High-temperature protective coating for slowing down al consumption and its preparation method and application
By depositing a NiAlHfR coating on the surface of a nickel-based superalloy substrate, the problem of rapid Al consumption during the high-temperature oxidation process of the β-NiAl phase coating was solved, thereby reducing the oxide film growth rate and extending the coating life.
Patent Information
- Application Number
- CN202611590409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing β-NiAl phase coatings experience rapid Al consumption during high-temperature oxidation, leading to oxide film thickening, porosity, cracks, and interface undulations, which affects the high-temperature protective life of the coating.
A NiAlHfR coating is deposited on the surface of a nickel-based superalloy substrate, wherein R includes at least one of Y, Zr, La, Ce and Dy. The composition and thickness of the NiAlHfR coating are controlled by arc ion plating and vacuum heat treatment to slow down the consumption of Al.
It effectively reduces the growth rate of oxide film, improves the coating's resistance to high-temperature oxidation and service life, and enhances the stability of the oxide film-coating interface.
Smart Images

Figure CN123152997A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of protective coating technology, and more specifically, to a high-temperature protective coating that slows down Al consumption, its preparation method, and its application. Background Technology
[0002] Nickel-based superalloys possess excellent high-temperature mechanical properties and are widely used in hot-end components of equipment such as aero-engines and gas turbines. Since these hot-end components are exposed to high-temperature environments for extended periods, their surfaces are prone to oxidation; therefore, a high-temperature protective coating is typically applied to the surface of the nickel-based superalloy.
[0003] β-NiAl phase coatings have a high Al content and can form a protective Al2O3 oxide film on the surface under high-temperature conditions, making them a commonly used high-temperature protective coating. However, during long-term high-temperature oxidation, the continuous growth of the oxide film will continuously consume the Al element in the coating. As the Al content in the coating decreases, the coating's ability to form a protective oxide film gradually declines, and problems such as oxide film thickening, porosity, cracks, interface undulations, and an increase in non-protective oxides are prone to occur, affecting the high-temperature protective life of the coating.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a high-temperature protective coating that slows down Al consumption, as well as its preparation method and application, in order to solve or improve the above-mentioned technical problems.
[0006] This invention can be implemented as follows: In a first aspect, the present invention provides a high-temperature protective coating for slowing down Al consumption. The high-temperature protective coating includes a nickel-based superalloy substrate and a NiAlHfR coating deposited on the surface of the nickel-based superalloy substrate, wherein R includes at least one of Y, Zr, La, Ce and Dy. On an atomic percentage basis, the NiAlHfR coating contains 38.9 at.%~54.75 at.% Al, 0%~0.5 at.% Hf and 0%~0.5 at.% R, with the balance being Ni.
[0007] In an optional embodiment, the content of R element in the NiAlHfR coating is 0.05 at.% to 0.4 at.%; or, the content of Hf element in the NiAlHfR coating is 0.05 at.% to 0.5 at.%.
[0008] In an optional embodiment, the thickness of the NiAlHfR coating is 20 μm to 60 μm.
[0009] In an optional embodiment, after being oxidized at a constant temperature of 1200°C for 400 hours, the NiAlHfR coating contains 0%~20% of Al-rich β-NiAl phase and 80%~100% of γ′-Ni3Al phase.
[0010] In a second aspect, the present invention provides a method for preparing a high-temperature protective coating according to any of the foregoing embodiments, comprising the following steps: depositing a NiAlHfR coating on the surface of a nickel-based high-temperature alloy substrate by arc ion plating, followed by vacuum heat treatment.
[0011] In an optional embodiment, the process parameters for arc ion plating include: furnace temperature of 300℃~400℃, deposition gas pressure of 0.8Pa~1.2Pa, arc target current of 50A~120A, substrate bias voltage of -50V~-150V, duty cycle of 70%~90%, and deposition time of 180min~500min.
[0012] In an optional embodiment, the process parameters for arc ion plating include: furnace temperature of 300°C, deposition gas pressure of 1 Pa, arc target current of 100 A, substrate bias voltage of -50 V, duty cycle of 70%, and deposition time of 185 min.
[0013] In an optional embodiment, the vacuum heat treatment temperature is 800℃~1000℃, and the holding time is 3h~5h.
[0014] In an optional embodiment, the vacuum heat treatment temperature is 900°C and the holding time is 4 hours.
[0015] In an optional implementation, after heat treatment, the mixture is cooled to room temperature using argon air cooling.
