven nitrided layer thickness, looseness, or surface oxidation. At the same time, prolonged high-temperature heat preservation leads to large thermal deformation of the mold and coarsening of the matrix structure, which seriously restricts the efficiency of die casting production and the overall service performance of the mold. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a long-life H13 type die-casting mold plasma nitriding process and the mold prepared therefrom, which solves the technical problems of long gas nitriding treatment cycles, uneven nitriding in complex cavities and deep holes, and easy occurrence of loose nitrided layers and surface oxidation.
[0006] The present invention is further configured such that the above-mentioned technical objective of the present invention is achieved through the following technical solution:
[0007] A long-life H13 type die-casting mold plasma nitriding process includes the following steps:
[0008] Step S1, Pretreatment: Clean, polish and dry the surface of the H13 type die casting mold;
[0009] Step S2, Loading and Vacuuming: Fix the pre-treated mold on the cathode turntable inside the vacuum furnace to insulate the workpiece from the furnace anode, evacuate to a background vacuum of ≤1×10⁻³Pa, and heat the furnace body;
[0010] Step S3, Ion Etching: Argon gas is introduced into the furnace. Under the low pressure environment of 0.2-1.0 Pa in the furnace, argon ions are used to bombard the surface of the mold to remove the residual oxide layer and activate the surface.
[0011] Step S4, Nitriding treatment: A nitrogen-containing atmosphere is introduced into the furnace, and plasma nitriding treatment is carried out at a temperature of 500-600℃ and a furnace pressure of 0.2-1.0 Pa to form a nitrided layer on the mold surface.
[0012] Step S5, Cooling and Unloading: After cooling the mold in a vacuum environment, unload it from the oven.
[0013] The present invention is further configured as follows: in step S1, the cleaning is performed by ultrasonic cleaning with acetone or anhydrous ethanol for 20-30 minutes; the polishing is performed by polishing with SiC sandpaper of 240 mesh to 2000 mesh in stages; for the polished mold, Cr2O3 polishing powder is used to polish it to a mirror surface; the drying temperature is ≤100℃.
[0014] The present invention is further configured such that: in step S2, the temperature of the heating furnace body is 300-600℃, so as to remove the volatile impurities remaining in the furnace.
[0015] The present invention is further configured such that the process parameters for ion etching in step S3 are: furnace pressure 0.2-1.0 Pa, argon flow rate 180-200 mL / min, workpiece negative bias voltage 300-500 V, arc target current 80-85 A, and etching time 30-60 minutes; the purity of the argon gas is ≥99.99%; and the arc target is a Ti target.
[0016] The present invention is further configured such that: in step S4, the nitrogen-containing atmosphere includes nitrogen and hydrogen, and the flow ratio of nitrogen to hydrogen is 1:1; the process parameters for nitriding treatment are: furnace pressure 0.2-1.0 Pa, nitrogen flow rate 25-50 mL / min, hydrogen flow rate 25-50 mL / min, workpiece negative bias voltage 300-500 V, pulse frequency 10-20 kHz, duty cycle 0.8-1.0, arc target current 80-85 A, and nitriding time 60-120 minutes; the purity of both nitrogen and hydrogen is ≥99.99%.
[0017] The present invention is further configured such that: in step S4, argon gas with a purity ≥99.99% is introduced to adjust the gas pressure inside the furnace, and the argon gas flow rate is 80-120 mL / min.
[0018] The present invention is further configured such that: in step S4, a pulse power supply is used to power the workpiece and the uniformity of nitriding on the mold surface is ensured by rotating the workpiece, and the rotation speed of the cathode turntable is 5 to 10 rpm.
[0019] The present invention is further configured such that: in step S4, an active screen ion nitriding method is used to apply a cathode potential to a metal screen surrounding the workpiece, and the workpiece is at a floating potential or an auxiliary bias voltage is applied to avoid the corner effect of complex shaped molds.
