Pvd copper plated substrate, method for manufacturing the same, and display device

By introducing a nickel oxide transition layer with a gradient oxygen content into a copper-plated substrate, the problem of insufficient interfacial bonding performance is solved, and the adhesion and stability of the substrate are improved, making it suitable for high-density packaging and flexible electronic applications.

CN123152995APending Publication Date: 2026-11-24WG TECH(JIANGXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611360025.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing copper-plated substrates have insufficient interfacial bonding performance, especially under conditions such as high-temperature and low-temperature cycling or bending, which easily leads to interfacial stress concentration, affecting bonding stability and reliability.

Method used

A transition layer consisting of first and second nickel oxide layers with different oxygen contents is introduced between the substrate and the copper layer, forming a gradient distribution of oxygen content from high to low from the substrate side to the copper layer side. The first nickel oxide layer provides high-density chemical bonding, while the second nickel oxide layer buffers thermal stress, synergistically improving the bonding stability.

Benefits of technology

It improves the adhesion and stability of copper-plated substrates, reduces the risk of warping, and is suitable for high-density packaging and flexible electronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123152995A_ABST
    Figure CN123152995A_ABST
Patent Text Reader

Abstract

This application discloses a PVD copper-plated substrate, its fabrication method, and a display device. The copper-plated substrate includes a substrate, a transition layer, and a copper layer sequentially stacked. The transition layer includes a first nickel oxide layer and a second nickel oxide layer, with the second nickel oxide layer disposed between the first nickel oxide layer and the copper layer. The oxygen content of the second nickel oxide layer is lower than that of the first nickel oxide layer. By forming a low-stress nickel oxide transition layer with a difference in oxygen content, this application can improve the interfacial bonding performance between the substrate and the copper layer, thereby enhancing the structural stability and reliability of the copper-plated substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of coating technology, specifically to PVD copper-plated substrates and their preparation methods, and display devices. Background Technology

[0002] Copper-plated substrates are fundamental materials in the manufacture of electronic packaging, display panels, and printed circuit boards. They achieve circuit conductivity by forming a conductive copper layer on the substrate surface. With the rapid development of electronic devices towards higher density, higher reliability, and greater flexibility, higher requirements are placed on the film adhesion, bending resistance, and weather resistance of copper-plated substrates.

[0003] To improve the bonding performance between the substrate and the copper layer, some products incorporate a transition layer between them. However, existing transition layers are mostly homogeneous films with a single structure, which cannot simultaneously meet the bonding requirements with both the substrate and the copper layer, easily leading to interfacial stress concentration during use. Especially under conditions such as high-temperature, low-temperature cycling, or bending, the accumulation of internal stress in the film layer may cause and propagate interfacial defects, thereby affecting the bonding stability between the copper layer and the substrate, as well as the reliability of the copper-plated substrate.

[0004] Therefore, it is necessary to improve traditional technologies. Summary of the Invention

[0005] To address the aforementioned technical problems, this application provides a PVD copper-plated substrate with high adhesion and low stress, a method for preparing the substrate, and a display device.

[0006] This application provides the following technical solution:

[0007] The first aspect of this application provides a copper-plated substrate, comprising a substrate, a transition layer and a copper layer stacked sequentially, wherein the transition layer comprises a first nickel oxide layer and a second nickel oxide layer, the second nickel oxide layer being disposed between the first nickel oxide layer and the copper layer, and the oxygen content of the second nickel oxide layer being lower than the oxygen content of the first nickel oxide layer.

[0008] The aforementioned copper-plated substrate, by sequentially stacking a substrate, a transition layer containing first and second nickel oxides with different oxygen contents, and a copper layer, creates a gradient distribution of oxygen content from high to low along the film thickness direction, from the substrate side to the copper layer side. This structural design produces a synergistic effect: the first nickel oxide layer, with its high oxygen content and rich in oxygen vacancies and dangling bonds, can form high-density chemical bonds with the substrate surface, providing a stronger interface anchoring effect and reducing the possibility of interface separation between the copper layer and the substrate under bending, thermal shock, and other conditions; the second nickel oxide layer, with its low oxygen content, can effectively buffer the thermal stress caused by the difference in thermal expansion coefficients between the substrate and the copper layer, making the stress distribution within the film layer more uniform and significantly reducing the risk of substrate warping. The synergistic effect of the two nickel oxide layers results in good overall stress dissipation capacity of the transition layer, effectively improving the bending reliability of the copper-plated substrate.

[0009] The copper-plated substrate of this application has high adhesion, low stress and high stability, and can be applied to different types of substrate systems to meet the application needs of high-density packaging and flexible electronics.

[0010] In some embodiments, the transition layer satisfies one or more of the following conditions:

[0011] (1) The molar ratio of oxygen to nickel in the first nickel oxide layer is 1.1:1 to 1.5:1;

[0012] (2) The molar ratio of oxygen to nickel in the second nickel oxide layer is 0.5:1 to 1.0:1.

[0013] In some embodiments, the transition layer satisfies one or more of the following conditions:

[0014] (1) Thickness is 9 nm to 16 nm;

[0015] (2) The thickness ratio of the first nickel oxide layer to the second nickel oxide layer is 0.5:1 to 2:1;

[0016] (3) Membrane stress ≤ 90 MPa.

[0017] In some embodiments, the copper layer satisfies one or more of the following conditions:

[0018] (1) Thickness is 100 nm to 450 nm;

[0019] (2) Resistivity ≤ 2.6 μΩ·cm;

[0020] (3) The adhesion between the copper layer and the substrate reaches level 5B after cross-cut test.

[0021] In some embodiments, the substrate includes one or more of soda-lime silica glass, borosilicate glass, polyimide film, and polyethylene terephthalate film.

[0022] A second aspect of this application provides a method for preparing a copper-plated substrate, comprising the following steps:

[0023] Using a nickel target as raw material and argon and oxygen as working gases, a transition layer is deposited on at least one surface of a substrate using a first magnetron sputtering process; the deposition process of the transition layer includes a first deposition stage and a second deposition stage performed sequentially, wherein the oxygen flow rate in the second deposition stage is lower than the oxygen flow rate in the first deposition stage;

[0024] A copper layer is prepared on the surface of the transition layer away from the substrate.

