Method for producing hydrogenated amorphous silicon film by ion beam sputtering and processing method, hydrogenated amorphous silicon film and application thereof

Hydrogenated amorphous silicon thin films were prepared by a three-beam ion synergistic coupling method, which solved the problems of high optical absorption, numerous defects, and poor refractive index stability in existing hydrogenated amorphous silicon thin films. This method enables the preparation of hydrogenated amorphous silicon thin films with high refractive index and low absorption, which are suitable for multilayer dielectric interference filters and improve the spectral performance of the filters.

CN123153012APending Publication Date: 2026-11-24FOSHAN IBD TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611533496.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing hydrogenated amorphous silicon thin films suffer from problems such as high optical absorption, numerous defects, poor refractive index stability, and significant angular effects during the preparation process, making it difficult to meet the requirements of low loss and large-angle applications for high-precision filters.

Method used

A three-beam ion synergistic coupling method is adopted to prepare a hydrogenated amorphous silicon film with high refractive index and low absorption by simultaneously using a main sputtering ion source, an auxiliary ion source and a hydrogen pyrolysis auxiliary ion source. Silicon sputtering particles are generated by bombarding the silicon target with an argon-hydrogen mixed gas, the auxiliary ion source is used for surface modification, and the hydrogen pyrolysis auxiliary ion source generates active hydrogen particles. Combined with radio frequency bias control, in-situ hydrogenation and densification improvement of the film are achieved.

Benefits of technology

Hydrogenated amorphous silicon thin films with high refractive index, ultra-low extinction coefficient, and low surface roughness were prepared. These films are suitable for multilayer dielectric interference filters, improving the angular effect of the filters, widening the cutoff band range, and reducing the light absorption loss of optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153012A_ABST
    Figure CN123153012A_ABST
Patent Text Reader

Abstract

This application provides a method and processing system for preparing hydrogenated amorphous silicon films by ion beam sputtering, as well as the hydrogenated amorphous silicon films and their applications. The method includes: preparing a substrate to be coated and a silicon target; starting a main sputtering ion source to bombard the silicon target and generate silicon sputtered particles; starting an auxiliary ion source to perform particle bombardment modification on the substrate surface; starting a hydrogen pyrolysis auxiliary ion source to pyrolyze hydrogen-containing gas to generate active hydrogen ions; through the synergistic effect of the three ion beams from the main sputtering ion source, the auxiliary ion source, and the hydrogen pyrolysis auxiliary ion source, the active hydrogen ions react with the silicon sputtered particles on the substrate surface to complete in-situ hydrogenation, and depositing the target high-refractive-index, low-absorption hydrogenated amorphous silicon film on the substrate surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of optical thin film material preparation technology, specifically to a method for preparing hydrogenated amorphous silicon films by ion beam sputtering, the processing method thereof, hydrogenated amorphous silicon films and their applications. Background Technology

[0002] With the rapid development of precision optical imaging, laser detection, and optical communication technologies, the application scenarios of wide-angle incident filters are constantly expanding, placing higher demands on the large-angle spectral stability, cutoff band width, and fabrication efficiency of filters. The angle effect of filters is the core issue restricting the performance of filters in large-angle applications: conventional high-refractive-index thin film materials such as tantalum pentoxide, titanium dioxide, and hafnium oxide generally have refractive indices below 2.3, and the refractive index ratio of high- and low-refractive-index materials is relatively small. To achieve the target cutoff bandwidth, a film structure of dozens or even hundreds of layers needs to be designed, resulting in a large total film thickness, long fabrication cycle, and low production efficiency. At the same time, the increase in film thickness will further aggravate the spectral shift and passband contraction under large-angle incident conditions, making it impossible to meet the filtering performance requirements under large-angle conditions.

[0003] Hydrogenated amorphous silicon (a-Si:H) is an optical thin film material with an ultra-high refractive index, exceeding 3.5 in the visible to near-infrared band, far surpassing traditional high-refractive-index oxide materials. When hydrogenated amorphous silicon is used as a high-refractive-index film layer in interference filters, the refractive index ratio of the high- and low-refractive-index materials is significantly improved. This allows for a wider cutoff band with fewer film layers, drastically reducing the overall film thickness, effectively mitigating the angular effect of the filter, and significantly shortening deposition time and improving production efficiency. Currently, the mainstream preparation methods for hydrogenated amorphous silicon thin films include plasma-enhanced chemical vapor deposition (PECVD) and magnetron sputtering. PECVD relies on flammable and explosive gas sources such as silanes, posing a high safety risk, and produces thin films with low density, numerous defects, and insufficient laser damage threshold. Magnetron sputtering produces thin films with poor controllability of hydrogen content, high defect state density, and large optical absorption loss, failing to meet the low-loss requirements of high-precision filters.

[0004] Ion beam sputtering technology boasts significant advantages such as high thin film density, high thickness control precision, and good batch stability, making it a core process for fabricating high-precision optical thin films. However, when using ion beam sputtering to prepare hydrogenated amorphous silicon thin films, the precise introduction of hydrogen and the control of bonding within the silicon-based network present technical challenges. This makes it difficult to simultaneously achieve high refractive index and low absorption performance, thus limiting the large-scale application of such films in low-angle, wide-angle filters. Summary of the Invention

[0005] To address the shortcomings of existing hydrogenated amorphous silicon thin films, such as high optical absorption, numerous defects, poor refractive index stability, and significant angular effects, this application provides a method for preparing hydrogenated amorphous silicon films by ion beam sputtering, the hydrogenated amorphous silicon films themselves, and their applications. Through the synergistic coupling of three ion beams, high-quality hydrogenated amorphous silicon thin films with high refractive index, ultra-low extinction coefficient, and low surface roughness are obtained, which are suitable for the application requirements of multilayer dielectric interference filters.