[0020] The present invention is further configured such that: in step S5, the vacuum degree inside the furnace is maintained at ≤1×10⁻³Pa during the cooling process, the furnace body circulating cooling water system is turned on for cooling, the cooling time is 60~120 minutes, and the mold temperature is ≤50℃ when it exits the furnace.
[0021] An H13 type die-casting mold prepared by plasma nitriding process, wherein the mold surface hardness is 1000-1300HV, the nitriding layer thickness is 15-35μm, and the phase composition of the nitriding layer includes one or more of CrN, MoN and VN, and may further include TiN.
[0022] Compared to the beneficial effects achieved by existing technologies:
[0023] First, this invention uses highly active nitrogen ions generated by glow discharge to directly bombard the mold surface, accelerating the diffusion and penetration of nitrogen atoms. The nitriding and heat preservation time is only 1-2 hours, while traditional gas nitriding requires 20-50 hours, improving efficiency by more than 10 times. This significantly shortens the mold turnaround time and improves production efficiency, making it particularly suitable for large-scale, high-cycle die-casting production lines.
[0024] Secondly, this invention performs plasma nitriding in a vacuum environment, avoiding the problems of loose nitrided layers or oxidation caused by uneven ammonia decomposition in traditional gas nitriding. The resulting nitrided layer has a dense structure and a surface hardness of 1000-1300 HV with a gentle hardness gradient, effectively reducing the risk of sudden hardness changes and peeling between the nitrided layer and the substrate. The nitrided layer contains hard phases such as TiN, CrN, MoN, and VN, which can resist repeated scouring and wear from the high-temperature molten aluminum alloy during die casting, significantly extending the mold's service life. At the same time, the low coefficient of friction of the nitrided layer effectively reduces the sticking phenomenon between the die casting and the cavity surface, lowers the demolding force, avoids surface scratches or dimensional deviations caused by sticking, and improves the surface quality and density of the die-cast products.
[0025] Third, this invention performs nitriding treatment at a relatively low temperature of 500-600℃ and uses direct heating via glow discharge, combined with the rotation of the cathode turntable, resulting in uniform temperature distribution and minimal thermal deformation of the mold. This maintains the dimensional accuracy of the cavity and reduces the workload of subsequent finishing processes. In contrast, traditional gas nitriding treatment involves higher temperatures and uneven heating, which can easily lead to mold deformation and require additional straightening processes.
[0026] Fourth, the power consumption of this invention is only 1 / 2 to 1 / 5 of that of traditional gas nitriding, and there is no need to use a large amount of ammonia. The nitriding atmosphere uses high-purity nitrogen and hydrogen, and there are no harmful waste gas emissions during the process. The main emission is hydrogen, which can be safely discharged through a vacuum pump. The vacuum environment also avoids oxidation pollution, further ensuring the surface quality of the workpiece.
[0027] Fifth, it has a wide range of applications and is compatible with complex working conditions. This invention ensures uniform nitriding by rotating the cathode turntable, and can process workpieces of various shapes and sizes. For molds with complex cavities, deep holes, narrow slits, etc., an active screen ion nitriding method can be used, applying the cathode potential to the metal screen surrounding the workpiece, fundamentally eliminating the edge effect and ensuring uniform nitriding in all parts of the complex geometric mold, meeting the high precision and high complexity requirements of molds in industries such as automotive, IT, and packaging.
[0028] Sixth, the H13 type die-casting molds treated with the process of this invention exhibit significantly improved thermal fatigue resistance. The overall service life of the molds is 1-2 times longer than untreated molds or those treated with traditional gas nitriding, significantly reducing maintenance costs and replacement frequency, bringing considerable economic benefits to die-casting companies. This process is particularly effective for high-pressure die-casting applications such as automotive wheel hubs, engine blocks, and gearbox housings. Attached Figure Description
[0029] Figure 1 This is a flowchart illustrating the process steps of an embodiment of the present invention. Detailed Implementation
[0030] The technical solutions of the present invention will be further described below with reference to the accompanying drawings and embodiments.
