A polysilicon deposition process

By dynamically adjusting the radio frequency power in the PECVD equipment using a variable radio frequency power supply, the problems of film density and damage in the preparation of polycrystalline silicon thin films for TOPCon cells using PECVD equipment were solved, thereby improving the cell conversion efficiency.

CN123153033APending Publication Date: 2026-11-24SUNSNYC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611591509.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing PECVD equipment suffers from problems such as insufficient film density, inaccurate thickness control, and high-frequency plasma damage to the silicon substrate when preparing polycrystalline silicon thin films for TOPCon batteries, resulting in low battery conversion efficiency.

Method used

By employing a variable radio frequency power supply and combining low-frequency and high-frequency radio frequency power, the plasma state is controlled in segments. The radio frequency power is dynamically adjusted during the growth stages of the tunneling silicon oxide layer and the amorphous silicon thin film to form a dense polycrystalline silicon thin film.

Benefits of technology

It improves the density of polycrystalline silicon thin films, reduces damage to the silicon substrate, enhances the conversion efficiency of solar cells, and narrows the efficiency gap with LPCVD processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153033A_ABST
    Figure CN123153033A_ABST
Patent Text Reader

Abstract

This invention discloses a polycrystalline silicon deposition process, including the preparation of a tunneling silicon oxide layer, initial deposition of doped amorphous silicon, and final deposition of doped amorphous silicon: Low-frequency radio frequency (RF) power is output to excite the process gas to form plasma, forming a tunneling silicon oxide film at a low deposition rate; high-frequency RF power excites the process gas to form high-energy plasma, forming an initially dense amorphous silicon film at a high deposition rate; low-frequency RF power is used to form the remaining amorphous silicon film at a low deposition rate, with plasma active particles filling the micropores and voids within the amorphous silicon film. In this invention, low-frequency RF output is used in the tunneling oxide layer deposition stage, significantly reducing the damage to the silicon substrate caused by plasma bombardment and ensuring the electrical properties of the silicon wafer. This invention, through a high-frequency-low-frequency combined process, balances the deposition rate and film density of the amorphous silicon film, effectively reducing the number of internal pores and defects in the film and improving the passivation effect of the polycrystalline silicon layer obtained by subsequent annealing and crystallization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of TOPCon battery technology, and more particularly to a polycrystalline silicon deposition process. Background Technology

[0002] Tunnel oxide passivated contact (TOPCon) is currently the mainstream technology for crystalline silicon solar cells. The core process involves the fabrication of the back-side tunnel oxide passivation layer: a 1.5-2 nm thick silicon oxide tunneling film is grown on the back surface of the silicon wafer, followed by the deposition of a phosphorus-doped amorphous silicon film. After annealing, the amorphous silicon crystallizes to form a doped polycrystalline silicon layer. Currently, the industry mainstream uses LPCVD and PECVD equipment to complete this film fabrication. LPCVD has a slow deposition rate but excellent film uniformity; PECVD has a fast deposition rate, but the film uniformity and density need further improvement.

[0003] PECVD, or Plasma-Enhanced Chemical Vapor Deposition, is a process where the gas inside the reaction chamber is ionized under an electric field, generating a plasma composed of positive ions, electrons, and neutral particles. The specific working mechanism is as follows: an excitation voltage is applied to two sets of electrodes in the reaction chamber. The cathode emits electrons, which gain kinetic energy under the influence of the electric field and collide with molecules and atoms of the process gas introduced into the chamber. This excitation, decomposition, and ionization of the gas molecules produces a glow discharge effect, generating a large number of electrons, ions, active groups, and metastable particles within the chamber. These active particles migrate to the surface of the silicon substrate through complex physicochemical reactions, where they are deposited to form the target thin film.

[0004] Process conditions that can affect the quality of PECVD film deposition include radio frequency (RF) frequency, chamber temperature, deposition time, chamber pressure, pulse duty cycle, and process gas composition and flow rate. The RF frequency is controlled by the RF power supply, with commonly used industrial RF power supplies operating in the 50kHz-13.56MHz range. Currently, commercially available PECVD equipment is equipped with RF power supplies operating in a fixed power output mode, making it impossible to dynamically switch the output power during a single batch of film deposition.