[0016] In an optional embodiment, prior to arc ion plating, the process further includes: polishing and cleaning the nickel-based superalloy substrate, followed by ion bombardment cleaning.
[0017] Thirdly, the present invention provides a hot-end component comprising a high-temperature protective coating according to any of the foregoing embodiments.
[0018] The beneficial effects of this invention include: The high-temperature protective coating provided by this invention comprises a nickel-based superalloy substrate and a NiAlHfR coating deposited on the surface of the nickel-based superalloy substrate, wherein R includes at least one of Y, Zr, La, Ce, and Dy; by atomic percentage, the NiAlHfR coating contains 38.9 at.% to 54.75 at.% Al, no more than 0.5 at.% Hf, and no more than 0.5 at.% R, with the balance being Ni. By adding an appropriate amount of active elements to the NiAlHf coating, the consumption of Al elements during high-temperature oxidation can be slowed down, the oxide film growth rate can be reduced, and the high-temperature oxidation resistance and service life of the coating can be improved. This high-temperature protective coating can be used for surface protection of aero-engines, gas turbines, and other high-temperature alloy hot-end components. Attached Figure Description
[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 The image shows a cross-sectional SEM image of the NiAlHfY coating prepared in Example 1. Figure 2 Here is a cross-sectional SEM image of the coating prepared in Comparative Example 2; Figure 3 In the test example, the SEM image of the NiAlHfY coating prepared in Example 1 after oxidation at 1200℃ for 400h is shown. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0022] The following is a detailed description of the high-temperature protective coating for mitigating Al consumption provided by the present invention, its preparation method, and its application.
[0023] The present invention provides a high-temperature protective coating for slowing down Al consumption. The high-temperature protective coating includes a nickel-based superalloy substrate and a NiAlHfR coating deposited on the surface of the nickel-based superalloy substrate, wherein R includes at least one of Y, Zr, La, Ce and Dy.
[0024] It should be noted that while NiAl coatings containing active elements can improve antioxidant properties to some extent, the type and amount of active elements added will affect the protective effect of the coating. If the amount of active elements added is inappropriate, it will be difficult to effectively slow down the consumption of Al elements in the coating, and may even affect the stability of the oxide film.
[0025] The active element R of this invention is at least one of Y, Zr, La, Ce and Dy, which has the advantages of low cost and can slow down the consumption of Al element in the coating and improve the stability of the oxide film with a low addition amount. If other commonly used active elements, such as Pt and Sc, are used as active elements, it will easily lead to an increase in the preparation cost of alloy target and coating, which is not conducive to large-scale engineering applications.
[0026] In this invention, the NiAlHfR coating contains 38.9 at.% to 54.75 at.% Al, 0% to 0.5 at.% Hf, and 0% to 0.5 at.% R, with the balance being Ni, by atomic percentage.
[0027] In some alternative embodiments, the Al content in the NiAlHfR coating can be 38.9 at.%, 39.0 at.%, 49.5 at.%, 49.55 at.%, 49.6 at.%, 49.65 at.%, 49.7 at.%, 49.75 at.%, 49.8 at.%, 49.85 at.%, 49.9 at.%, 49.99 at.%, 50.55 at.%, 51.55 at.%, 52.55 at.%, 53.55 at.%, 54.55 at.%, 54.70 at.%, or 54.75 at.%, or other values within the range of 38.9 at.% to 54.75 at.%.
[0028] If the Al content in the NiAlHfR coating is less than 38.9 at.%, it is easy for the Al content to fall below the stable range of β-NiAl single phase, and the microstructure will transform into β-NiAl+γ. -Ni3Al dual-phase, decreased temperature resistance, which is detrimental to improving the coating's high-temperature oxidation resistance, while β / γ Phase interface causes thermal stress, reducing the thermal cycling life of the coating. If the Al content is higher than 54.75 at.%, it is easy for the Al content to exceed the stable range of the β-NiAl single phase, and the microstructure will transform into a β-NiAl + δ-Al3Ni dual phase. δ-Al3Ni is a highly brittle intermetallic compound, which significantly reduces the plasticity and thermal shock resistance of the coating. Under thermal cycling conditions, microcracks are easy to initiate and propagate in the δ phase and phase interface. Moreover, the β / δ thermal expansion mismatch exacerbates the peeling of the oxide layer, and the interdiffusion at the interface is easy to induce Kirkendal voids, reducing the bonding strength of the coating.