[0031] Example 1:
[0032] Reference Figure 1 This invention addresses the problems of thermal fatigue cracks, sticking, and surface wear that easily occur in H13 type die casting molds under repeated scouring by high-temperature molten aluminum alloy and rapid cooling and heating conditions. It provides a plasma nitriding surface strengthening process.
[0033] like Figure 1As shown, the H13 type die-casting mold undergoes pretreatment first, including cleaning, polishing, and drying. Cleaning involves ultrasonic cleaning with acetone or anhydrous ethanol for 20-30 minutes. Polishing is performed using SiC sandpaper ranging from 240 to 2000 grit, sequentially using 240, 400, 600, 800, 1000, 1200, 1500, and 2000 grit sandpaper, with each polishing direction perpendicular to the previous one to eliminate scratches left by the previous one. For polished molds, Cr2O3 polishing powder is used to polish to a mirror finish with a surface roughness Ra ≤ 0.05 μm. The drying temperature is ≤ 100℃, and the drying time is 30-60 minutes to avoid excessively high temperatures causing tempering and softening of the mold surface.
[0034] like Figure 1 As shown, the pretreated mold is then fixed on the cathode turntable inside the vacuum furnace, ensuring the workpiece is insulated from the furnace anode. After placement, the vacuum furnace is evacuated using a combination of mechanical and molecular pumps until the background vacuum level is ≤1×10⁻³Pa, and the furnace body is heated. The furnace body is heated to 300-600℃ and held for 30-60 minutes to remove residual volatile impurities and moisture adsorbed on the furnace walls, ensuring the purity of the subsequent nitriding atmosphere.
[0035] like Figure 1 As shown, further ion etching is performed by introducing argon gas into the furnace. Under a low-pressure environment of 0.2-1.0 Pa, argon ions bombard the mold surface to remove residual oxide layers and activate the surface. The argon gas flow rate is 180-200 mL / min, the workpiece negative bias voltage is 300-500 V, the arc target current is 80-85 A, and the etching time is 30-60 minutes. The purity of the argon gas is ≥99.99%, and the arc target is a Ti target. During the etching process, the Ti atoms generated by sputtering from the Ti target help to further clean and activate the substrate surface, promoting the penetration of nitrogen atoms in the subsequent nitriding stage and the metallurgical bonding between the nitrided layer and the substrate.
[0036] like Figure 1As shown, nitriding is then performed by introducing a nitrogen-containing atmosphere into the furnace and conducting plasma nitriding at a temperature of 500-600℃ and a furnace pressure of 0.2-1.0 Pa to form a nitrided layer on the mold surface. This nitrogen-containing atmosphere consists of nitrogen and hydrogen, with a nitrogen-to-hydrogen flow ratio of 1:1, a nitrogen flow rate of 25-50 mL / min, and a hydrogen flow rate equal to the nitrogen flow rate. The workpiece is subjected to a negative bias voltage of 300-500 V, a pulse frequency of 10-20 kHz, a duty cycle of 0.8-1.0, an arc target current of 80-85 A, and a nitriding time of 60-120 minutes. The purity of both nitrogen and hydrogen is ≥99.99%. Argon gas with a purity ≥99.99% can also be introduced to adjust the furnace pressure, with an argon flow rate of 80-120 mL / min. During nitriding, a pulsed power supply can be used, and the uniformity of nitriding on the mold surface is ensured by rotating the workpiece. The rotation speed of the cathode turntable is 5-10 rpm. The combination of a pulse frequency of 10-20 kHz and a duty cycle of 0.8-1.0 generates periodic high-density ion bombardment on the workpiece surface, ensuring a continuous nitrogen ion injection rate while homogenizing the surface temperature through pulse intervals, preventing localized overheating and coarsening of the nitrided layer. Hydrogen gas plays a reducing and cleaning role during nitriding, promptly removing any trace oxides that may form on the workpiece surface and maintaining a highly active surface state, which is conducive to the continuous penetration of nitrogen atoms. An N2 to H2 flow ratio of 1:1 has been experimentally verified as the optimal ratio, achieving an optimal balance between the hardness and density of the nitrided layer.
