A process for electroless plating of large-size copper foil with nickel-phosphorus alloy with high uniformity of square resistance
By applying synergistic flow field control of mechanical oscillation and cyclic reflux during the electroless plating process, the problem of uniformity in the plating of large-size copper foil was solved, achieving high uniformity of plating and consistent device performance, while avoiding damage to the copper foil.
Patent Information
- Application Number
- CN202611312515.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
In the process of electroless plating of nickel-phosphorus alloy layers on large-size copper foil, the problem of coating uniformity leads to sheet resistance fluctuations, which affects the consistency of electrochemical performance. Existing improvement methods are prone to damaging the copper foil or changing the mature formula.
By applying mechanical oscillation and cyclic reflux synergistic flow field control during the electroless plating process, process parameters such as oscillation frequency, amplitude, reflux position and flow rate are optimized to ensure coating uniformity.
It achieves a sheet resistance uniformity of over 90% for large-size copper foil plating, improving the performance consistency of electronic devices and batteries, while protecting the copper foil from damage and making the testing method more accurate.
Smart Images

Figure CN123153036A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic materials and surface technology, and more specifically, to a chemical plating process for large-size copper foil nickel-phosphorus alloy with high sheet resistance and uniformity. Background Technology
[0002] In the manufacturing of new energy batteries (such as solid-state batteries and lithium metal batteries) and high-end printed circuit boards (PCBs), it is often necessary to chemically plate a nickel-phosphorus (Ni-P) alloy layer on the surface of copper foil to serve as a barrier layer, improve interfacial wettability, or enhance corrosion resistance.
[0003] However, when this process is scaled up from laboratory samples to industrial-sized copper foil (such as large sheets or rolls-to-roll copper foil with a width ≥ 500 mm), coating uniformity becomes the core bottleneck restricting yield. Because copper foil is extremely thin and flexible, it is highly susceptible to hydrodynamic influences in the plating bath. In traditional processes, the fluid renewal rate differs significantly between the edges and center of large-size copper foil, resulting in excessively fast deposition at the edges and excessively slow deposition at the center. This uneven spatial distribution of thickness and phosphorus content directly manifests as drastic fluctuations in the sheet resistance of the coating. In current industrial production, the sheet resistance uniformity of large-size copper foil coatings is often below 85%, severely affecting the consistency of the electrochemical performance of subsequent devices.
[0004] Existing improvement methods mostly rely on adjusting the plating solution formulation, but this alters the intrinsic properties of the plating layer; or they employ strong stirring alone, which easily leads to wrinkles, damage, or excessive scouring of the soft copper foil at the edges. Currently, there is a lack of a process that can significantly improve sheet resistance uniformity by optimizing the flow field characteristics of large-size copper foil without damaging the copper foil or altering the established formulation. Summary of the Invention
[0005] To address the aforementioned technical problems, the present invention aims to provide a high-uniformity electroless plating process for large-size copper foil nickel-phosphorus alloy sheet resistance. This process is characterized by comprising the following steps:
[0006] S1. Pretreatment: Degreasing and activation treatment of industrial-sized copper foil;
[0007] S2. Chemical Plating: Pre-treated industrial-sized copper foil is placed in a plating bath containing a chemical plating solution for plating. During plating, mechanical vibration is applied to the copper foil, while the chemical plating solution is simultaneously circulated back. The process parameters for the mechanical vibration are controlled as follows: vibration frequency of 0.05 ~ 0.5 Hz, vibration amplitude of 5 ~ 25 mm; the process parameters for the circulation backflow are controlled as follows: the backflow port is positioned vertically at a distance of 20 ~ 33 cm from the edge of the copper foil, and the backflow velocity is controlled as 0.01 ~ 0.05 m / s.
[0008] S3. Post-processing and testing: The copper foil after plating is cleaned and dried, and the sheet resistance of the plating is tested by etching to evaluate the uniformity of the plating.
[0009] The beneficial effects of this invention are:
[0010] 1. Breakthrough in sheet resistance uniformity: For industrial-sized copper foil, the sheet resistance uniformity of the coating is stably achieved at over 90%, which greatly improves the performance consistency of downstream electronic / battery devices.
[0011] 2. Protects the copper foil substrate: The gentle synergistic flow field avoids mechanical damage (such as wrinkles and breaks) to the soft copper foil caused by strong agitation.
[0012] 3. Precise testing: A sheet resistance testing method combining local etching was defined, eliminating interference from the copper substrate and making the uniformity evaluation more scientific and accurate. Attached Figure Description
[0013] Figure 1 This is a flowchart of the chemical plating process of the present invention.