[0029] The Hf content in the NiAlHfR coating can be 0%, 0.01at.%, 0.05at.%, 0.1at.%, 0.2at.%, 0.3at.%, 0.4at.%, or 0.5at.%, or other values within the range of 0% to 0.5at.%.
[0030] If the Hf content is higher than 0.5 at.%, it can easily lead to internal oxidation of the coating, which will damage the integrity of the oxide film and accelerate the oxidation and consumption of Al.
[0031] In some typical implementations, the Hf content in the NiAlHfR coating is 0.05 at.% to 0.5 at.%. Within this range, it can better promote the formation of the oxide film. The HfO2 dispersed at the Al2O3 / coating interface can effectively pin the Al2O3 grain boundaries, inhibit the formation of interface pores, and reduce oxide film peeling. If the Hf content in the NiAlHfR coating is less than 0.05 at.%, it may not play an effective role as an active element, resulting in limited pinning effect of the dispersed HfO2 particles on the alumina grain boundaries. Pores at the Al2O3 / coating interface are difficult to be effectively suppressed, and the static isothermal oxidation rate is relatively less affected.
[0032] In the NiAlHfR coating, the content of R can be 0%, 0.01at.%, 0.05at.%, 0.1at.%, 0.2at.%, 0.3at.%, 0.4at.%, or 0.5at.%, or other values within the range of 0% to 0.5at.%.
[0033] If the content of R is higher than 0.5 at.%, it is easy to cause an excess of active elements, forming and enriching oxides or second phases related to R elements, increasing the inhomogeneity of the coating and oxide film structure, causing severe internal oxidation, and accelerating the consumption of Al elements.
[0034] In some typical implementations, the content of element R in the NiAlHfR coating is 0.05 at.% to 0.4 at.%. Within this range, the consumption of element Al during long-term high-temperature oxidation can be better mitigated. If the content of R in the NiAlHfR coating is less than 0.05 at.%, it may not be able to fully exert its effect on improving the overall oxidation resistance of the coating, and its effect on mitigating the consumption of element Al will be reduced.
[0035] In some typical embodiments, the NiAlHfR coating contains, by atomic percentage, 49.55 at.% to 49.90 at.% Al, 0.05 at.% Hf, and 0.05 at.% to 0.4 at.% R, with the balance being Ni.
[0036] In some optional embodiments, the thickness of the NiAlHfR coating can be 20μm to 60μm, such as 20μm, 25μm, 28μm, 30μm, 32μm, 35μm, 40μm, 45μm, 50μm, 55μm or 60μm, or other values within the range of 20μm to 60μm.
[0037] If the thickness of the NiAlHfR coating is less than 20 μm, it is not conducive to the continuous formation of the protective Al2O3 oxide film during long-term high-temperature oxidation. If the thickness of the NiAlHfR coating is greater than 60 μm, it is not conducive to the stability of the coating, leading to an increase in residual stress inside the coating, increasing the risk of crack generation and local peeling, reducing the overall protective performance of the coating, and also increasing the preparation cost of the NiAlHfR coating.
[0038] In some typical implementations, the thickness of the NiAlHfR coating is 30 μm to 50 μm.
[0039] In an optional embodiment, after isothermal oxidation at 1200°C for 400 hours, the NiAlHfR coating contains 0%~20% Al-rich β-NiAl phase and 80%~100% γ′-Ni3Al phase. In some more typical embodiments, after isothermal oxidation at 1200°C for 400 hours, the NiAlHfR coating still contains Al-rich β-NiAl phase, such as its content being greater than 0% and ≤20%.
[0040] The aforementioned Al-rich β-NiAl phase can maintain the continuous formation of a protective Al2O3 oxide film during high-temperature oxidation. If the amount of Al-rich β-NiAl phase in the NiAlHfR coating is too small, it is not conducive to the continuous formation of a continuous and dense protective alumina on the surface of the coating during oxidation, resulting in a decrease in the protective performance of the coating.
[0041] As described above, the high-temperature protective coating provided by this invention can slow down the consumption of Al elements in the coating during high-temperature oxidation, reduce the growth rate of the oxide film, improve the stability of the oxide film and coating interface, improve the oxidation resistance of the coating, and retain a large amount of β-NiAl phase in the coating after oxidation, showing a good Al element retention effect.