[0037] like Figure 1 As shown, the mold is finally cooled under vacuum before being removed from the furnace. During the cooling process, the vacuum level inside the furnace is maintained at ≤1×10⁻³Pa. The furnace's circulating cooling water system is activated for cooling, using programmed temperature control. The cooling time is 60–120 minutes, and the mold temperature upon removal from the furnace is ≤50℃. This vacuum cooling method avoids secondary oxidation caused by the mold coming into contact with air at high temperatures, ensuring that the surface quality of the nitrided layer is not damaged.
[0038] The molds manufactured using the above process have a surface hardness of 1000-1300 HV and a nitrided layer thickness of 15-35 μm. The phase composition of the nitrided layer includes one or more of TiN, CrN, MoN, and VN. The hardness gradient between the nitrided layer and the substrate is gentle, and the width of the transition zone is approximately 2-3 times the thickness of the nitrided layer, effectively reducing abrupt hardness changes between the nitrided layer and the substrate and minimizing the risk of peeling during use.
[0039] According to the applicant's verification, under the conditions of nitriding temperature of 550℃, time of 90min, and bias voltage of 400V, the obtained mold surface hardness is 1180HV, nitrided layer thickness is 28μm, and thermal deformation is <0.008mm, which is the best overall performance.
[0040] The surface hardness was measured using a Vickers hardness tester under a load of 0.98 N; the nitrided layer thickness was measured by metallographic sectioning according to GB / T 11354-2005; and the thermal deformation was characterized by the difference in the three-coordinate measurement of the key dimensions of the mold cavity before and after nitriding.
[0041] Working principle:
[0042] In a vacuum environment, a glow discharge is generated between the workpiece at the cathode and the furnace body at the anode using a pulsed DC power supply, ionizing the nitrogen-containing atmosphere into highly reactive nitrogen and hydrogen ions. Accelerated by an electric field, the nitrogen ions bombard the workpiece surface with energy of hundreds of electron volts, sputtering away residual oxides and simultaneously injecting into the workpiece surface layer to react with alloying elements such as Fe, Cr, Mo, and V in the matrix, forming a dispersed hard nitride phase. Simultaneously, the reducing effect of hydrogen ions effectively inhibits surface oxidation, ensuring the density and uniformity of the nitride layer. The rotation of the cathode turntable ensures that the glow discharge uniformly covers all surfaces of the mold, preventing uneven localized nitriding.
[0043] Example 2:
[0044] The difference from Example 1 is that the nitriding process employs an active screen ion nitriding method. A cathode potential is applied to a metal screen surrounding the workpiece, placing the workpiece at a floating potential or subject to an auxiliary bias voltage. This avoids corner effects in complex-shaped molds. The floating potential and auxiliary bias voltage are standard technical parameters of the ASPN process and are common knowledge to those skilled in the art when implementing ASPN. The metal screen is a cylindrical or irregularly shaped metal mesh screen adapted to the mold cavity shape, made of low-carbon steel or stainless steel. Those skilled in the art can adjust the distance between the metal screen and the workpiece according to the mold size. In active screen mode, glow discharge mainly occurs between the metal screen and the furnace anode. The active nitrogen atoms and ions sputtered on the metal screen surface uniformly reach the workpiece surface via diffusion, fundamentally eliminating the problems of electric field concentration and corner overheating caused by irregular workpiece geometry in traditional DC plasma nitriding. This method is particularly suitable for die-casting molds with features such as deep holes, narrow slits, and complex cavities, such as die-casting molds for automobile engine cylinder blocks and die-casting molds for multi-cavity electronic components. Except for the workpiece biasing method and the setting of the metal screen, the other process parameters such as the temperature, gas pressure, time, gas type and flow rate, pulse frequency, duty cycle, arc target current, and cathode turntable speed of the nitriding treatment are the same as those in Example 1.