[0006] To achieve the above objectives, this application provides the following technical solution: As a first aspect, this application relates to a method for preparing a high-refractive-index, low-absorption hydrogenated amorphous silicon film by ion beam sputtering, which includes the following steps: Prepare the substrate to be coated and the silicon target; The main sputtering ion source, the auxiliary ion source, and the hydrogen pyrolysis auxiliary ion source are started simultaneously. The main sputtering ion source bombards the silicon target to generate silicon sputtering particles. The auxiliary ion source is used to perform particle bombardment modification on the substrate surface. The hydrogen pyrolysis auxiliary ion source is used to pyrolyze hydrogen-containing gas to generate active hydrogen particles. Through the synergistic effect of three ion beams—the main sputtering ion source, the auxiliary ion source, and the hydrogen pyrolysis auxiliary ion source—active hydrogen particles react with silicon sputtering particles on the substrate surface, completing in-situ hydrogenation and depositing the target high-refractive-index, low-absorption hydrogenated amorphous silicon film on the substrate surface.

[0007] Further setting: The purity of the silicon target material is greater than 4N.

[0008] Further settings: The main sputtering ion source uses an argon-hydrogen mixture with a gas flow rate of 10~50 sccm and an ion acceleration voltage of 100~1500V.

[0009] Further settings: The auxiliary ion source uses an argon-hydrogen mixture with a gas flow rate of 0~50 sccm and an ion acceleration voltage of 100~1000V.

[0010] Further settings: The hydrogen cracking auxiliary ion source uses high-purity hydrogen gas, with a gas flow rate of 0~50 sccm and a working power of 0~500W.

[0011] Further settings include a step of applying and controlling an RF bias voltage to the substrate, with the RF bias voltage power being 0~500W.

[0012] Further settings: The baseline vacuum of the system before deposition is 1×10⁻⁶. -4 Pa ~ 1×10 -2 Pa, the deposition temperature of the substrate to be coated is 100~250℃.

[0013] Further settings: After the amorphous silicon film is deposited, annealing is performed at a temperature of 300~350℃ and a holding time of 60~120min.

[0014] As a second aspect, this application relates to a processing system for preparing high refractive index, low absorption hydrogenated amorphous silicon films by ion beam sputtering, which is applicable to the above-mentioned method for preparing high refractive index, low absorption hydrogenated amorphous silicon films by ion beam sputtering. The processing system includes a vacuum chamber and a silicon target, a main sputtering ion source, an auxiliary ion source, and a hydrogen pyrolysis auxiliary ion source disposed within the vacuum chamber. A substrate station is provided inside the vacuum chamber for placing the substrate to be coated. The ion beam outlet of the main sputtering ion source faces the silicon target, and the silicon sputtered particles generated by the silicon target are directed towards the substrate station. The ion beam outlet of the auxiliary ion source faces the substrate station, and the particle exit port of the hydrogen pyrolysis auxiliary ion source faces the substrate station. The main sputtering ion source, auxiliary ion source, and hydrogen pyrolysis auxiliary ion source are configured to be activated simultaneously to deposit a hydrogenated amorphous silicon thin film on the substrate surface.

[0015] As a third aspect, this application relates to a hydrogenated amorphous silicon film, which is prepared by the above-described method for preparing a high-refractive-index, low-absorption hydrogenated amorphous silicon film by ion beam sputtering. The hydrogenated amorphous silicon film has a refractive index ≥ 3.45 and an extinction coefficient k ≤ 1 × 10⁻⁶ in the visible to infrared band. -4 Surface roughness < 0.5 nm.

[0016] As a fourth aspect, this application relates to the application of a hydrogenated amorphous silicon film in a multilayer dielectric interference filter, wherein the hydrogenated amorphous silicon film is the aforementioned hydrogenated amorphous silicon film, or the hydrogenated amorphous silicon film is prepared by the aforementioned method for preparing a high refractive index, low absorption hydrogenated amorphous silicon film by ion beam sputtering.

[0017] Compared with existing technologies, the solution in this application has the following advantages: 1. In the method for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering disclosed in this application, three ion beams—a main sputtering ion source, an auxiliary ion source, and a hydrogen pyrolysis auxiliary ion source—work synergistically. The main sputtering ion source uses an argon-hydrogen mixture as the working gas to bombard the silicon target, providing the sputtering particles required for film formation. The auxiliary ion source outputs a low-energy ion beam to bombard and modify the surface of the growing film, improving its density. The hydrogen pyrolysis auxiliary ion source generates high-density active hydrogen particles by pyrolyzing high-purity hydrogen gas. Simultaneously, the hydrogen in the working gas used by the main sputtering ion source and the auxiliary ion source forms a dual hydrogenation system, thereby achieving thorough and uniform hydrogenation of the film from the surface to the interior. This method can efficiently passivate silicon dangling bond defects to reduce film light absorption and prevent excessive hydrogenation from causing a decrease in refractive index, thus stably preparing hydrogenated amorphous silicon films with both high refractive index and low absorptivity.

[0018] 2. In the method for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering involved in this application, a radio frequency bias voltage can be applied to the substrate during the deposition process. The radio frequency bias voltage forms a controllable negative bias electric field on the substrate surface, thereby regulating the movement of incident silicon sputtered particles and active hydrogen particles.

[0019] 3. In the method for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering involved in this application, both the main sputtering ion source and the auxiliary ion source use an argon-hydrogen mixture as the working gas. After ionization, argon gas can form high-energy argon ions, which can ensure the sputtering yield of silicon target material and the stable discharge of ion source. After ionization, hydrogen active particles are obtained, which can achieve shallow in-situ pre-hydrogenation during film growth. Together with the hydrogen pyrolysis auxiliary ion source, silicon dangling bonds are passivated, while silicon oxide impurity defects are suppressed, which is beneficial for preparing low-absorption films.