[0042] Accordingly, the present invention also provides a method for preparing the above-mentioned high-temperature protective coating, comprising the following steps: depositing a NiAlHfR coating on the surface of a nickel-based high-temperature alloy substrate by arc ion plating, followed by vacuum heat treatment.
[0043] In some alternative implementations, prior to arc ion plating, the process further includes polishing and cleaning the nickel-based superalloy substrate, followed by ion bombardment cleaning.
[0044] The grinding and cleaning process may include: grinding the nickel-based superalloy substrate with sandpaper of grits of 800, 1200, and 2000 in sequence, followed by cleaning and drying.
[0045] Ion bombardment cleaning can be performed inside a vacuum coating equipment furnace, with the vacuum level set to 5×10⁻⁶. -3 Below Pa; after introducing Ar gas, the nickel-based superalloy matrix is subjected to ion bombardment cleaning, and the cleaning time can be 40 min.
[0046] In some optional embodiments, the process parameters for arc ion plating include: furnace temperature of 300℃~400℃, deposition gas pressure of 0.8Pa~1.2Pa, arc target current of 50A~120A, substrate bias voltage of -50V~-150V, duty cycle of 70%~90%, and deposition time of 180min~500min.
[0047] The furnace temperature can be 300℃, 320℃, 350℃, 380℃ or 400℃, or other values within the range of 300℃ to 400℃.
[0048] If the furnace temperature is below 300℃, the migration ability of deposited particles on the substrate surface will decrease, which is not conducive to the densification of the coating and the good bonding between the coating and the substrate. If the furnace temperature is above 400℃, the substrate temperature will rise during the deposition process, which will easily lead to the coarsening of the coating structure and may intensify the interdiffusion of elements between the coating and the substrate, which is not conducive to the stability of the coating structure and composition.
[0049] The deposition pressure can be 0.8 Pa, 0.9 Pa, 1.0 Pa, 1.1 Pa or 1.2 Pa, or other values in the range of 0.8 Pa to 1.2 Pa.
[0050] If the deposition gas pressure is below 0.8 Pa, the working gas content is low, which cannot maintain a stable plasma environment and affects the stability of the deposition process and the uniformity of the coating. If the deposition gas pressure is above 1.2 Pa, the collision frequency between the deposited particles and the gas particles during the transport process increases, which reduces the energy of the particles reaching the substrate surface and is not conducive to the formation of a dense coating.
[0051] The arc target current can be 50A, 60A, 70A, 80A, 90A, 100A, 110A or 120A, or other values within the range of 50A to 120A.
[0052] If the arc target current is below 50 A, the evaporation and ionization of the target material decrease, resulting in a lower deposition rate, which is not conducive to obtaining a coating with sufficient thickness and uniform composition. If the arc target current is above 120 A, the target material evaporates too violently, which can easily increase surface defects such as droplets and large particles, thus reducing the surface quality of the coating.
[0053] The substrate bias voltage can be -50V, -80V, -100V, -120V or -150V, or other values within the range of -50V to -150V.
[0054] If the absolute value of the substrate bias voltage is less than 50V, the acceleration of deposited particles and the ion bombardment effect on the substrate surface are weak, which is not conducive to improving the density and interfacial bonding performance of the coating. If the absolute value of the substrate bias voltage is greater than 150V, the ion bombardment effect is too strong, which can easily cause re-sputtering and may also increase the residual stress and defects inside the coating.
[0055] The duty cycle can be 70%, 75%, 80%, 85% or 90%, or other values within the range of 70% to 90%.
[0056] If the duty cycle is below 70%, the effective ion bombardment is insufficient, which is not conducive to the dense packing of deposited particles and the bonding between the coating and the substrate; if the duty cycle is above 90%, the strong ion bombardment and thermal effect may increase resputtering and residual stress, which is not conducive to the stability of the coating structure.
[0057] The deposition time can be 180 min, 200 min, 220 min, 250 min, 280 min, 300 min, 320 min, 340 min, 360 min, 380 min, 400 min, 420 min, 440 min, 460 min, 480 min, or 500 min, or other values within the range of 180 min to 500 min.
[0058] If the deposition time is less than 180 min, it is difficult to obtain a NiAlHfR coating of sufficient thickness. The insufficient Al content in the coating is not conducive to the continuous formation of the protective Al2O3 oxide film during long-term high-temperature oxidation. If the deposition time is longer than 500 min, the coating thickness will increase further, the deposition efficiency will decrease, and the residual stress and defects inside the coating may increase, which is not conducive to the long-term service of the coating.