[0005] The output parameters of the radio frequency (RF) power supply directly determine the plasma state, which in turn affects the overall performance of the thin film: when the RF output frequency is low, the ion density in the cavity is low, the ion bombardment energy is weak, and the thin film deposition rate is low; the deposited particles gain limited energy, and their surface diffusion and migration ability after reaching the silicon substrate is insufficient, resulting in a loose thin film structure and weak adhesion between the thin film and the silicon substrate, posing a risk of film delamination. However, under low-frequency conditions, particle bombardment damage is small, and the silicon substrate is not easily damaged by plasma bombardment.

[0006] At higher radio frequency output frequencies, the plasma ion bombardment effect is enhanced, leading to increased ion concentration, which helps improve film density and deposition rate. However, excessively high bombardment energy can cause significant thermal effects, introducing numerous lattice defects and damage to the silicon substrate; especially when preparing tunneling oxide layers that directly contact the silicon substrate, high-frequency plasmas can easily damage the silicon matrix. Simultaneously, the particle migration rate on the film surface cannot keep up with the epitaxial growth rate, interfering with the normal growth of amorphous silicon films.

[0007] All existing commercial PECVD equipment is equipped with a fixed-power radio frequency power supply. This configuration can meet production requirements when preparing silicon nitride passivation protective films. The silicon nitride film itself has excellent density, and the protective film can isolate plasma and protect the silicon substrate from bombardment damage.

[0008] However, when using PECVD to fabricate TOPCon solar cells with polysilicon structures, the fixed-power RF power supply reveals significant drawbacks: firstly, the amorphous silicon film itself lacks sufficient density; secondly, the tunneling oxide layer is extremely thin, making precise control of the film thickness difficult in the fixed-power mode. Compared to solar cells fabricated with polysilicon using LPCVD, the PECVD method results in a conversion efficiency approximately 0.05% lower. This is because the amorphous silicon film has poor density, leading to a high defect density within the doped polysilicon layer after annealing and crystallization, resulting in reduced passivation contact effectiveness and ultimately, a loss in cell efficiency.

[0009] Therefore, it is necessary to develop a polycrystalline silicon deposition process to solve the above problems. Summary of the Invention

[0010] The purpose of this invention is to design a polycrystalline silicon deposition process to solve the above-mentioned problems.

[0011] The present invention achieves the above objectives through the following technical solutions: A polycrystalline silicon deposition process, comprising: S1. Preparation of tunneling silicon oxide layer: The silicon wafer is fed into the PECVD reaction chamber. The variable RF power supply is connected to the PECVD chamber electrode. The variable RF power supply is controlled to output low-frequency RF power to excite the process gas to form plasma. The active oxygen component in the plasma reacts with the silicon substrate surface to form a tunneling silicon oxide film at a low deposition rate. S2. Initial deposition of doped amorphous silicon: After the tunneling silicon oxide layer is prepared, the variable RF power supply is switched to output high-frequency RF power. The high-frequency RF power excites the process gas to form high-energy plasma, which accelerates the decomposition of silane and phosphine, increases the concentration of plasma particles in the cavity, and forms an initial dense amorphous silicon film at a high deposition rate. S3, Final deposition of doped amorphous silicon: When the amorphous silicon film grows to the preset thickness, the variable RF power supply is controlled to switch back to output low-frequency RF power; the remaining amorphous silicon film is formed at a low deposition rate, and plasma active particles fill the micropores and voids inside the amorphous silicon film.

[0012] Preferably, in step S1, the low-frequency radio frequency power is 70-80W; in step S2, the high-frequency radio frequency power is 140-150W; and in step S3, the low-frequency radio frequency power is 70-80W.

[0013] Preferably, in step S1, the tunneling silicon oxide film formed is 1.5-2 nm thick.