[0020] 4. The hydrogenated amorphous silicon film prepared by ion beam sputtering exhibits high refractive index, low absorption, and excellent surface quality in the visible-infrared operating band. It can be applied to multilayer dielectric interference filters, especially suitable for optical components with high requirements for film refractive index, absorption loss, and surface flatness, such as large-angle filters and wide-cutoff-band interference filters. Using this hydrogenated amorphous silicon film as a high-refractive-index layer in a multilayer film system can improve the angle effect of the filter, broaden the cutoff band range, reduce the overall light absorption loss of the device, and improve the spectral performance of the filter.

[0021] Additional aspects and advantages of this application will be set forth in part in the description which follows, and will become apparent from the description or may be learned by practice of this application. Attached Figure Description

[0022] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the following description of the embodiments taken in conjunction with the accompanying drawings, wherein: Figure 1 A schematic diagram of the processing system for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to this application; Figure 2 Visible-near-infrared transmission spectrum of hydrogenated amorphous silicon film on JGS1 quartz substrate surface; Figure 3 The dispersion curve of the refractive index of the hydrogenated amorphous silicon film as a function of wavelength; Figure 4 The extinction coefficient of the hydrogenated amorphous silicon film varies with wavelength. Figure 5 The transmission spectra of hydrogenated amorphous silicon films before and after water boiling aging are compared. Figure 6An atomic force microscope image of the surface morphology of a hydrogenated amorphous silicon film; Figure 7 The images show the transmission spectra of thin film samples from multiple embodiments.

[0023] In the figure, 1 is the vacuum chamber; 2 is the substrate; 3 is the main sputtering ion source; 4 is the silicon target; 5 is the auxiliary ion source; and 6 is the hydrogen pyrolysis auxiliary ion source. Detailed Implementation

[0024] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0025] It should be understood that the various steps described in the method embodiments of the present invention may be performed in different orders and / or in parallel. Furthermore, the method embodiments may include additional steps and / or omit the steps shown. The scope of the present invention is not limited in this respect.

[0026] The term "comprising" and its variations as used herein are open-ended, meaning "including but not limited to". The term "connection" can refer to a direct connection or an indirect connection via intermediate components (elements). The term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one additional embodiment"; the term "some embodiments" means "at least some embodiments". Definitions of other terms will be given in the following description.

[0027] It should be noted that the concepts of "first" and "second" mentioned in this invention are only used to distinguish between devices, modules or units, and are not intended to limit these devices, modules or units to necessarily be different devices, modules or units, nor are they intended to limit the order or interdependence of the functions performed by these devices, modules or units.

[0028] Please combine Figure 1 This application discloses a processing system for preparing high refractive index and low absorption hydrogenated amorphous silicon films by ion beam sputtering. The system includes a vacuum chamber 1 and a silicon target 4, a main sputtering ion source 3, an auxiliary ion source 5 and a hydrogen cracking auxiliary ion source 6 disposed in the vacuum chamber 1. At the same time, a substrate station is provided inside the vacuum chamber 1 for placing the substrate 2 to be coated.

[0029] Specifically, the main sputtering ion source 3 is arranged on the side wall of the vacuum chamber 1, with its ion beam outlet facing the silicon target 4. The main sputtering ion source 3 outputs an ion beam to bombard the silicon target 4, generating silicon sputtered particles. The transport direction of these silicon sputtered particles is towards the substrate, providing a silicon source for thin film growth. The auxiliary ion source 5 is mounted on the top of the vacuum chamber 1, with its ion beam outlet facing the substrate. It outputs a low-energy ion beam to the substrate 2 and the growing thin film, activating the surface of the substrate 2 and dynamically bombarding the film to improve the density of the deposited film. The hydrogen pyrolysis auxiliary ion source 6 is located at the bottom of the vacuum chamber 1, with its particle exit port facing the substrate. The hydrogen pyrolysis auxiliary ion source 6 pyrolyzes hydrogen gas to generate high-density, directional active hydrogen particles. These active hydrogen particles act on the substrate film-forming interface, undergoing an in-situ hydrogenation reaction with the silicon sputtered particles, passivating silicon dangling bonds and defect states within the thin film.

[0030] In this application, the main sputtering ion source 3, the auxiliary ion source 5, and the hydrogen pyrolysis auxiliary ion source 6 are configured to be activated simultaneously, with the three ion sources working together to deposit hydrogenated amorphous silicon thin films on the surface of the substrate 2. Alternatively, depending on the requirements for thin film performance control, some of the ion sources can be selectively activated to achieve the preparation of thin films with different hydrogenation levels.

[0031] Furthermore, the substrate station is equipped with a heating unit and an RF bias application unit. The heating unit can heat the substrate 2 to be coated, thereby controlling the deposition temperature and regulating the nucleation and growth behavior of the thin film. The RF bias application unit can apply an RF bias to the substrate 2 to control the ion energy at the deposition interface, thereby optimizing the film density and defect state density. During the deposition process, the heating unit and the RF bias application unit can be turned on or off according to the film performance requirements.

[0032] Based on the above-mentioned processing system for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering, this application also discloses a method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering, the specific steps of which are as follows: S1. Prepare the substrate 2 to be coated and the silicon target 4.

[0033] Fused silica or K9 optical glass was selected as the substrate 2 to be coated. The substrate 2 was ultrasonically cleaned with acetone and anhydrous ethanol in sequence, followed by cleaning with deionized water. After cleaning, it was dried with high-purity nitrogen and then sent to a vacuum oven to dry in order to remove particles, oil, organic residues and other contaminants from the surface of the substrate 2.