[0025] In some embodiments, one or more of the following conditions are met in the first magnetron sputtering process:

[0026] (1) The oxygen flow rate in the first deposition stage is 0.9 sccm to 1.5 sccm;

[0027] (2) The duration of the first deposition stage is 1.5 min to 2.5 min;

[0028] (3) The oxygen flow rate in the second deposition stage is 0.2 sccm ~ 0.6 sccm;

[0029] (4) The second deposition stage lasts for 2.5 min to 3.5 min.

[0030] In some embodiments, one or more of the following conditions are met in the first magnetron sputtering process:

[0031] (1) The working air pressure is 0.3 Pa to 0.5 Pa;

[0032] (2) The first magnetron sputtering process is DC pulse magnetron sputtering;

[0033] (3) The sputtering power is 90 W~130 W, the pulse frequency is 30 kHz~100 kHz, and the duty cycle is 30%~50%;

[0034] (4) The temperature of the substrate is ≤90℃.

[0035] In some embodiments, the copper layer is prepared using a second magnetron sputtering process, wherein the second magnetron sputtering process satisfies one or more of the following conditions:

[0036] (1) Argon is used as the working gas;

[0037] (2) The working air pressure is 0.35 Pa to 0.45 Pa;

[0038] (3) The substrate negative bias voltage is -30 V to -50 V;

[0039] (4) The second magnetron sputtering process is DC pulse magnetron sputtering;

[0040] (5) The sputtering power is 140 W to 220 W, the pulse frequency is 30 kHz to 100 kHz, and the duty cycle is 30% to 50%.

[0041] In some embodiments, after the copper layer is prepared, the following step is further included: isothermal annealing in a vacuum environment.

[0042] Optionally, the isothermal annealing treatment satisfies one or more of the following conditions:

[0043] (1) Vacuum degree ≤ 5×10 -4 Pa;

[0044] (2) The temperature is 90℃~100℃;

[0045] (3) The time is 18 min to 28 min.

[0046] In some embodiments, prior to depositing the transition layer, the method further includes the step of plasma activation treatment of the substrate surface using a radio frequency ion source.

[0047] Optionally, the plasma activation treatment satisfies one or more of the following conditions:

[0048] (1) Argon and oxygen are used as working gases, and the partial pressure ratio of argon to oxygen is 2:1 to 9:1;

[0049] (2) The working air pressure is 0.7 Pa to 0.9 Pa;

[0050] (3) The power of the radio frequency ion source is 180 W to 250 W;

[0051] (4) The substrate negative bias voltage is -40 V to -60 V;

[0052] (5) The time is 4 min to 6 min;

[0053] (6) Substrate temperature ≤ 80℃.

[0054] A third aspect of this application provides a display device comprising the copper-plated substrate described above, or a copper-plated substrate prepared by the aforementioned preparation method. Attached Figure Description

[0055] Figure 1This is a schematic diagram of an overall layered structure of a copper-plated substrate;

[0056] Figure 2 This is a process flow diagram of a method for preparing a copper-plated substrate;

[0057] Figure label:

[0058] 100: Copper-plated substrate;

[0059] 10: Substrate; 20: Transition layer; 30: Copper layer;

[0060] 21: First nickel oxide layer; 22: Second nickel oxide layer. Detailed Implementation

[0061] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings. Preferred embodiments of this application are shown in the drawings. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0062] It should be noted that when a component is said to be "fixed to" another component, it can be directly attached to the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component.

[0063] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0064] The terms "preferred," "more preferably," "better," and "even better" used in this application refer to embodiments of this application that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this application. That is, in this application, "preferred," "more preferably," "better," and "even better" are merely descriptions of implementations or embodiments with better effects, but do not constitute a limitation on the scope of protection of this application.

[0065] In this application, terms such as "further," "even further," and "particularly" are used to describe purposes and indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0066] When a numerical range is disclosed in this application, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Further, when the range refers to an integer, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included. Only a few numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0067] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions, and the new technical solutions formed by the combination also fall within the scope of this application.

[0068] Research has found that the insufficient interfacial bonding performance of traditional copper-plated substrates mainly stems from the lack of an effective interfacial transition structure between the copper layer and the substrate. Due to differences in thermal expansion coefficients, surface energy, and chemical properties between the copper layer and the substrate, direct bonding easily leads to interfacial stress concentration and makes it difficult to form a stable interfacial bond. This results in the copper layer peeling off under external forces such as temperature cycling and mechanical bending. Therefore, it is necessary to introduce a transition structure between the copper layer and the substrate that can regulate interfacial properties to improve the bonding stability of copper-plated substrates.

[0069] See Figure 1 One embodiment of this application provides a copper-plated substrate 100, including a substrate 10, a transition layer 20 and a copper layer 30 stacked sequentially. The transition layer 20 includes a first nickel oxide layer 21 and a second nickel oxide layer 22. The second nickel oxide layer 22 is disposed between the first nickel oxide layer 21 and the copper layer 30, and the oxygen content of the second nickel oxide layer 22 is lower than the oxygen content of the first nickel oxide layer 21.

[0070] The aforementioned copper-plated substrate 100 is constructed by sequentially stacking a substrate 10, a transition layer 20 comprising a first nickel oxide layer 21 and a second nickel oxide layer 22 with varying oxygen contents, and a copper layer 30. This creates a gradient distribution of oxygen content from high to low along the film thickness direction, from the substrate 10 side to the copper layer 30 side. This structural design produces a synergistic effect: the first nickel oxide layer 21, with its high oxygen content and rich in oxygen vacancies and dangling bonds, can form high-density chemical bonds with the surface of the substrate 10, providing a stronger interface anchoring effect and reducing the possibility of interface separation between the copper layer 30 and the substrate 10 under bending, thermal shock, and other conditions; the second nickel oxide layer 22, with its low oxygen content, can effectively buffer the thermal stress caused by the difference in thermal expansion coefficients between the substrate 10 and the copper layer 30, making the stress distribution within the film layer more uniform and significantly reducing the risk of substrate warping. The synergistic effect of the two nickel oxide layers improves the overall stress dissipation capacity of the transition layer 20, effectively enhancing the bending reliability of the copper-plated substrate 100.