[0014] Preferably, in step S3, the preset thickness is 80% of the total designed thickness of the amorphous silicon thin film.

[0015] Specifically, in step S1, the process gases are oxygen and argon; the low deposition rate is 0.1-0.3 nm / min.

[0016] Specifically, in step S2, the process gases are silane, phosphine, and argon; the high deposition rate is 2.0-4.0 nm / min.

[0017] Specifically, in step S3, the low deposition rate is 0.4-0.8 nm / min.

[0018] The beneficial effects of this invention are as follows: In this invention, low-frequency radio frequency output is used in the tunnel oxide layer deposition stage, which greatly reduces the damage to the silicon wafer substrate caused by plasma bombardment and ensures the electrical performance of the silicon wafer.

[0019] This invention utilizes a high-frequency-low-frequency combined process to balance the deposition rate and density of amorphous silicon thin films, effectively reducing the number of internal pores and defects in the thin film and improving the passivation effect of the polycrystalline silicon layer obtained by subsequent annealing and crystallization. Attached Figure Description

[0020] Figure 1 This is a flowchart illustrating the process of this application. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.

[0022] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.

[0023] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0024] In the description of this invention, it should be understood that the terms "upper," "lower," "inner," "outer," "left," "right," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of this invention is in use, or the orientation or positional relationship commonly understood by those skilled in the art. They are only used to facilitate the description of this invention and to simplify the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0025] Furthermore, the terms "first," "second," etc., are used only to distinguish descriptions and should not be interpreted as indicating or implying relative importance.

[0026] In the description of this invention, it should also be noted that, unless otherwise explicitly specified and limited, terms such as "set" and "connection" should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0027] The specific embodiments of the present invention will now be described in detail with reference to the accompanying drawings.

[0028] like Figure 1 As shown, a polycrystalline silicon deposition process includes: S1. Preparation of tunneling silicon oxide layer: The silicon wafer is fed into the PECVD reaction chamber. The variable RF power supply is connected to the PECVD chamber electrode. The variable RF power supply is controlled to output low-frequency RF power of 70-80W. The process gas composed of oxygen and argon is introduced and excited to form plasma. The active oxygen component in the plasma reacts with the silicon substrate surface to form a 1.5-2nm tunneling silicon oxide film at a low deposition rate of 0.1-0.3nm / min. S2. Initial deposition of doped amorphous silicon: After the tunneling silicon oxide layer is prepared, the variable RF power supply is controlled to switch the output of high-frequency RF power, which is 140-150W. The high-frequency RF power excites the process gas composed of silane, phosphine and argon to form a high-energy plasma, which accelerates the decomposition of silane and phosphine, increases the plasma particle concentration in the cavity, improves the film deposition rate and improves the uniformity of film coverage on the silicon wafer surface, and forms an initially dense amorphous silicon film at a high deposition rate of 2.0-4.0nm / min. S3. Final deposition of doped amorphous silicon: When the amorphous silicon film grows to the preset thickness (the preset thickness is 80% of the total designed thickness of the amorphous silicon film), the variable RF power supply is controlled to switch back to output low-frequency RF power, which is 70-80W; the remaining amorphous silicon film is formed at a low deposition rate of 0.4-0.8nm / min. The low-frequency RF reduces plasma energy and deposition rate, weakens the damage of high-energy particles to the formed amorphous silicon film, and the plasma active particles fill the micropores and voids inside the amorphous silicon film.

[0029] The principle applied in this application is that radio frequency (RF) power directly affects the thin film deposition rate and film density. Higher RF power results in a faster deposition rate, and high-power films exhibit better density than those prepared with low power. The purpose of this invention is to overcome the technical limitations of fixed RF power supplies by using a dynamically adjustable RF power supply to segmentally match the power requirements of different stages in the growth of the tunneling oxide layer and amorphous silicon thin films. This improves the density of polysilicon thin films prepared by PECVD, reduces film defects, and narrows the efficiency gap with LPCVD processes. The RF output power of this application can be flexibly adjusted. Facing the iteratively updated TOPCon cell technology, only the power supply output parameters need to be modified for adaptation, without replacing the entire RF hardware, thus reducing equipment upgrade and modification costs.