[0034] The silicon target 4 is made of high-purity single-crystal silicon with a purity greater than 4N, meaning the total impurity content is less than 100ppm. At this purity, the content of metal impurities, oxygen impurities, and carbon impurities inside the target is low, which can reduce the number of impurity atoms sputtered into the hydrogenated amorphous silicon film during the ion beam sputtering process.

[0035] The substrate 2 to be coated and the silicon target 4 are installed into the vacuum chamber 1 and clamped. The substrate 2 to be coated is installed at the substrate station. The vacuum chamber 1 is closed, and the vacuum system is evacuated to achieve a base vacuum of 1×10⁻⁶ before deposition. -4 Pa ~ 1×10 -2 Pa.

[0036] Furthermore, since the silicon target 4 is prone to forming a surface oxide layer when exposed to the atmospheric environment, it needs to be pre-sputtered before deposition to remove the oxide layer on the target surface and prevent oxygen impurities in the oxide layer from being sputtered into the hydrogenated amorphous silicon film, thus reducing film defects. During the pre-sputtering process of the silicon target 4, a baffle is used to completely shield the substrate 2, and the main sputtering ion source 3 is turned on to bombard the silicon target 4 to remove the natural oxide layer and residual contaminants on the target surface. The baffle can prevent oxygen-containing impurities and particles generated during the pre-sputtering process from sputtering onto the surface of the substrate 2 and causing contamination to the substrate 2.

[0037] After pre-sputtering, the baffle is removed, and the substrate 2 to be coated is heated and stabilized at 100~250℃. In this application, the substrate 2 is heated and stabilized at 100~250℃ during the deposition process. This rapidly removes adsorbed moisture and residual gases from the surface of the substrate 2, reducing film impurity defects. Simultaneously, the increased temperature enhances the surface migration ability of silicon sputtered particles reaching the substrate 2 and facilitates the diffusion of active hydrogen particles within the grown film, thus improving hydrogenation uniformity. However, it is important to control the temperature carefully to prevent excessive heat from causing Si-H bond dissociation.

[0038] After the substrate temperature stabilizes, the hydrogen pyrolysis auxiliary ion source 6 is activated separately to perform active hydrogen plasma cleaning on the substrate surface to be coated. The pre-cleaning time is 120 seconds, using high-density active hydrogen particles to further passivate dangling bonds on the substrate surface and remove trace surface impurities. After pre-cleaning, a certain time interval needs to be allowed to allow the plasma state and particle concentration inside the chamber to stabilize, eliminating the interference of residual pre-cleaning effects on the initial film formation interface. Then, the deposition process can proceed.

[0039] S2. Simultaneously start the main sputtering ion source 3, the auxiliary ion source 5, and the hydrogen pyrolysis auxiliary ion source 6. The main sputtering ion source 3 bombards the silicon target 4 to generate silicon sputtering particles, the auxiliary ion source 5 is used to perform particle bombardment modification on the substrate surface, and the hydrogen pyrolysis auxiliary ion source 6 is used to pyrolyze hydrogen-containing gas to generate active hydrogen particles.

[0040] The main sputtering ion source 3, auxiliary ion source 5, and hydrogen pyrolysis auxiliary ion source 6 are activated simultaneously to achieve synergistic effects of three ion beams. The main sputtering ion source 3 uses an argon-hydrogen mixture as its working gas. Under set gas flow rates and ion acceleration voltage conditions, the high-energy argon-hydrogen mixed ion beam generated by ionization bombards the silicon target 4 to produce silicon sputtered particles. These silicon sputtered particles are directionally transported to the surface of the substrate 2 under vacuum conditions to deposit a thin film on the substrate 2 surface. The auxiliary ion source 5 also uses an argon-hydrogen mixture as its working gas. Under set gas flow rates and corresponding ion acceleration voltage conditions, it generates low-energy ion beams... The continuous bombardment of the sub-beams on the surface of substrate 2 can activate the surface of substrate 2, improve the microstructure of the surface of substrate 2, and perform dynamic bombardment modification on the growing film to avoid the generation of defects such as looseness, pores and microcracks in the film, effectively improving the density and uniformity of the film. The hydrogen cracking auxiliary ion source 6 uses high-purity hydrogen gas as the working gas and performs efficient cracking of hydrogen gas through radio frequency or microwave plasma excitation. The high-density active hydrogen particles generated react with silicon sputtering particles on the surface of substrate 2 to complete in-situ hydrogenation, so as to deposit a hydrogenated amorphous silicon film with high refractive index and low absorption on the surface of substrate 2.

[0041] This application utilizes in-situ hydrogenation during the deposition process. High-density active hydrogen ions directly combine with numerous unsaturated silicon dangling bonds generated during the deposition of the amorphous silicon network by silicon sputtering particles to form Si-H bonds, reducing defect state density and minimizing light absorption loss. Furthermore, simultaneous hydrogen doping during film growth ensures uniform distribution of hydrogen within the film, regulating the random silicon network, suppressing local crystallization, and guaranteeing the high refractive index and low absorption optical properties of the hydrogenated amorphous silicon film. Simultaneously, the continuous bombardment of the substrate surface by the auxiliary ion source 5 promotes the migration of active hydrogen particles into the film interior, further enhancing the efficiency of in-situ hydrogenation.