[0071] In some embodiments, the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.1:1 to 1.5:1. For example, the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, or any value within the range defined by any two of the above values. It is understood that controlling the molar ratio of oxygen to nickel in the first nickel oxide layer 21 results in a higher oxygen content in the first nickel oxide layer 21, which is beneficial for controlling the bonding force between the first nickel oxide layer 21 and the substrate 10, thereby improving the interfacial bonding performance between the transition layer 20 and the substrate 10.

[0072] In some embodiments, the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 0.5:1 to 1.0:1. As an example, the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 0.5:1, 0.6:1, 0.7:1, 0.8:1, 1.0:1, or any value within the range defined by any two of the above values. It is understood that controlling the molar ratio of oxygen to nickel in the second nickel oxide layer 22 results in a lower oxygen content in the second nickel oxide layer 22. This ensures good adhesion to the copper layer 30 while also helping to control the interfacial reaction between the second nickel oxide layer 22 and the copper layer 30, thereby maintaining the stability of the adhesion with the copper layer 30.

[0073] In some embodiments, the thickness of the transition layer 20 is 9 nm to 16 nm. For example, the thickness of the transition layer 20 is 9 nm, 10 nm, 12 nm, 14.5 nm, 16 nm, or any value within the range defined by any two of the above values ​​as endpoints. It is understood that controlling the thickness of the transition layer 20 is beneficial for the transition layer 20 to effectively perform its connection and buffering function between the substrate and the copper layer.

[0074] In some embodiments, the thickness ratio of the first nickel oxide layer 21 to the second nickel oxide layer 22 is 0.5:1 to 2:1. As examples, the thickness ratio of the first nickel oxide layer 21 to the second nickel oxide layer 22 is 0.5:1, 0.95:1, 1.0:1, 1.8:1, 2:1, or any value within the range defined by any two of the above points as endpoints. It can be understood that by controlling the thickness ratio of the first nickel oxide layer 21 to the second nickel oxide layer 22, a suitable structural match is formed between the first nickel oxide layer 21 and the second nickel oxide layer 22, which is beneficial for balancing the bonding performance between the transition layer 20 and the substrate 10 and the copper layer 30.

[0075] In some embodiments, the intramural stress of the transition layer 20 is ≤90 MPa. As an example, the intramural stress of the transition layer 20 is 10 MPa, 20 MPa, 30 MPa, 78 MPa, 90 MPa, or any value within the range of any two of the above values. Optionally, the intramural stress of the transition layer 20 is 30 MPa to 90 MPa. It is understood that the minimum physical limit of the intramural stress is greater than 0 MPa and cannot be negative. By controlling the intramural stress of the transition layer 20, it is beneficial to control the peel resistance of the transition layer 20.

[0076] In some embodiments, the transition layer is an amorphous dense film. It is understood that the amorphous structure helps to prevent copper atoms from rapidly diffusing into the organic substrate along the grain boundaries, and helps to control the migration of copper ions; the isotropic distribution of internal stress in the amorphous structure helps to control the internal tensile or compressive stress, and control the macroscopic warping caused by the mismatch of thermal expansion coefficients at the microscopic level.

[0077] In some embodiments, the thickness of the copper layer 30 is 100 nm to 450 nm. As examples, the thickness of the copper layer 30 is 100 nm, 200 nm, 280 nm, 320 nm, 450 nm, or any value within the range defined by any two of the above values ​​as endpoints. It can be understood that by controlling the thickness of the copper layer 30, the copper layer 30 can possess suitable structural strength and conductivity.

[0078] In some embodiments, the resistivity of copper layer 30 is ≤2.6 μΩ·cm. As examples, the resistivity of copper layer 30 is 0.5 μΩ·cm, 1.0 μΩ·cm, 1.67 μΩ·cm, 2.4 μΩ·cm, 2.6 μΩ·cm, or any value within the range of any two of the above values. Optionally, the resistivity of copper layer 30 is 1.67 μΩ·cm to 2.6 μΩ·cm. It is understood that the minimum physical limit of the resistivity of copper layer 30 is greater than 0 μΩ·cm and cannot be negative. By controlling the resistivity of copper layer 30, it is beneficial to control losses during current transmission.

[0079] In some embodiments, the adhesion between the copper layer 30 and the substrate 10 achieves a 5B grade in a cross-cut test. It is understood that 5B is the highest grade in the cross-cut test, indicating high adhesion between the copper layer 30 and the transition layer 20.

[0080] In some embodiments, the substrate 10 includes one or more of soda-lime silica glass, borosilicate glass, polyimide film, and polyethylene terephthalate film. It is understood that by selecting different substrates 10, which possess corresponding mechanical properties, heat resistance properties, or flexibility properties according to actual application requirements, the copper-plated substrate 100 can adapt to different application scenarios.

[0081] See Figure 2 One embodiment of this application provides a method for preparing a copper-plated substrate 100, comprising the following steps:

[0082] S102: Using a nickel target as raw material and argon and oxygen as working gases, a transition layer 20 is deposited on at least one surface of a substrate 10 using a first magnetron sputtering process; the deposition process of the transition layer 20 includes a first deposition stage and a second deposition stage performed sequentially, wherein the oxygen flow rate in the second deposition stage is lower than that in the first deposition stage.

[0083] S103: A copper layer 30 is prepared on the surface of the transition layer 20 away from the substrate 10.

[0084] The above preparation method controls the oxygen flow rate in the first deposition stage and the second deposition stage to form a first nickel oxide layer 21 and a second nickel oxide layer 22 in the transition layer 20, and makes the first nickel oxide layer 21 have a higher oxygen content, which is beneficial to balance the bonding performance and adhesion between the transition layer 20 and the substrate 10 and the copper layer 30.

[0085] In some embodiments, the oxygen flow rate in the first deposition stage is 0.9 sccm to 1.5 sccm. As examples, the oxygen flow rate in the first deposition stage is 0.9 sccm, 1.0 sccm, 1.1 sccm, 1.2 sccm, 1.5 sccm, or any value within a range defined by any two of the above values ​​as endpoints. Optionally, the oxygen flow rate in the first deposition stage is 0.9 sccm to 1.1 sccm. It is understood that controlling the oxygen flow rate in the first deposition stage within a predetermined range is beneficial for forming a first nickel oxide layer 21 with a suitable high oxygen content, thereby creating a suitable bonding interface between the first nickel oxide layer 21 and the substrate 10.