[0014] Figure 2 This is a comparison diagram of sheet resistance distribution at different locations (from edge to center) of industrial-sized copper foil in Example 1 and Comparative Example 1. Detailed Implementation
[0015] The present invention will be further described in detail below with reference to specific embodiments. The substrate used in this embodiment is an industrial-sized electrolytic copper foil of 680*720mm. The chemical plating solution is a conventional acidic chemical nickel plating solution (nickel sulfate 30 g / L, sodium hypophosphite 25 g / L, complexing agent 20 g / L, pH 4.5, temperature 85℃).
[0016] 1. Determination of optimal process parameters (orthogonal experimental procedure): The sheet resistance uniformity of a 680*720 mm copper foil (defined as: Using ROI as the evaluation index, four factors were selected: ROI location (A), ROI velocity (B), oscillation frequency (C), and oscillation amplitude (D). 16 (4)4 Orthogonal experiment. The factor level table is shown in Table 1.
[0017] Table 1. Factor Level Table for Orthogonal Experiment Factor Level A: Reflux position (cm) B: Flow velocity (m / s) C: Frequency (Hz) D: Amplitude (mm) 1 20 0.01 0.05 5 2 24 0.015 0.1 10 3 27 0.02 0.2 15 4 30 0.03 0.35 20
[0018] Table 2. Results of Orthogonal Experiments and Range Analysis Test No. A (location) B (flow rate) C (frequency) D (amplitude) Sheet resistance uniformity (%) 1 1 1 1 1 61.2 2 1 2 2 2 75.8 3 1 3 3 3 89.1 4 1 4 4 4 87.6 5 2 1 2 3 77.3 6 2 2 1 4 81.4 7 2 3 4 1 77.9 8 2 4 3 2 81.8 9 3 1 3 4 84.6 10 3 2 4 3 86.2 11 3 3 1 2 82.7 12 3 4 2 1 76.8 13 4 1 4 2 72.4 14 4 2 3 1 72.1 15 4 3 2 4 90.3 16 4 4 1 3 78.9 K1 313.7 295.5 304.2 288 K2 318.4 315.5 320.2 312.7 K3 330.3 340 327.6 331.5 K4 313.7 325.1 324.1 343.9 k1 78.4 73.9 76.1 72 k2 79.6 78.9 80.1 78.2 k3 82.6 85 81.9 82.9 k4 78.4 81.3 81 86 Range R 4.2 11.1 5.8 14 Affecting sorting 4 2 3 1
[0019] Table 2 analyzes the k-value and range R of "sheet resistance uniformity". The order of influence of each factor on the uniformity of large-size copper foil chemical plating is: D (amplitude) > B (flow rate) > C (frequency) > A (reflow position).
[0020] Optimal parameter combination determination: Since the evaluation index is "sheet resistance uniformity", a higher value indicates a better process. Therefore, the level with the largest k value among each factor is selected: the maximum k value for factor A is k3 (82.6%) - A3, the maximum k value for factor B is k3 (85.0%) - B3, the maximum k value for factor C is k3 (81.9%) - C3, and the maximum k value for factor D is k4 (86.0%) - D4. The derived optimal process parameter combination aimed at achieving the highest spatial distribution uniformity is: A3B3C3D4 (i.e., reflux port distance from the edge 27 cm, reflux velocity 0.02 m / s, oscillation frequency 0.2 Hz, oscillation amplitude 20 mm). Example
[0021] Example 1 (Orthogonal optimal combination A3B3C3D4)
[0022] (1) Pretreatment: The electrolytic copper foil with a size of 680 * 720 mm was degreased with alkaline solution and washed with water; then activated with 5% dilute sulfuric acid for 120 s and washed with water.
[0023] (2) Chemical plating: Place the copper foil in the plating tank and plate for 50 s. During the plating process, apply vertical reciprocating oscillation to the copper foil, control the oscillation frequency to be 0.2 Hz and the amplitude to be 20 mm; at the same time, turn on the circulation pump, with the return port 27 cm away from the edge of the copper foil and the return flow rate 0.02 m / s;
[0024] (3) Post-processing and testing: water washing and hot air drying. A 10 mm × 10 mm sheet resistance test isolation island was etched on the surface of the plated copper foil using CuCl2 etching solution. Then, the sheet resistance values of nine regions, including the left, middle, right and edge of the copper foil, were measured using a four-probe tester, and the average value and uniformity were calculated.
[0025] Example 2
[0026] The difference from Example 1 is that the process parameters are controlled within a higher upper range: the oscillation frequency is controlled at 0.35 Hz, the amplitude at 20 mm; the reflux position is 30 cm from the edge, and the reflux velocity is 0.03 m / s. The remaining conditions and steps are the same as in Example 1.
[0027] Example 3
[0028] The difference from Example 1 is that the process parameters are controlled within a lower limit range: the oscillation frequency is controlled at 0.1 Hz, the amplitude is 15 mm, the reflux position is 24 cm from the edge, and the reflux velocity is 0.015 m / s. The remaining conditions and steps are the same as in Example 1.