[0042] In addition, both the main sputtering ion source 3 and the auxiliary ion source 5 use an argon-hydrogen mixture as their working gas. Argon ions obtained by ionization have the advantages of high mass and high momentum. The main sputtering ion source 3 mainly relies on argon ions to bombard the silicon target 4, thereby obtaining sufficient silicon sputtered particles. The auxiliary ion source 5, on the other hand, relies on argon ions to achieve low-energy bombardment of the grown film, improving the film density. The hydrogen in the mixture can be decomposed in the plasma environment of the ion source to generate some active hydrogen, which is used to replenish hydrogen at the interface at the moment of silicon sputtered particle deposition. This forms a dual hydrogenation system with the hydrogen decomposition auxiliary ion source 6. The two work together to effectively eliminate film defects, reduce parasitic light absorption, and thus improve the hydrogenation uniformity and process stability of the film layer.

[0043] Specifically, the gas flow rate of the main sputtering ion source is 10~50 sccm. This flow rate range can ensure stable plasma discharge and sufficient sputtering rate, while also providing an appropriate amount of hydrogen ions to participate in primary hydrogenation, avoiding a sharp drop in sputtering yield due to excessive hydrogen content. The ion acceleration voltage is 100~1500V, where lower voltage (100~300 V) is suitable for low-damage deposition, while higher voltage (800~1500 V) is beneficial for improving the kinetic energy of silicon particles and the density of the film.

[0044] The gas flow rate of the auxiliary ion source 5 can be adjusted within the range of 0~50 sccm. Within this range, the auxiliary ion source 5 can perform low-energy ion bombardment modification on the thin film during the growth process. When the gas flow rate is 0 sccm, the auxiliary ion source 5 can use the residual argon gas in the vacuum chamber 1 to perform weak discharge, and the resulting low-energy argon ion beam continues to activate the surface of the thin film. The ion acceleration voltage of the auxiliary ion source 5 is 100~1000V. In this embodiment, it is preferably controlled in the low-energy range of 100~200V. When the acceleration voltage exceeds 500V, although it can enhance the activation effect on the surface of the substrate 2, the ion beam bombardment energy is too high, which can easily produce a strong etching effect on the growing thin film and easily cause lattice damage to the thin film.

[0045] The hydrogen cracking auxiliary ion source 6 has a gas flow rate of 0-50 sccm and an operating power range of 0-500 W. Higher operating power results in higher hydrogen cracking efficiency and higher active hydrogen density, which is beneficial for achieving bulk hydrogenation with high hydrogen content and low defect density. However, excessive power may lead to plasma damage. When the flow rate is 0 sccm and the operating power is 0 W, the hydrogen cracking auxiliary ion source 5 is in the off state, suitable for the preparation of thin films with low hydrogen content.

[0046] In addition, during the deposition process, a radio frequency (RF) bias can be applied to the substrate 2 for regulation. The RF bias can form a controllable negative bias electric field on the surface of the substrate 2 to regulate the motion energy and migration behavior of the deposited silicon sputtered particles and active hydrogen particles. This can enhance the surface diffusion and migration ability of the deposited particles, promote the filling of microscopic pores and gaps in the thin film by silicon sputtered particles, and further improve the overall density and uniformity of the thin film. The power range of the RF bias in this application is between 0 and 500 W. When the RF bias power is 0 W, the substrate 2 is in a state without bias, and the deposited particles are naturally deposited by vacuum transport, without any electric field regulation effect. When an RF bias power greater than 0 is applied, the particle migration is enhanced by the electric field, and active hydrogen is driven to diffuse into the interior of the thin film, improving the bulk hydrogenation effect of the thin film. In this embodiment, the RF bias power is preferably controlled in the low-to-medium power range of 50 to 200 W, which can form a moderate negative bias electric field and drive the active hydrogen particles to migrate and diffuse into the interior of the thin film, further improving the hydrogenation uniformity of the film layer.

[0047] S3. After the amorphous silicon film is deposited, it is annealed at a temperature of 300~350℃ for 60~120min.

[0048] Although the deposited hydrogenated amorphous silicon film has undergone in-situ hydrogenation, a small number of unpassivated silicon dangling bonds and metastable Si-H bonds remain within the film. Annealing within this temperature range can further reduce parasitic light absorption, eliminate localized areas of insufficient hydrogenation, further stabilize the Si-H bond structure, and improve the film's optical stability. Simultaneously, annealing can moderately release the internal stress accumulated during the film deposition process, improving the film's mechanical stability. Thus, without damaging the amorphous structure of the film or causing significant hydrogen desorption, parasitic light absorption is eliminated to the greatest extent, achieving ultra-low absorption optical performance.

[0049] It should be noted that this application can directly obtain a hydrogenated amorphous silicon film through the three-beam ion synergistic in-situ hydrogenation deposition in step S2, resulting in a target thin film with high refractive index and low absorption characteristics. The annealing treatment in step S3 is an optional post-processing optimization step and is not a necessary step for forming a hydrogenated amorphous silicon film. If the annealing treatment is not performed, the deposited thin film can still achieve the basic optical indicators of this application.

[0050] To verify the effect of the three-beam ion synergistic in-situ hydrogenation process on the overall performance improvement of the thin film, and to verify whether the thin film achieves the design goals of high refractive index and low absorption, the optical parameters and surface morphology of the prepared thin film samples were characterized, as follows: (1) Thin film transmittance spectrum test The transmission spectrum of the hydrogenated amorphous silicon film sample prepared by the above method was measured using a PHOTONRT spectrophotometer. The test wavelength range was 380 nm to 5000 nm. Before the test, a blank substrate was used for baseline calibration to eliminate the interference of substrate, environmental and system errors on the test results.

[0051] The substrate 2 with the hydrogenated amorphous silicon film deposited is placed in the test optical path, and the transmission spectrum of the thin film sample in a continuous wavelength range is collected to obtain the characteristic curve of the transmittance as a function of wavelength. Based on the inversion fitting of the transmittance curve, the refractive index and extinction coefficient of the obtained hydrogenated silicon thin film are calculated.