[0086] In some embodiments, the duration of the first deposition stage is 1.5 min to 2.5 min. For example, the duration of the first deposition stage is 1.5 min, 1.6 min, 1.8 min, 2.0 min, 2.5 min, or any value within a range defined by any two of the above values ​​as endpoints. It is understood that controlling the duration of the first deposition stage within a predetermined range is beneficial for adjusting the thickness and structural characteristics of the first nickel oxide layer 21.

[0087] In some embodiments, the oxygen flow rate in the second deposition stage is 0.2 sccm to 0.6 sccm. As examples, the oxygen flow rate in the second deposition stage is 0.2 sccm, 0.3 sccm, 0.4 sccm, 0.5 sccm, 0.6 sccm, or any value within a range defined by any two of the above values ​​as endpoints. Optionally, the oxygen flow rate in the second deposition stage is 0.4 sccm to 0.6 sccm. It is understood that controlling the oxygen flow rate in the second deposition stage within a predetermined range is beneficial for forming a second nickel oxide layer 22 with a suitable low oxygen content, thereby creating a suitable bonding interface between the second nickel oxide layer 22 and the copper layer 30.

[0088] In some embodiments, the duration of the second deposition stage is 2.5 min to 3.5 min. As an example, the duration of the first deposition stage is 2.5 min, 2.6 min, 2.8 min, 3.0 min, or 3.5 min, or any value within a range defined by any two of the aforementioned values ​​as endpoints. It is understood that controlling the duration of the second deposition stage within a predetermined range is beneficial for adjusting the thickness of the second nickel oxide layer 22 and the interlayer structure between it and the first nickel oxide layer 21.

[0089] In some embodiments, the operating gas pressure of the first magnetron sputtering process is 0.3 Pa to 0.5 Pa. As examples, the operating gas pressure of the first magnetron sputtering process is 0.3 Pa, 0.34 Pa, 0.4 Pa, 0.46 Pa, 0.5 Pa, or any value within the range defined by any two of the above points as endpoints. It can be understood that controlling the operating gas pressure of the first magnetron sputtering process is beneficial for adjusting the motion state of the sputtered particles and the deposition process, thereby obtaining a structurally uniform transition layer 20.

[0090] Optionally, the first magnetron sputtering process is DC pulsed magnetron sputtering. It can be understood that using DC pulsed magnetron sputtering to deposit the transition layer 20 is beneficial for adjusting the stability of the deposition process of the transition layer 20.

[0091] In some embodiments, the sputtering power of the first magnetron sputtering process is 90 W to 130 W, the pulse frequency is 30 kHz to 100 kHz, and the duty cycle is 30% to 50%. As an example, the sputtering power of the first magnetron sputtering process is 90 W, 100 W, 110 W, 120 W, or 130 W, or any value within the range defined by any two of the above values; the pulse frequency is 30 kHz, 50 kHz, 68 kHz, 92 kHz, or 100 kHz, or any value within the range defined by any two of the above values; and the duty cycle is 30%, 34%, 40%, 46%, or 50%, or any value within the range defined by any two of the above values. It is understood that by controlling the sputtering power, pulse frequency, and duty cycle of the first magnetron sputtering process within a predetermined range, it is beneficial to adjust the sputtering rate of the nickel target material and the deposition state of the transition layer 20.

[0092] In some embodiments, the temperature of the substrate 10 during the deposition of the transition layer 20 is ≤90°C. As an example, the substrate temperature during the deposition of the transition layer 20 is 0°C, 70°C, 85°C, 88°C, or 90°C, or any value within a range defined by any two of the above points as endpoints. It is understood that controlling the temperature of the substrate 10 during the deposition of the transition layer 20 is beneficial for controlling the deformation or performance changes of the substrate 10 caused by thermal effects.

[0093] Optionally, the copper layer 30 is prepared using a second magnetron sputtering process.

[0094] Optionally, the second magnetron sputtering process uses argon as the working gas. It can be understood that using argon as the working gas for the second magnetron sputtering process is beneficial for stabilizing the sputtering process of the copper target material, thereby facilitating the stable formation of the copper layer 30.

[0095] In some embodiments, the operating gas pressure of the second magnetron sputtering process is 0.35 Pa to 0.45 Pa. As examples, the operating gas pressure of the second magnetron sputtering process is 0.35 Pa, 0.36 Pa, 0.4 Pa, 0.42 Pa, 0.45 Pa, or any value within the range defined by any two of the above points as endpoints. It can be understood that controlling the operating gas pressure of the second magnetron sputtering process is beneficial for adjusting the deposition behavior of copper atoms and controlling the uniformity and density of the copper layer 30.

[0096] In some embodiments, the substrate negative bias voltage of the second magnetron sputtering process is -30 V to -50 V. As an example, the operating gas pressure of the second magnetron sputtering process is -30 V, -32 V, -40 V, -46 V, -50 V, or any value within the range defined by any two of the above points as endpoints. It can be understood that the substrate negative bias voltage of the second magnetron sputtering process refers to the negative bias voltage applied to the substrate stage supporting the substrate 10 and the transition layer 20 already formed on its surface. It mainly affects the side of the transition layer 20 away from the substrate 10 and is used to adjust the energy state during the copper atom deposition process.

[0097] Optionally, the second magnetron sputtering process is DC pulse magnetron sputtering. It is understood that using DC pulse magnetron sputtering to prepare the copper layer 30 is beneficial for adjusting the stability of the copper layer 30 deposition process.

[0098] In some embodiments, the sputtering power of the second magnetron sputtering process is 140 W to 220 W, the pulse frequency is 30 kHz to 100 kHz, and the duty cycle is 30% to 50%. As an example, the sputtering power of the second magnetron sputtering process is 140 W, 160 W, 180 W, 200 W, 220 W, or any value within the range defined by any two of the above values; the pulse frequency is 30 kHz, 50 kHz, 68 kHz, 92 kHz, 100 kHz, or any value within the range defined by any two of the above values; and the duty cycle is 30%, 34%, 40%, 46%, 50%, or any value within the range defined by any two of the above values. It can be understood that controlling the sputtering power, pulse frequency, and duty cycle of the second magnetron sputtering process is beneficial for adjusting the deposition rate and microstructure of the copper layer 30.