[0045] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A plasma nitriding process for long-life H13 type die-casting molds, characterized in that: Includes the following steps: Step S1, Pretreatment: Clean, polish and dry the surface of the H13 type die casting mold; Step S2, Loading and Vacuuming: Fix the pre-treated mold on the cathode turntable inside the vacuum furnace to insulate the workpiece from the furnace anode, evacuate to a background vacuum of ≤1×10⁻³Pa, and heat the furnace body; Step S3, Ion Etching: Argon gas is introduced into the furnace. Under the low pressure environment of 0.2-1.0 Pa in the furnace, argon ions are used to bombard the surface of the mold to remove the residual oxide layer and activate the surface. Step S4, Nitriding treatment: A nitrogen-containing atmosphere is introduced into the furnace, and plasma nitriding treatment is carried out at a temperature of 500-600℃ and a furnace pressure of 0.2-1.0 Pa to form a nitrided layer on the mold surface. Step S5, Cooling and Unloading: After cooling the mold in a vacuum environment, unload it from the oven.
2. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S1, the cleaning is performed by ultrasonic cleaning with acetone or anhydrous ethanol for 20-30 minutes; the polishing is performed by polishing with SiC sandpaper ranging from 240 grit to 2000 grit in stages. For polished molds, further polishing with Cr2O3 polishing powder is used to achieve a mirror finish; The drying temperature is ≤100℃.
3. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S2, the temperature of the furnace body is heated to 300-600℃ to remove residual volatile impurities in the furnace.
4. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: The process parameters for ion etching in step S3 are as follows: furnace pressure 0.2-1.0 Pa, argon flow rate 180-200 mL / min, workpiece negative bias voltage 300-500 V, arc target current 80-85 A, etching time 30-60 minutes; the purity of the argon gas is ≥99.99%; the arc target is a Ti target.
5. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S4, the nitrogen-containing atmosphere includes nitrogen and hydrogen, with a nitrogen to hydrogen flow rate ratio of 1:
1. The process parameters for nitriding are: furnace pressure 0.2-1.0 Pa, nitrogen flow rate 25-50 mL / min, hydrogen flow rate 25-50 mL / min, workpiece negative bias voltage 300-500 V, pulse frequency 10-20 kHz, duty cycle 0.8-1.0, arc target current 80-85 A, and nitriding time 60-120 minutes. The purity of both nitrogen and hydrogen is ≥99.99%.
6. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 5, characterized in that: In step S4, argon gas with a purity of ≥99.99% is introduced to adjust the gas pressure inside the furnace, and the argon gas flow rate is 80-120 mL / min.
7. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S4, a pulse power supply is used to ensure the uniformity of nitriding on the mold surface by rotating the workpiece. The rotation speed of the cathode turntable is 5 to 10 rpm.
8. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S4, an active screen ion nitriding method is used to apply a cathode potential to a metal screen surrounding the workpiece. The workpiece is at a floating potential or an auxiliary bias voltage is applied to avoid the corner effect of complex-shaped molds.
9. The plasma nitriding process for a long-life H13 type die-casting mold according to claim 1, characterized in that: In step S5, the vacuum degree inside the furnace is kept ≤1×10⁻³Pa during the cooling process. The furnace body circulating cooling water system is turned on for cooling. The cooling time is 60 to 120 minutes. The mold temperature is ≤50℃ when the mold is taken out of the furnace.
10. An H13 type die-casting mold obtained by the process described in any one of claims 1 to 9, characterized in that, The surface hardness of the mold is 1000-1300HV, the thickness of the nitriding layer is 15-35μm, and the phase composition of the nitriding layer includes one or more of CrN, MoN and VN, and may further include TiN.