[0052] Please see Figure 2The figure reflects the visible-near-infrared transmission spectrum of the hydrogenated amorphous silicon film on the JGS1 quartz substrate. The film exhibits significant light absorption and low transmittance in the short-wavelength range of 400–600 nm. It displays regular interference oscillation characteristics in the 600–1650 nm range, and the refractive index and extinction coefficient of the film can be obtained by fitting the interference spectrum. The transmittance reaches its highest value near 1650 nm, indicating that the film has low parasitic absorption in this band, which confirms that the hydrogenated amorphous silicon film prepared in this application has excellent optical properties with low absorption.

[0053] Figure 3 The dispersion curves of the refractive index of the hydrogenated amorphous silicon film as a function of wavelength show that the film exhibits normal dispersion characteristics within the test wavelength range of 680–1680 nm. Specifically, the refractive index is higher in the shorter wavelength regions, gradually decreasing with increasing wavelength. After wavelengths exceed 1300 nm, the refractive index tends to stabilize above 3.4, demonstrating that the film prepared in this application possesses excellent high refractive index characteristics in the near-infrared band. The smooth and uniform curve trend indicates that the film has uniform composition and a dense microstructure, making it suitable for applications requiring large-angle filters and wide-cutoff interference filters.

[0054] Figure 4 The curve shows the extinction coefficient of the hydrogenated amorphous silicon film as a function of wavelength. In the visible light range of 680–1080 nm, the extinction coefficient decreases rapidly with increasing wavelength. In the near-infrared region with wavelengths greater than 1080 nm, the extinction coefficient approaches zero, and the parasitic light absorption of the film is extremely weak. This demonstrates that the hydrogenated amorphous silicon film prepared in this application has excellent low absorption characteristics in the near-infrared working band, which can reduce the light energy loss of the filter device and improve the optical performance of the device.

[0055] Figure 5 The transmission spectrum comparison curves of the hydrogenated amorphous silicon film after water boiling aging are used to verify the damp heat resistance stability of the film prepared in this application. The blue dashed line in the figure represents the film sample before boiling, and the red dashed line represents the film sample after boiling. It can be seen from the figure that the two curves before and after boiling almost overlap, and the positions of the interference peaks and valleys are basically consistent, with only a very small deviation. That is, the optical properties of the film prepared in this application did not deteriorate after the water boiling test, indicating that the hydrogenated amorphous silicon film prepared in this application has a dense film structure, a reliable interface adhesion, and excellent stability in damp heat environment, and can be adapted to the complex working scenarios of various optical devices for a long time.

[0056] (2) Thin film surface roughness and optical signal-to-noise ratio test Atomic force microscopy was used to characterize the microstructure of the obtained amorphous silicon film and to measure its roughness. The roughness test was used to verify the compactness of the film layer, demonstrating that the light scattering loss at the film interface is weak and unnecessary optical absorption is reduced, thus synergistically confirming the excellent low absorption characteristics of the film prepared in this application.

[0057] Figure 6 The image shows the surface morphology of the hydrogenated amorphous silicon film obtained by atomic force microscopy, with a scanning area of ​​5 μm × 5 μm. As can be seen from the morphology image, the film surface exhibits fine and uniform particles, without obvious large particle protrusions or pore defects, indicating good film density. Furthermore, the root mean square roughness Sq of the film was calculated using software. In this embodiment, the measured root mean square roughness Sq is only 110.949 pm, and the arithmetic mean roughness Sa is 82.535 pm, indicating that the surface undulations are in the sub-nanometer range. The small extreme value difference in morphology and the absence of obvious pores and large particle defects demonstrate that the hydrogenated amorphous silicon film prepared in this application has excellent surface smoothness, which can significantly reduce interfacial light scattering loss.

[0058] Furthermore, based on the preceding transmission spectrum test data, the optical signal-to-noise ratio can be calculated using the 1200-1600 nm wavelength range. The average transmittance within this range is taken as the effective signal, and the standard deviation of transmittance fluctuation is used as noise for calculation. The thin film surface of this application is smooth, resulting in low scattering noise and a high optical signal-to-noise ratio, ensuring the reliability of the refractive index and extinction coefficient inversion results.

[0059] (3) High temperature and high humidity reliability test The hydrogenated amorphous silicon film sample was placed in a high-temperature and high-humidity test chamber, and the test conditions were set to 85℃ and 85%RH for constant humidity and heat accelerated aging test. After the test, the film sample was removed, and the transmission spectrum and surface roughness of the film were tested again. The changes in the optical curve and surface morphology of the film before and after the aging test were compared to verify the working stability of the film under high temperature and high humidity environment. Then, the film's resistance to water vapor erosion and the bonding strength between the film and the substrate were tested.

[0060] If the transmission spectrum and roughness of the thin film do not deteriorate significantly after high temperature and humidity aging at 85°C, it can be proven that the hydrogenated amorphous silicon film prepared in this application has excellent moisture and heat resistance reliability.

[0061] The hydrogenated amorphous silicon film prepared by the above-described method for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering exhibits high refractive index, low absorption, and excellent surface quality in the visible-infrared working band. The amorphous silicon film of this application has a refractive index of not less than 3.45 in the visible-infrared band and an extinction coefficient k ≤ 1 × 10⁻⁶. -4 The surface roughness is less than 0.5 nm. This application possesses a high refractive index, which allows for a larger refractive index difference with low-refractive-index layers in a multilayer dielectric film structure. For large-angle filters and wide-cutoff-band interference filters, a larger refractive index difference is beneficial for suppressing angle shifts, improving low-angle effects, and reducing the number of stacked layers. The extinction coefficient k of the amorphous silicon film in this application is ≤1×10⁻⁶. -4The amorphous silicon film exhibits extremely low absorption levels, meaning that the absorption loss of light energy in the working wavelength band is minimal. Therefore, when applied to optical filters, this avoids signal attenuation and device heating caused by the film's own absorption, thus improving the filter's signal-to-noise ratio. This makes it suitable for infrared beam splitting and imaging optical systems sensitive to light loss. Furthermore, the amorphous silicon film has a surface roughness of less than 0.5 nm, which is a sub-nanometer level flat surface. The small surface undulations significantly reduce interfacial scattering losses and also improve the adhesion and interface quality of subsequent layered films.