[0099] In some embodiments, the temperature of the substrate 10 during the preparation of the copper layer 30 is ≤100°C.

[0100] In some embodiments, after preparing the copper layer 30, the following steps are also included:

[0101] S104: Perform constant temperature annealing in a vacuum environment.

[0102] The above preparation method, through isothermal annealing, is beneficial to the interfacial bonding between the copper layer 30 and the transition layer 20, and regulates the stability of the film structure of the copper layer 30.

[0103] In some embodiments, the vacuum degree of the isothermal annealing process is ≤5×10⁻⁵. -4 Pa. As an example, the vacuum degree of isothermal annealing is 1 × 10⁻⁶ Pa. -5 Pa, 5×10 -5 Pa, 2×10-4 Pa, 4×10 -4 Pa, 5×10 -4 Pa, or any value within the range formed by any two of the above point values ​​and 0 Pa. Optionally, the vacuum degree of the isothermal annealing treatment is 2.0 × 10⁻⁶. -4 Pa~5×10 -4 Pa. It is understandable that the minimum physical limit of vacuum in isothermal annealing is greater than 0 Pa, and cannot be negative. Controlling the vacuum level during isothermal annealing helps to control the influence of external gases on the copper layer 30 during the annealing process.

[0104] In some embodiments, the isothermal annealing temperature is 90°C to 100°C. For example, the isothermal annealing temperature is 90°C, 92°C, 94°C, 96°C, or 100°C, or any value within the range of any two of the above values. It is understood that controlling the isothermal annealing temperature is beneficial for regulating the interfacial diffusion and bonding between the copper layer 30 and the transition layer 20, and also for controlling the deformation or performance changes of the substrate 10 caused by thermal effects.

[0105] In some embodiments, the isothermal annealing time is 18 min to 28 min. For example, the isothermal annealing time is 18 min, 20 min, 22 min, 24 min, 28 min, or any value within the range of any two of the above values. It can be understood that controlling the isothermal annealing time facilitates a sufficient interfacial interaction between the copper layer 30 and the transition layer 20.

[0106] In some embodiments, the following steps are included before depositing the transition layer 20:

[0107] S101: The surface of the substrate 10 is subjected to plasma activation treatment using a radio frequency ion source.

[0108] It is understandable that plasma activation treatment of the surface of substrate 10 can help change the activity of the surface of substrate 10 and help regulate the bonding performance between transition layer 20 and substrate 10.

[0109] In some embodiments, the plasma activation process uses argon and oxygen as the working gases, with a partial pressure ratio of argon to oxygen of 2:1 to 9:1. As examples, the partial pressure ratios of argon to oxygen are 2:1, 4:1, 6:1, 8:1, 9:1, or any value within the range of any two of the above values. It is understood that controlling the partial pressure ratio of argon to oxygen is beneficial for adjusting the activation level and surface chemical state of the substrate 10, and for regulating the interfacial bonding performance between the substrate 10 and the transition layer 20.

[0110] In some embodiments, the working gas pressure for plasma activation treatment is 0.7 Pa to 0.9 Pa. As examples, the working gas pressure for plasma activation treatment is 0.7 Pa, 0.74 Pa, 0.8 Pa, 0.86 Pa, 0.9 Pa, or any value within the range formed by any two of the above points. It can be understood that controlling the working gas pressure for plasma activation treatment is beneficial for regulating the motion state of active particles in the plasma.

[0111] In some embodiments, the power of the radio frequency ion source is 180 W to 250 W. As examples, the power of the radio frequency ion source is 180 W, 200 W, 220 W, 240 W, 250 W, or any value within the range formed by any two of the above points. It can be understood that by controlling the power of the radio frequency ion source, it is beneficial to adjust the energy of the ions in the plasma, thereby regulating the processing uniformity and activation effect of the substrate 10 surface.

[0112] In some embodiments, the negative bias voltage of the plasma-activated substrate is -40 V to -60 V. As examples, the negative bias voltage of the plasma-activated substrate is -40 V, -42 V, -50 V, -54 V, -60 V, or any value within the range of any two of the above values. It can be understood that the negative bias voltage of the plasma-activated substrate refers to the negative bias voltage applied to the substrate stage supporting the substrate 10, which is used to adjust the bombardment energy of plasma ions on the surface of the substrate 10.

[0113] In some embodiments, the plasma activation treatment time is 4 to 6 minutes. For example, the plasma activation treatment time is 4 minutes, 4.2 minutes, 5 minutes, 5.6 minutes, 6 minutes, or any value within the range of any two of the above values. It can be understood that controlling the plasma activation treatment time is beneficial for fully activating the surface of the substrate 10.

[0114] In some embodiments, the substrate temperature for plasma activation treatment is ≤80°C. As an example, the substrate temperature for plasma activation treatment is 50°C, 60°C, 70°C, 75°C, 80°C, or any value within the range of any two of the above values. It is understood that by controlling the temperature of the substrate 10 during plasma activation treatment, it is beneficial to control the performance changes of the substrate 10 caused by thermal effects, while ensuring the activation effect on the surface of the substrate 10.

[0115] In some embodiments, prior to plasma activation treatment, the following steps are included: placing the substrate into a vacuum chamber and evacuating the base vacuum to a vacuum level ≤3×10⁻⁶. -4 Pa.

[0116] In some embodiments, the following steps are included prior to the plasma activation treatment:

[0117] The substrate was ultrasonically cleaned sequentially with water-based cleaning agent, anhydrous ethanol, and deionized water, and then dried at low temperature; the temperature during the cleaning and drying process was ≤50℃.

[0118] One embodiment of this application provides a display device, including the copper-plated substrate described above, or the copper-plated substrate prepared by the above preparation method.

[0119] Therefore, the aforementioned display device uses this copper-plated substrate, which has good stability and reliability, can be adapted to applications in multiple scenarios, and extends the service life of the display device.

[0120] The following are specific examples.