[0029] Comparative Example 1 (Traditional static process): No mechanical vibration, no forced circulation backflow.
[0030] Comparative Example 2 (Recirculation Only, No Oscillation): Mechanical oscillation was eliminated, and the recirculation position was maintained at 24 cm with a flow rate of 0.02 m / s.
[0031] Comparative Example 3 (oscillation only, no reflux): Forced reflux was canceled, and the oscillation frequency was maintained at 0.2 Hz with an amplitude of 20 mm.
[0032] Comparative Example 4 (parameters beyond the scope of this invention): oscillation frequency of 1.0 Hz, amplitude of 30 mm; reflux position 10 cm from the edge, reflux velocity of 0.1 m / s.
[0033] Performance Testing and Result Comparison
[0034] The test results are shown in Table 3.
[0035] Table 3. Test results of sheet resistance uniformity and overall performance of copper foil coating Group Average sheet resistance (Ω / □) Maximum sheet resistance (Ω / □) Minimum sheet resistance (Ω / □) Sheet resistance uniformity (%) Example 1 50.2 51.8 48.6 93.8 Example 2 53.4 55.2 50.1 91.5 Example 3 55.1 57.3 52.0 90.8 Comparative Example 1 98.5 115.2 82.4 71.5 Comparative Example 2 85.2 96.5 74.8 77.6 Comparative Example 3 79.8 88.4 71.2 80.5 Comparative Example 4 92.3 108.6 78.5 72.3
[0036] Results Analysis
[0037] As shown in Table 3, Comparative Example 1, due to the lack of effective flow field control, exhibits a significant difference in mass transfer between the edge and center of the large-size copper foil, resulting in an average sheet resistance as high as 98.5 Ω / □ and a uniformity of only 71.5%. Comparative Examples 2 and 3 demonstrate that using only reflow or only oscillation as a single control method cannot achieve a sheet resistance uniformity exceeding 81%. In Comparative Example 4, the excessively high oscillation frequency and flow velocity caused severe turbulent scouring of the plating solution at the edges, leading to a significant decrease in uniformity to 72.3%.
[0038] In contrast, Examples 1-3, through the efficient synergy of oscillation and reflow parameters within a specific range, eliminated the flow dead zone and boundary layer accumulation on the surface of large-size copper foil, stably controlling the average sheet resistance of the coating within the range of 50-55 Ω / □, and achieving a breakthrough improvement in sheet resistance uniformity to over 90% (with the optimal Example 1 reaching 93.8%). This result is highly consistent with the theoretical optimal parameters and the laws governing primary and secondary factors derived from orthogonal experiments, verifying the significant effect of the synergistic flow field process of this invention on improving the uniformity of coatings on industrial-sized copper foil.
Claims
1. A chemical plating process for large-size copper foil nickel-phosphorus alloy sheet resistance uniformity, characterized in that, Includes the following steps: S1. Pretreatment: Degreasing and activation treatment of industrial-sized copper foil; S2. Chemical plating: The pre-treated industrial-sized copper foil is placed in a plating tank containing a chemical plating solution for plating; during the plating process, mechanical vibration is applied to the copper foil, and the chemical plating solution is circulated back at the same time; The process parameters for the mechanical oscillation are controlled as follows: oscillation frequency is 0.5~3.0 Hz, and oscillation amplitude is 5~30 mm; The process parameters for the recirculation are controlled as follows: the recirculation port is set at a distance of 5~20 cm from the edge of the copper foil, and the recirculation flow rate is controlled at 0.2~1.5 m / s; S3. Post-processing and testing: The copper foil after plating is cleaned and dried, and the sheet resistance of the plating is tested by etching to evaluate the uniformity of the plating.
2. The chemical plating process according to claim 1, characterized in that: In step S1, the micro-etching process uses a dilute sulfuric acid solution with a volume fraction of 3-10% and a micro-etching time of 600 s to remove the oxide film on the copper foil surface and form micro-roughness.
3. The chemical plating process according to claim 1, characterized in that: The industrial-size copper foil is defined as: electrolytic copper foil or rolled copper foil with a width ≥ 500 mm.
4. The electroless plating process according to claim 1, characterized in that: In step S3, the specific method for assisting in the sheet resistance test by local etching is as follows: a specific isolation pattern is etched on the surface of the plated copper foil using a chemical etching solution to eliminate the interference of the parallel resistance of the underlying copper foil on the measurement results. Then, the sheet resistance value of different areas is measured using the four-probe method.
5. The chemical plating process according to claim 1, characterized in that: Through the synergistic flow field control of mechanical oscillation and cyclic reflux, the sheet resistance uniformity of the nickel-phosphorus alloy coating on the surface of industrial-sized copper foil can reach over 90%.