[0062] The amorphous silicon film prepared in this application can be used in multilayer dielectric interference filters, especially suitable for optical components with high requirements for film refractive index, absorption loss and surface flatness, such as large-angle filters and wide-cutoff-band interference filters. Using this hydrogenated amorphous silicon film as a high-refractive-index film layer in a multilayer film system can improve the angle effect of the filter, broaden the cutoff band range, reduce the overall light absorption loss of the device and improve the spectral performance of the filter.

[0063] To further illustrate the method for preparing hydrogenated amorphous silicon films by ion beam sputtering in this application, multiple specific embodiments are set up for demonstration, taking into account the defined process parameter range, vacuum pretreatment process and the synergistic effect mechanism of multiple ion sources.

[0064] All embodiments uniformly employ a pre-treatment step, in which the JGS1 quartz substrate to be coated and the high-purity single-crystal silicon target (purity ≥99.999%) are clamped and fixed in a vacuum chamber, the vacuum chamber is closed, and the vacuum system is evacuated to achieve a background vacuum level of 1×10⁻⁶ before deposition. -4 Pa ~ 1×10 -2 Pa, target distance 120mm.

[0065] Example 1: Using three ion sources, all activated simultaneously. In this embodiment, the main sputtering ion source 3 is supplied with an argon-hydrogen mixture at a flow rate of 22 sccm and an ion acceleration voltage of 750V; the auxiliary ion source 5 is supplied with an argon-hydrogen mixture at a flow rate of 14 sccm and an ion acceleration voltage of 180V; the hydrogen cracking auxiliary ion source 6 is supplied with high-purity hydrogen at a flow rate of 10 sccm and an operating power of 350W; and the deposition time is 110 min.

[0066] Example 2: Only the main sputtering ion source is turned on Only the main sputtering ion source is turned on, while the auxiliary ion source and the hydrogen pyrolysis auxiliary ion source are turned off; the argon-hydrogen mixed gas flow rate of the main sputtering ion source is 22 sccm, the ion acceleration voltage is 750V, and the deposition time is 110 min.

[0067] Example 3: Turn on the main sputtering ion source and the hydrogen pyrolysis auxiliary ion source, and turn off the auxiliary ion source. In this embodiment, the main sputtering ion source has an argon-hydrogen mixed gas flow rate of 22 sccm and an accelerating voltage of 750V; the hydrogen cracking auxiliary ion source has a hydrogen gas flow rate of 10 sccm and a power of 350W; and the deposition time is 110 min.

[0068] Example 4: Turn on the main sputtering ion source and replace the hydrogen pyrolysis auxiliary ion source with a microwave hydrogen pyrolysis source. Turn on the main sputtering ion source and microwave hydrogen pyrolysis source, and turn off the auxiliary ion source; the main sputtering ion source has an argon-hydrogen mixed gas flow rate of 22 sccm and an accelerating voltage of 750V; the microwave hydrogen pyrolysis source has a hydrogen flow rate of 10 sccm and a microwave power of 350W; the deposition time is 110 min.

[0069] Example 5: Turn on the main sputtering ion source and the auxiliary ion source, and turn off the hydrogen pyrolysis auxiliary ion source. In this embodiment, the main sputtering ion source has an argon-hydrogen mixed gas flow rate of 22 sccm and an accelerating voltage of 750 V; the auxiliary ion source has an argon-hydrogen mixed gas flow rate of 14 sccm and an accelerating voltage of 180 V; and the deposition time is 110 min.

[0070] Example 6: Using a blank substrate reference sample JGS1 quartz glass substrates are used directly without ion beam coating.

[0071] The test structure can be found here. Figure 7 The schematic transmission spectrum shows that the optically transparent region of the thin film sample (green curve) prepared by the three-beam ion synergy in Example 1 is significantly broadened. At the same time, the interference peak heights corresponding to each half wavelength are closer to the reference level of JGS1-white film (light blue curve), indicating that the light absorption of the thin film is effectively suppressed and the extinction coefficient is low.

[0072] For Examples 2 to 5, thin film samples were prepared using either single-source or dual-source methods. Figure 7 It can be seen that not only is the transparent region relatively narrow, but the interference peaks of each order also deviate significantly downward from the white film reference curve. In particular, the thin film sample prepared using only the main sputtering ion source in Example 2 (orange curve) has the largest peak drop, and the corresponding film absorption is the most severe. While Examples 3 and 4 also use auxiliary ion sources, although partial hydrogenation can be achieved, the interference peaks are significantly different from the white film, and the light absorption effect is worse than that of the thin film sample prepared using the synergistic effect of three ions in Example 1. Example 5 lacks a hydrogen pyrolysis source and in-situ hydrogenation, resulting in high defect density, significant shrinkage of the transparent region, a large deviation of the peaks from the white film, and increased light absorption.

[0073] This confirms that only when the main sputtering ion source 3, the auxiliary ion source 5, and the hydrogen pyrolysis auxiliary ion source 6 work together, both by passivating thin film defects with active hydrogen to broaden the transparent region and by enhancing the density of the thin film through low-energy ion bombardment, can the interference peak be made as close as possible to the white film reference, thus obtaining a hydrogenated amorphous silicon thin film with low absorption and high refractive index.