[0121] Example 1: Copper-plated substrate of ultrathin glass substrate and its preparation method and performance testing:

[0122] The copper-plated substrate 100 of the ultra-thin glass substrate Figure 1 As shown, the structure includes a substrate 10, a nickel oxide transition layer 20, and a copper layer 30 stacked sequentially. The substrate 10 has a thickness of 0.7 mm, and the copper layer 30 has a thickness of 280 nm. The first nickel oxide layer 21 has a molar ratio of oxygen to nickel of 1.1:1 and a thickness of 3.8 nm. The second nickel oxide layer 22 has a molar ratio of oxygen to nickel of 0.6:1 and a thickness of 8.2 nm.

[0123] The method for preparing the copper-plated substrate 100 of the ultrathin glass substrate is as follows:

[0124] S101: Using 0.7 mm thin sodium-calcium-silicon optical glass as substrate 10, ultrasonic cleaning is performed sequentially with water-based cleaning agent, anhydrous ethanol, and deionized water at 45°C, followed by drying at 48°C. The glass is then placed in a vacuum chamber, and a base vacuum is evacuated to a vacuum level of 2.6 × 10⁻⁶. -4 The surface of substrate 10 was plasma activated using argon and oxygen as working gases and an RF ion source. The partial pressure ratio of argon to oxygen was 4:1, the working gas pressure was 0.8 Pa, the power of the RF ion source was 220 W, the negative bias voltage of the plasma activated substrate was -50 V, the substrate temperature was 75 °C, and the activation treatment lasted for 6 min.

[0125] S102: Using a nickel target as the raw material and argon and oxygen as the working gases, a transition layer 20 is deposited on one side of the substrate 10 using a DC pulsed magnetron sputtering process; the working gas pressure is 0.4 Pa, the sputtering power is 110 W, the pulse frequency is 50 kHz, the duty cycle is 40%, and the substrate temperature is 88℃; the deposition process of the transition layer 20 includes a first deposition stage and a second deposition stage performed sequentially; in the first deposition stage, the oxygen flow rate is 1.0 sccm and the time is 2.0 min; in the second deposition stage, the oxygen flow rate is 0.5 sccm and the time is 3.0 min; thus, a first nickel oxide layer and a second nickel oxide layer are formed sequentially.

[0126] S103: Using a copper target as raw material and pure argon as working gas, a copper layer 30 is prepared on the surface of the transition layer 20 away from the substrate 10 using a DC pulsed magnetron sputtering process; the working gas pressure is 0.3 Pa, the substrate negative bias voltage of the second magnetron sputtering process is -40V, the sputtering power is 180 W, the pulse frequency is 50 kHz, the duty cycle is 50%, and the substrate temperature is up to 96℃.

[0127] S104: Maintain vacuum level at 4.0 × 10⁻⁶ -4 Pa was subjected to constant temperature annealing at 98°C for 22 min in a vacuum environment, and the vacuum was maintained until it was naturally cooled to 42°C before being removed from the furnace, resulting in a copper-plated substrate 100 of ultra-thin glass substrate.

[0128] Example 2: Copper-plated substrate of CPI flexible material and its preparation method and performance testing:

[0129] The copper-plated substrate 100 of the flexible polyethylene terephthalate (CPI) substrate Figure 1 As shown, the structure includes a substrate 10, a nickel oxide transition layer 20, and a copper layer 30 stacked sequentially. The substrate 10 has a thickness of 50 μm, and the copper layer 30 has a thickness of 200 nm. The first nickel oxide layer 21 has a molar ratio of oxygen to nickel of 1.3:1 and a thickness of 3.6 nm. The second nickel oxide layer 22 has a molar ratio of oxygen to nickel of 0.7:1 and a thickness of 7.6 nm.

[0130] The method for preparing the copper-plated substrate 100 of the ultrathin glass substrate is as follows:

[0131] S101: A 50 μm polyethylene terephthalate (CPI) flexible optical film was used as substrate 10. It was ultrasonically cleaned with isopropanol at 45°C, dried at 45°C, and then placed into a vacuum chamber. The vacuum level was evacuated to 2.6 × 10⁻⁶. -4The surface of substrate 10 was plasma activated using argon and oxygen as working gases and an RF ion source. The partial pressure ratio of argon to oxygen was 4:1, the working gas pressure was 0.8 Pa, the power of the RF ion source was 200 W, the negative bias voltage of the plasma activated substrate was -45 V, the substrate temperature was 70℃, and the activation treatment lasted for 6 min.

[0132] S102: Using a nickel target as the raw material and argon and oxygen as the working gases, a transition layer 20 is deposited on one side of the substrate 10 using a DC pulsed magnetron sputtering process; the working gas pressure is 0.4 Pa, the sputtering power is 100 W, the pulse frequency is 50 kHz, the duty cycle is 40%, and the substrate temperature is 85℃; the deposition process of the transition layer 20 includes a first deposition stage and a second deposition stage performed sequentially; in the first deposition stage, the oxygen flow rate is 1.1 sccm and the time is 2.0 min; in the second deposition stage, the oxygen flow rate is 0.6 sccm and the time is 3.0 min;

[0133] S103: Using a copper target as raw material and pure argon as working gas, a copper layer 30 is prepared on the surface of the transition layer 20 away from the substrate 10 using a DC pulsed magnetron sputtering process; the working gas pressure is 0.3 Pa, the substrate negative bias voltage of the second magnetron sputtering process is -35V, the sputtering power is 160 W, the pulse frequency is 50 kHz, the duty cycle is 50%, and the substrate temperature is up to 96℃.

[0134] S104: Maintain vacuum level at 4.0 × 10⁻⁶ -4 Pa was subjected to constant temperature annealing at 95°C for 20 min in a vacuum environment, and then naturally cooled to 42°C while maintaining the vacuum level before being removed from the furnace to obtain copper-plated substrate 100 of CPI flexible substrate.

[0135] Example 3:

[0136] The difference from Example 1 is that the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.5:1, and the thickness of the first nickel oxide layer 21 is 3.5 nm; the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 0.5:1, and the thickness of the second nickel oxide layer 22 is 8.6 nm.

[0137] In S102, the oxygen flow rate in the first deposition stage was 1.2 sccm, and the time was 2.0 min; the oxygen flow rate in the second deposition stage was 0.3 sccm, and the time was 3.0 min.

[0138] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0139] Example 4:

[0140] The difference from Example 1 is that the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.5:1, and the thickness of the first nickel oxide layer 21 is 3.5 nm; the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 0.6:1, and the thickness of the second nickel oxide layer 22 is 8.2 nm.