[0059] In some typical implementations, the process parameters for arc ion plating include: furnace temperature of 300°C, deposition gas pressure of 1 Pa, arc target current of 100 A, substrate bias voltage of -50 V, duty cycle of 70%, and deposition time of 180 min.
[0060] In some alternative embodiments, the nominal composition of the target material used for arc ion plating is NiAl. z-x-y Hf x R y, wherein 0.0<x≤0.5, 0.0<y≤0.5, and 38.9≤z≤54.75. The content of each component of the target matches the content of elements in the NiAlHfR coating.
[0061] In some optional embodiments, the vacuum heat treatment is performed at 800°C to 1000°C for a holding time of 3 h to 5 h.
[0062] The temperature of the vacuum heat treatment may be 800°C, 850°C, 900°C, 950°C or 1000°C, or may also be other values within the range of 800°C to 1000°C.
[0063] The holding time of the vacuum heat treatment may be 3 h, 3.5 h, 4 h, 4.5 h or 5 h, or may also be other values within the range of 3 h to 5 h.
[0064] If the temperature of the vacuum heat treatment is lower than 800°C, it is unfavorable for element diffusion in the coating, homogenization of microstructure and composition in the coating, and interface bonding between the coating and the substrate. If the temperature of the vacuum heat treatment is higher than 1000°C, it is unfavorable for the controlled diffusion of elements between the coating and the substrate, which aggravates the diffusion of Al in the coating to the substrate and the diffusion of Ni in the substrate to the coating, resulting in thickening of the interdiffusion zone and the secondary reaction zone, leading to precipitation of TCP brittle phases inside the substrate and damaging the high-temperature mechanical properties of the single crystal substrate. If the holding time of the vacuum heat treatment is shorter than 3 h, it is unfavorable for element diffusion and homogenization of microstructure and composition in the coating, and is unfavorable for the stability of the β-NiAl phase and the formation of good interface bonding between the coating and the substrate. If the holding time of the vacuum heat treatment is longer than 5 h, it is unfavorable for the stability of the coating, which aggravates the diffusion of Al in the coating to the substrate and the diffusion of Ni in the substrate to the coating, causing the β-NiAl in the coating to transform to γ -Ni3Al and growth of TCP precipitates, impairing the high-temperature mechanical properties of the substrate.
[0065] In some more typical embodiments, the vacuum heat treatment is performed at 900°C for a holding time of 4 h.
[0066] Further, after the heat treatment is completed, cooling to room temperature is performed by argon air cooling.
[0067] In addition, the present invention further provides a hot end component, which includes the above high-temperature protective coating.
[0068] The features and properties of the present invention will be further described in detail below in conjunction with examples.
[0069] Example 1 This embodiment provides a high-temperature protective coating, which includes a nickel-based superalloy substrate and a NiAlHfR coating deposited on the surface of the nickel-based superalloy substrate. By atomic percentage, the NiAlHfR coating contains 49.90 at.% Al, 0.05 at.% Hf, and 0.05 at.% Y, with the balance being Ni. The thickness of the NiAlHfR coating is 33 μm.
[0070] The preparation method of this high-temperature protective coating includes the following steps: S1. Matrix pretreatment.
[0071] Using a nickel-based superalloy as the base material, it is processed to the required size and then polished with sandpaper of 800, 1200, and 2000 grit in sequence. After polishing, it is cleaned and dried.
[0072] S2, Ion bombardment cleaning.
[0073] The pretreated nickel-based superalloy substrate is placed in a vacuum coating equipment, and the vacuum chamber is evacuated to a vacuum level not exceeding 5 × 10⁻⁶. -3 Pa, argon gas is introduced to perform ion bombardment cleaning on the substrate surface for 40 minutes.
[0074] S3, Coating deposition.
[0075] Using Ni as the nominal composition 50 Al 49.90 Hf 0.05 Y 0.05 The alloy target material is used to deposit a NiAlHfY coating on the surface of a nickel-based superalloy substrate by arc ion plating.
[0076] The process parameters for arc ion plating are as follows: furnace temperature is 300℃, deposition gas pressure is 1Pa, arc target current is 100A, substrate bias voltage is -50V, duty cycle is 70%, and deposition time is 185min.
[0077] S4, Vacuum heat treatment.