[0074] In summary, the method for preparing low-absorption hydrogenated amorphous silicon films by ion beam sputtering in this application employs the synergistic effect of three ion beams: a main sputtering ion source 3, an auxiliary ion source 5, and a hydrogen pyrolysis auxiliary ion source 6. The main sputtering ion source 3 uses an argon-hydrogen mixture as the working gas to bombard the silicon target 4, providing the sputtering particles required for film formation. The auxiliary ion source 5 outputs a low-energy ion beam to bombard and modify the surface of the growing film, improving its density. The hydrogen pyrolysis auxiliary ion source 6 generates high-density active hydrogen particles by pyrolyzing high-purity hydrogen gas. Simultaneously, the hydrogen in the working gas used by the main sputtering ion source 3 and the auxiliary ion source 5 forms a dual hydrogenation system, thereby achieving thorough and uniform hydrogenation of the film from the surface to the interior. This method can efficiently passivate silicon dangling bond defects to reduce film light absorption and prevent excessive hydrogenation from causing a decrease in refractive index, thus stably preparing hydrogenated amorphous silicon films with both high refractive index and low absorption.

[0075] In this application, a radio frequency bias voltage can be applied to the substrate 2 during the deposition process. The radio frequency bias voltage forms a controllable negative bias electric field on the surface of the substrate 2, thereby regulating the movement of incident silicon sputtered particles and active hydrogen particles.

[0076] Both the main sputtering ion source 3 and the auxiliary ion source 5 in this application use an argon-hydrogen mixture as the working gas. After ionization, argon gas can form high-energy argon ions, which can ensure the sputtering yield of silicon target 4 and the stable discharge of the ion source. After ionization, hydrogen active particles are obtained, which can achieve shallow in-situ pre-hydrogenation during film growth. Together with the hydrogen pyrolysis auxiliary ion source 6, they passivate silicon dangling bonds and suppress silicon oxide impurity defects, which is beneficial for the preparation of low-absorption films.

[0077] The above description is only a partial embodiment of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of this application, and these improvements and modifications should also be considered within the scope of protection of this application.

Claims

1. A method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering, characterized in that, Includes the following steps: Prepare the substrate to be coated and the silicon target; The main sputtering ion source, the auxiliary ion source, and the hydrogen pyrolysis auxiliary ion source are started simultaneously. The main sputtering ion source bombards the silicon target to generate silicon sputtering particles. The auxiliary ion source is used to perform particle bombardment modification on the substrate surface. The hydrogen pyrolysis auxiliary ion source is used to pyrolyze hydrogen-containing gas to generate active hydrogen particles. Through the synergistic effect of three ion beams—the main sputtering ion source, the auxiliary ion source, and the hydrogen pyrolysis auxiliary ion source—active hydrogen particles react with silicon sputtering particles on the substrate surface, completing in-situ hydrogenation and depositing the target high-refractive-index, low-absorption hydrogenated amorphous silicon film on the substrate surface.

2. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, The purity of the silicon target material is greater than 4N.

3. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, The main sputtering ion source uses an argon-hydrogen mixture with a gas flow rate of 10-50 sccm and an ion acceleration voltage of 100-1500 V.

4. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, The auxiliary ion source uses an argon-hydrogen mixture with a gas flow rate of 0-50 sccm and an ion acceleration voltage of 100-1000V.

5. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, The hydrogen cracking auxiliary ion source uses high-purity hydrogen gas with a gas flow rate of 0~50 sccm and a working power of 0~500W.

6. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, It also includes the step of applying a radio frequency bias voltage to the substrate for regulation, with the radio frequency bias voltage power being 0~500W.

7. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, The background vacuum of the system before deposition was 1×10 -4 Pa ~ 1×10 -2 Pa, the deposition temperature of the substrate to be coated is 100~250℃.

8. The method for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering according to claim 1, characterized in that, After the amorphous silicon film is deposited, it is annealed at a temperature of 300~350℃ for 60~120min.

9. A processing system for preparing high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering, characterized in that, This method is applicable to the preparation of high-refractive-index, low-absorption hydrogenated amorphous silicon films by ion beam sputtering as described in any one of claims 1 to 8; The processing system includes a vacuum chamber and a silicon target, a main sputtering ion source, an auxiliary ion source, and a hydrogen pyrolysis auxiliary ion source disposed within the vacuum chamber. A substrate station is provided inside the vacuum chamber for placing the substrate to be coated. The ion beam outlet of the main sputtering ion source faces the silicon target, and the silicon sputtered particles generated by the silicon target are directed towards the substrate station. The ion beam outlet of the auxiliary ion source faces the substrate station, and the particle exit port of the hydrogen pyrolysis auxiliary ion source faces the substrate station. The main sputtering ion source, auxiliary ion source, and hydrogen pyrolysis auxiliary ion source are configured to be activated simultaneously to deposit a hydrogenated amorphous silicon thin film on the substrate surface.

10. A hydrogenated amorphous silicon film, characterized in that, The high-refractive-index, low-absorption hydrogenated amorphous silicon film is prepared by ion beam sputtering as described in any one of claims 1 to 8. The hydrogenated amorphous silicon film has a refractive index ≥ 3.45 and an extinction coefficient k ≤ 1 × 10⁻⁶ in the visible to infrared range. -4 Surface roughness < 0.5 nm.

11. The application of a hydrogenated amorphous silicon film in a multilayer dielectric interference filter, characterized in that, The hydrogenated amorphous silicon film is prepared using the hydrogenated amorphous silicon film as described in claim 9, or the hydrogenated amorphous silicon film is prepared using the method for preparing a high refractive index, low absorption hydrogenated amorphous silicon film by ion beam sputtering as described in any one of claims 1 to 8.