[0141] In S102, the oxygen flow rate in the first deposition stage was 1.2 sccm, and the time was 2.0 min; the oxygen flow rate in the second deposition stage was 0.5 sccm, and the time was 3.0 min.

[0142] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0143] Example 5:

[0144] The difference from Example 1 is that the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.1:1, and the thickness of the first nickel oxide layer 21 is 2.9 nm; the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 0.6:1, and the thickness of the second nickel oxide layer 22 is 9.6 nm.

[0145] In S102, the oxygen flow rate in the first deposition stage is 1.0 sccm, and the deposition time is 1.5 min; in the second deposition stage, the oxygen flow rate is 0.5 sccm, and the deposition time is 3.5 min.

[0146] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0147] Example 6:

[0148] The difference from Example 1 is that the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 1.1:1, and the thickness of the first nickel oxide layer 21 is 4.8 nm; the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 0.6:1, and the thickness of the second nickel oxide layer 22 is 6.8 nm.

[0149] In S102, the oxygen flow rate in the first deposition stage was 1.0 sccm, and the deposition time was 2.5 min; in the second deposition stage, the oxygen flow rate was 0.5 sccm, and the deposition time was 2.5 min.

[0150] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0151] Comparative Example 1: Copper-plated substrate with homogeneous nickel oxide transition layer and its preparation method and performance testing:

[0152] The copper-plated substrate with the homogeneous nickel oxide transition layer and its preparation method are basically the same as those in Example 1, except that the molar ratio of oxygen to nickel in the nickel oxide transition layer is 1.1:1 and the thickness of the nickel oxide transition layer is 9.5 nm.

[0153] In S102, the deposition stage conditions are: oxygen flow rate of 1.0 sccm and time of 5.0 min, forming a monolayer homogeneous nickel oxide transition layer;

[0154] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0155] Comparative Example 2:

[0156] The difference from Example 1 is that the molar ratio of oxygen to nickel in the first nickel oxide layer 21 is 0.6:1, and the thickness of the first nickel oxide layer 21 is 5.5 nm; the molar ratio of oxygen to nickel in the second nickel oxide layer 22 is 1.3:1, and the thickness of the second nickel oxide layer 22 is 5.7 nm.

[0157] In S102, the oxygen flow rate in the first deposition stage was 0.5 sccm, and the time was 2.0 min; in the second deposition stage, the oxygen flow rate was 1 sccm, and the time was 3.0 min.

[0158] Furthermore, under the same conditions, the substrate 10 in S101 was replaced with a CPI flexible optical film instead of thinned sodium-calcium-silicon optical glass, and a copper-plated substrate of CPI flexible substrate under the same conditions was prepared.

[0159] Table 1 shows some parameters of the transition layer prepared in each embodiment and comparative example S102, as well as some parameters of the transition layer in the copper-plated substrate.

[0160] Table 1

[0161]

[0162] In Table 1, "O:Ni" refers to the molar ratio of oxygen to the element.

[0163] The copper-plated substrates prepared in each embodiment and comparative example were subjected to performance tests:

[0164] Resistivity ρ0 test method: The four-probe method is used. The four probes are arranged at equal intervals along the same straight line and pressed vertically on the surface of the copper layer 30 away from the substrate 10. The two outer probes are supplied with a constant DC current, and the two inner probes are tested for voltage drop. The sheet resistance is calculated by the probe geometric coefficients and then converted into volume resistivity by combining the thickness of the copper layer 30.

[0165] Adhesion test method: The test is conducted according to ASTM D3359. A vertically intersecting grid (1mm*1mm grid) is drawn on the surface of the copper layer 30. The copper layer 30 and the transition layer 20 are cut through to the substrate 10. The copper layer 30 is then cut through to the substrate 10. Pressure-sensitive adhesive tape with a specified peel strength is applied and then quickly removed. The adhesion level of the copper-plated substrate 100 is evaluated based on the percentage of the area of ​​the copper layer 30 that has fallen off.

[0166] Film internal stress test method: According to ASTM F1048-10(2021) standard, the total stress on the copper-plated substrate 100 was directly tested using a laser scanning thin film stress meter;

[0167] Humid heat aging performance test: The copper-plated substrate 100 was subjected to humid heat aging at a temperature of 85℃ and a relative humidity (RH) of 85%. After a certain period of time, the presence of peeling was observed.

[0168] High and low temperature resistance test: The copper-plated substrate 100 was subjected to 500 cycles of high and low temperature cycling within the range of -40℃ to 100℃. The resistivity ρ1 was measured, and the rate of change of resistance ρ was calculated. X =(ρ1-ρ0) / ρ0.

[0169] Bending test: Under the condition of bending radius R=1.5 mm, repeatedly bend 180°.

[0170] The results are shown in Table 2.

[0171] Table 2

[0172]

[0173] Table 2 shows that the resistivity of the copper layer 30 of the copper-plated substrate 100 prepared in Examples 1-6 are 2.3 μΩ·cm, 2.5 μΩ·cm, 2.2 μΩ·cm, 2.4 μΩ·cm, 2.2 μΩ·cm, and 2.4 μΩ·cm, respectively, and the adhesion cross-cut test all reach level 5B. The internal stress of the film layer of the copper-plated substrates in Examples 1, 3-6 are 72 MPa, 79 MPa, 99 MPa, 62 MPa, and 84 MPa, respectively. They were subjected to damp heat aging at 85°C and 85% relative humidity for 1000 h, 900 h, 800 h, 1200 h, and 850 h, respectively. There was no peeling within h. After 500 cycles of high and low temperature cycling in the range of −40℃ to 100℃, the resistance change rate was 2.9%, 3.1%, 3.5%, 2.5%, and 3.2%, respectively. It has high adhesion, low stress, good conductivity, and excellent weather resistance. The copper-plated substrates of CPI flexible substrates prepared in Examples 2 to 6 under the same conditions were subjected to repeated bending at 180° for 180,000, 160,000, 120,000, 200,000, and 140,000 times with a bending radius R=1.5 mm, respectively. The film layer did not curl or crack. In addition to having many of the properties of the copper-plated substrate 100 of the ultra-thin glass substrate prepared in Example 1, it can also be adapted to flexible folding display scenarios.