[0030] Example 1 A polycrystalline silicon deposition process, wherein a variable RF power supply is connected to the PECVD cavity electrode, and the process execution flow is as follows: 1) The silicon wafer is fed into the PECVD reaction chamber for tunneling silicon oxide deposition. The RF power supply is set to low frequency output with a power of 70W to complete the preparation of tunneling silicon oxide with a thickness of approximately 1.8nm; 2) The process automatically jumps to the initial stage of phosphorus-doped amorphous silicon deposition. The RF power supply switches to high frequency output with a power of 140W to perform rapid amorphous silicon deposition; 3) When the amorphous silicon film is deposited to 80% of the preset thickness, the RF power supply switches back to low frequency 70W to complete the deposition of the remaining film. Active particles fill the internal pores and defects of the film.

[0031] After the entire deposition process is completed, the silicon wafer is removed and subsequently subjected to annealing and crystallization treatment. Results: The film density is improved, silicon substrate bombardment damage is significantly reduced, and compared with conventional fixed-power PECVD methods, cell conversion efficiency is improved in cell testing.

[0032] Example 2 The variable RF power supply parameters can be adjusted according to the actual operating conditions of the production line. 80W is selected for low-frequency tunneling oxide deposition, 150W for high-frequency deposition in the initial stage of amorphous silicon, and then reduced back to 80W in the final stage of amorphous silicon deposition. Other process gas, temperature, and chamber pressure conditions remain unchanged from the original production line parameters. Results: Adapts to different equipment chamber conditions, achieving the same effects of substrate damage suppression and improved film density, with flexible process parameter adjustment.

[0033] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A polysilicon deposition process, characterized by, include: S1. Preparation of tunneling silicon oxide layer: The silicon wafer is fed into the PECVD reaction chamber. The variable RF power supply is connected to the PECVD chamber electrode. The variable RF power supply is controlled to output low-frequency RF power to excite the process gas to form plasma. The active oxygen component in the plasma reacts with the silicon substrate surface to form a tunneling silicon oxide film at a low deposition rate. S2. Initial deposition of doped amorphous silicon: After the tunneling silicon oxide layer is prepared, the variable RF power supply is switched to output high-frequency RF power. The high-frequency RF power excites the process gas to form high-energy plasma, which accelerates the decomposition of silane and phosphine, increases the concentration of plasma particles in the cavity, and forms an initial dense amorphous silicon film at a high deposition rate. S3, Final deposition of doped amorphous silicon: When the amorphous silicon film grows to the preset thickness, the variable RF power supply is controlled to switch back to output low-frequency RF power; the remaining amorphous silicon film is formed at a low deposition rate, and plasma active particles fill the micropores and voids inside the amorphous silicon film.

2. The polysilicon deposition process of claim 1, wherein, In step S1, the low-frequency radio frequency power is 70-80W; in step S2, the high-frequency radio frequency power is 140-150W; in step S3, the low-frequency radio frequency power is 70-80W.

3. The process for polysilicon deposition according to claim 1, wherein In step S1, the tunneling silicon oxide film formed is 1.5-2 nm thick.

4. The process for polysilicon deposition according to claim 1, wherein In step S3, the preset thickness is 80% of the total designed thickness of the amorphous silicon thin film.

5. The process for polysilicon deposition according to claim 1, wherein In step S1, the process gases are oxygen and argon; the low deposition rate is 0.1-0.3 nm / min.

6. The polycrystalline silicon deposition process according to claim 1, characterized in that, In step S2, the process gases are silane, phosphine, and argon; the high deposition rate is 2.0-4.0 nm / min.

7. The polycrystalline silicon deposition process according to claim 1, characterized in that, In step S3, the low deposition rate is 0.4-0.8 nm / min.