[0078] The sample with the NiAlHfY coating was placed in a vacuum heat treatment furnace and held at 900℃ for 4 hours. After the heat treatment was completed, it was cooled to room temperature by argon air cooling.
[0079] The cross-sectional SEM image of the obtained NiAlHfY coating is shown below. Figure 1 As shown, by Figure 1 It can be seen that the coating thickness is 33μm and the internal structure of the coating is uniform.
[0080] Example 2 The difference between this embodiment and Embodiment 1 is that, by atomic percentage, the NiAlHfR coating contains 49.85 at.% Al, 0.05 at.% Hf, and 0.1 at.% Y, with the balance being Ni. The thickness of this NiAlHfR coating is 31 μm.
[0081] Example 3 The difference between this embodiment and Embodiment 1 is that, by atomic percentage, the NiAlHfR coating contains 49.8 at.% Al, 0.05 at.% Hf, and 0.15 at.% Y, with the balance being Ni. The thickness of this NiAlHfR coating is 31 μm.
[0082] Example 4 The difference between this embodiment and Embodiment 1 is that, by atomic percentage, the NiAlHfR coating contains 49.55 at.% Al, 0.05 at.% Hf, and 0.4 at.% Y, with the balance being Ni. The thickness of this NiAlHfR coating is 30 μm.
[0083] Example 5 The difference between this embodiment and Embodiment 1 is that the furnace temperature for arc ion plating is 300℃, the arc target current is 50A, the substrate bias voltage is -50V, the duty cycle is 70%, the deposition gas pressure is 0.8Pa, and the deposition time is 300min. The thickness of the resulting NiAlHfY coating is 50μm.
[0084] Example 6 The difference between this embodiment and Embodiment 1 is that the furnace temperature for arc ion plating is 400℃, the arc target current is 120A, the substrate bias voltage is -150V, the duty cycle is 90%, the deposition gas pressure is 1.2Pa, and the deposition time is 210min. The thickness of the resulting NiAlHfY coating is 30μm.
[0085] Example 7 The difference between this embodiment and Embodiment 1 is that the vacuum heat treatment temperature is 800℃, the holding time is 5 hours, and after the heat treatment, it is cooled to room temperature using argon air cooling. The thickness of the resulting NiAlHfY coating is 33 μm.
[0086] Example 8 The difference between this embodiment and Embodiment 1 is that the vacuum heat treatment temperature is 1000℃, the holding time is 3 hours, and after the heat treatment, it is cooled to room temperature by argon air cooling. The thickness of the resulting NiAlHfY coating is 32 μm.
[0087] Example 9 The difference between this embodiment and Embodiment 1 is that element R is replaced by Zr instead of Y. The resulting NiAlHfZr coating has a thickness of 33 μm.
[0088] Example 10 The difference between this embodiment and Embodiment 1 is that element R is replaced by Ce instead of Y. The thickness of the resulting NiAlHfCe coating is 33 μm.
[0089] Comparative Example 1 The difference between this comparative example and Example 1 is that the coating does not contain element R. The coating composition is Ni. 50 Al 49.95 Hf 0.05 The thickness of the resulting NiAlHf coating is 33 μm.
[0090] Comparative Example 2 The difference between this comparative example and Example 1 is that no vacuum heat treatment was performed.
[0091] The thickness of the obtained NiAlHfY coating is 33 μm.
[0092] The cross-sectional SEM image of the obtained coating is shown below. Figure 2 As shown, by Figure 2 It can be seen that there is a clear boundary between the untreated coating and the substrate, indicating that the coating has poor adhesion to the substrate.
[0093] Comparative Example 3 The difference between this comparative example and Example 1 is that the Y content is 0.005%, and the coating composition is Ni. 50 Al 49.945 Hf 0.05 Y 0.005 .
[0094] Comparative Example 4 The difference between this comparative example and Example 1 is that the Y content is 0.55% and the coating composition is Ni. 50 Al 49.4 Hf 0.05 Y 0.55 .
[0095] Comparative Example 5 The difference between this comparative example and Example 1 is that Y is replaced with an equal amount of Co, and its coating composition is Ni. 50 Al 49.9 Hf 0.05 Co 0.05 .
[0096] Comparative Example 6 The difference between this comparative example and Example 1 is that Y is replaced with an equal amount of Cr, and its coating composition is Ni. 50 Al 49.9 Hf 0.05 Cr 0.05 .
[0097] Comparative Example 7 The difference between this comparative example and Example 1 is that the deposition time in the arc ion plating is 120 min.