[0174] The copper-plated substrate 100 with the homogeneous nickel oxide transition layer prepared in Comparative Example 1 achieved a 3B grade in the cross-cut adhesion test, with an internal stress of 156 MPa and microcracks appearing after 30,000 bending cycles. Under damp heat aging conditions of 85°C and 85% relative humidity, localized peeling occurred after 200 hours. After 500 cycles of high and low temperature cycling within the range of −40°C to 100°C, the resistivity change rate was 11.8%. Based on the above tests, it can be seen that the copper-plated substrate with the homogeneous nickel oxide transition layer in Comparative Example 1 has significantly inferior overall performance compared to the copper-plated substrate prepared in the embodiments of this application.

[0175] The resistivity of the copper layer 30 of the copper-plated substrate 100 prepared in Comparative Example 2 was 2.3 μΩ·cm, the adhesion cross-cut test achieved a 4B rating, and the film internal stress was 121 MPa. After 500 hours of damp heat aging at 85°C and 85% relative humidity, localized peeling occurred. After 500 cycles of high and low temperature cycling within the range of −40°C to 100°C, the resistivity change rate was 4.5%. Under the same conditions, the copper-plated substrate of the CPI flexible substrate, after 30,000 repeated 180° bends with a bending radius R = 1.5 mm, developed microcracks. The above tests show that the oxygen content of the second nickel oxide layer 22 of the copper-plated substrate 100 is higher than that of the first nickel oxide layer 21, and its overall performance is far inferior to that of the copper-plated substrate prepared in the examples.

[0176] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0177] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A copper-plated substrate, characterized in that, The material includes a substrate, a transition layer, and a copper layer stacked sequentially. The transition layer includes a first nickel oxide layer and a second nickel oxide layer. The second nickel oxide layer is disposed between the first nickel oxide layer and the copper layer. The oxygen content of the second nickel oxide layer is lower than that of the first nickel oxide layer.

2. The copper-plated substrate according to claim 1, characterized in that, The transition layer satisfies one or more of the following conditions: (1) The molar ratio of oxygen to nickel in the first nickel oxide layer is 1.1:1 to 1.5:1; (2) The molar ratio of oxygen to nickel in the second nickel oxide layer is 0.5:1 to 1.0:

1.

3. The copper-plated substrate according to claim 1, characterized in that, The transition layer satisfies one or more of the following conditions: (1) The total thickness of the transition layer is 9 nm to 16 nm; (2) The thickness ratio of the first nickel oxide layer to the second nickel oxide layer is 0.5:1 to 2:1; (3) The intramural stress of the transition layer is ≤90 MPa.

4. The copper-plated substrate according to any one of claims 1 to 3, characterized in that, The copper layer satisfies one or more of the following conditions: (1) The thickness of the copper layer is 100 nm to 450 nm; (2) The resistivity of the copper layer is ≤2.6 μΩ·cm; (3) The adhesion between the copper layer and the substrate is rated as 5B by cross-cut test.

5. The copper-plated substrate according to any one of claims 1 to 3, characterized in that, The substrate includes one or more of sodium-calcium silicate glass, borosilicate glass, polyimide film, and polyethylene terephthalate film.

6. A method for preparing a copper-plated substrate, characterized in that, Includes the following steps: Using a nickel target as raw material and argon and oxygen as working gases, a transition layer is deposited on at least one surface of a substrate using a first magnetron sputtering process. The deposition process of the transition layer includes a first deposition stage and a second deposition stage performed sequentially, wherein the oxygen flow rate in the second deposition stage is lower than that in the first deposition stage. A copper layer is prepared on the surface of the transition layer away from the substrate.

7. The method for preparing a copper-plated substrate according to claim 6, characterized in that, In the first magnetron sputtering process, one or more of the following conditions are met: (1) The oxygen flow rate in the first deposition stage is 0.9 sccm to 1.5 sccm; (2) The duration of the first deposition stage is 1.5 min to 2.5 min; (3) The oxygen flow rate in the second deposition stage is 0.2 sccm ~ 0.6 sccm; (4) The second deposition stage lasts for 2.5 min to 3.5 min.

8. The method for preparing a copper-plated substrate according to claim 6, characterized in that, In the first magnetron sputtering process, one or more of the following conditions are met: (1) The working air pressure is 0.3 Pa to 0.5 Pa; (2) The first magnetron sputtering process is DC pulse magnetron sputtering; (3) The sputtering power is 90 W~130 W, the pulse frequency is 30 kHz~100 kHz, and the duty cycle is 30%~50%; (4) The temperature of the substrate is ≤90℃.

9. The method for preparing a copper-plated substrate according to any one of claims 6 to 8, characterized in that, The copper layer is deposited using a second magnetron sputtering process, wherein the second magnetron sputtering process satisfies one or more of the following conditions: (1) Argon is used as the working gas; (2) The working air pressure is 0.35 Pa to 0.45 Pa; (3) The substrate negative bias voltage is -30 V to -50 V; (4) The second magnetron sputtering process is DC pulse magnetron sputtering; (5) The sputtering power is 140 W to 220 W, the pulse frequency is 30 kHz to 100 kHz, and the duty cycle is 30% to 50%.

10. The method for preparing a copper-plated substrate according to claim 9, characterized in that, After the copper layer is prepared, the following steps are also included: the substrate with the deposited copper layer is subjected to constant temperature annealing in a vacuum environment; Optionally, the isothermal annealing treatment satisfies one or more of the following conditions: (1) Vacuum degree ≤ 5×10 -4 Pa; (2) The temperature is 90℃~100℃; (3) The time is 18 min to 28 min.

11. The method for preparing a copper-plated substrate according to any one of claims 6-8 and 10, characterized in that, Before depositing the transition layer, the method further includes the following step: performing plasma activation treatment on the surface of the substrate using a radio frequency ion source; Optionally, the plasma activation treatment satisfies one or more of the following conditions: (1) Argon and oxygen are used as working gases, and the partial pressure ratio of argon to oxygen is 2:1 to 9:1; (2) The working air pressure is 0.7 Pa to 0.9 Pa; (3) The power of the radio frequency ion source is 180 W to 250 W; (4) The substrate negative bias voltage is -40 V to -60 V; (5) The time is 4 min to 6 min; (6) Substrate temperature ≤ 80℃.