[0098] Comparative Example 8 The difference between this comparative example and Example 1 is that the heat treatment temperature during the vacuum heat treatment process is 500°C.
[0099] Test case The samples prepared in Examples 1-10 and Comparative Examples 1-8 were subjected to isothermal static oxidation tests. Specifically, the samples were placed in a muffle furnace at 1200℃ for isothermal oxidation for 400 hours. The results are shown in Table 1 and... Figure 3 As shown.
[0100] The cross-sectional SEM image after the isothermal static oxidation test corresponding to Example 1 is shown below. Figure 3 As shown, by Figure 3 It can be seen that the β-NiAl phase in the coating continuously transforms into the γ′-Ni3Al phase as the oxidation time increases. The β-NiAl phase accounts for about 17.82% of the coating, and the rest is the γ′-Ni3Al phase.
[0101] According to HB 5258-2000 "Test Method for Determination of Oxidation Resistance of Steel and High-Temperature Alloys", in Table 1, "Completely Antioxidant Grade" refers to an average oxidation rate of less than 0.1 g·m⁻¹. -2 ·h -1 "Antioxidant grade" refers to an average oxidation rate of 0.1~1.0 g·m³. -2 ·h -1 .
[0102] Table 1 Test Results
[0103] As can be seen from Table 1, the NiAlHfR coating provided by the present invention can effectively slow down the consumption of Al elements during high-temperature oxidation, reduce the growth rate of the oxide film, and improve the coating's resistance to high-temperature oxidation and service life.
[0104] In summary, by adding an appropriate amount of active elements to the NiAlHf coating and combining it with specific arc ion plating and vacuum heat treatment processes, this invention can effectively reduce the oxidative weight gain of the coating during high-temperature oxidation, slow down the consumption of Al elements, and improve the coating's resistance to high-temperature oxidation.
[0105] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-temperature protective coating that slows down Al consumption, characterized in that, The high-temperature protective coating includes a nickel-based superalloy substrate and a NiAlHfR coating deposited on the surface of the nickel-based superalloy substrate, wherein R includes at least one of Y, Zr, La, Ce and Dy; The NiAlHfR coating contains, by atomic percentage, 38.9 at.% to 54.75 at.% Al, 0% to 0.5 at.% Hf and 0% to 0.5 at.% R, with the balance being Ni.
2. The high-temperature protective coating according to claim 1, characterized in that, In the NiAlHfR coating, the content of R element is 0.05 at.% to 0.4 at.%; or, in the NiAlHfR coating, the content of Hf element is 0.05 at.% to 0.5 at.%.
3. The high-temperature protective coating according to claim 1, characterized in that, The thickness of the NiAlHfR coating is 20μm~60μm.
4. The high-temperature protective coating according to any one of claims 1 to 3, characterized in that, After being oxidized at a constant temperature of 1200℃ for 400 hours, the NiAlHfR coating contains 0%~20% of Al-rich β-NiAl phase and 80%~100% of γ′-Ni3Al phase.
5. A method for preparing the high-temperature protective coating according to any one of claims 1 to 4, characterized in that, Includes the following steps: The NiAlHfR coating was deposited on the surface of the nickel-based superalloy substrate using an arc ion plating method, followed by vacuum heat treatment.
6. The preparation method according to claim 5, characterized in that, The process parameters for arc ion plating include: furnace temperature of 300℃~400℃, deposition gas pressure of 0.8Pa~1.2Pa, arc target current of 50A~120A, substrate bias voltage of -50V~-150V, duty cycle of 70%~90%, and deposition time of 180min~500min.
7. The preparation method according to claim 6, characterized in that, The process parameters for arc ion plating include: furnace temperature of 300℃, deposition gas pressure of 1Pa, arc target current of 100A, substrate bias voltage of -50V, duty cycle of 70%, and deposition time of 185min.
8. The preparation method according to claim 5, characterized in that, The temperature for vacuum heat treatment is 800℃~1000℃, and the holding time is 3h~5h; Preferably, the vacuum heat treatment temperature is 900℃ and the holding time is 4h; Preferably, after heat treatment, the mixture is cooled to room temperature using argon air cooling.
9. The preparation method according to any one of claims 5 to 7, characterized in that, Before arc ion plating, the process also includes polishing and cleaning the nickel-based high-temperature alloy substrate, followed by ion bombardment cleaning.