Laser cladding wear-resistant enhancement and surface hardening treatment method for grinding plate teeth of a pulp grinder
By acquiring the tooth surface morphology and matrix hardness data of the grinding wheel teeth of the pulping machine, local cladding areas and thermally sensitive boundaries are generated, the tooth surface heat input window and powder gradient scheme are calculated, and laser co-fusion cladding is performed using a partitioned scanning path. This solves the problems of insufficient wear-resistant layer bonding strength, difficulty in controlling tooth shape thermal deformation, uneven cladding layer thickness in the tooth side transition zone, and impact on the toughness of the matrix core in the surface treatment of grinding wheel teeth of the pulping machine. It achieves improved wear-resistant layer bonding strength, controlled tooth shape thermal deformation, and uniform cladding layer thickness.
Patent Information
- Application Number
- CN202611357755.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-24
AI Technical Summary
Existing surface treatment technologies for grinding mill discs are insufficient to simultaneously improve the bonding strength of the wear-resistant layer, control the thermal deformation of the tooth profile, ensure the uniformity of the cladding thickness in the tooth side transition zone, and maintain the toughness of the matrix core.
By acquiring data on the tooth surface morphology, tooth pitch deviation, and matrix hardness of the grinding wheel of the pulper, local cladding areas and thermally sensitive boundaries are generated. The tooth surface heat input window and powder gradient scheme are calculated. Laser co-fusion cladding is performed using a partitioned scanning path. Combined with accompanying cooling and feedback control, a metallurgical bonded cladding layer is formed.
It achieves a balance between improving the bonding strength of the wear-resistant layer, controlling the thermal deformation of the tooth profile, ensuring the uniformity of the cladding layer thickness, and maintaining the toughness of the core matrix. It also reduces the thermal impact depth of the tooth root avoidance zone and the tooth pitch offset, thereby improving the wear resistance and corrosion resistance of the ground teeth.
Smart Images

Figure CN123153045A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface strengthening technology for paper mill grinding discs, specifically relating to a method for laser cladding of grinding teeth in pulp mills to enhance wear resistance and surface hardening. Background Technology
[0002] Refining mill discs are key components in papermaking pulping equipment that directly act on pulp fibers. During operation, the grinding teeth of the refining mill discs are subjected to compressive loads within the disc gaps, scouring loads caused by high-speed pulp flow, abrasive wear from fibers and abrasive particles, and pitting corrosion from the humid and hot environment. The tooth tip bearing zone bears the main shearing and compressive forces, while the tooth flank transition zone guides pulp flow and disperses fibers. The tooth root avoidance zone needs to maintain tooth profile stability and matrix toughness. Therefore, the surface strengthening process of the grinding teeth must not only improve the hardness of the tooth surface and its resistance to abrasive wear, but also avoid excessive heat input that could lead to changes in tooth pitch, tooth flank collapse, or a decrease in the toughness of the matrix core.
[0003] Current surface treatment methods for grinding wheels in pulp mills typically include medium-frequency quenching, thermal spraying, arc welding, or conventional laser cladding. Medium-frequency quenching can improve the surface hardness of the grinding wheels, but it has a large heating range, making it difficult to simultaneously control the hardening depth and tooth profile deformation. The post-treatment hardness is usually in the HRC 40 to 52 range, making it prone to tooth surface wear, pitting, and scoring in high-consistency pulps, mortar-containing materials, or acid / alkali corrosive conditions. Thermal spraying can form a wear-resistant surface layer under relatively low substrate heat input conditions, but the sprayed layer and the grinding wheel substrate mainly rely on mechanical interlocking, making it prone to peeling, flaking, or localized delamination under heavy impact and high-frequency reciprocating shearing. Arc welding can form a thicker weld layer, but the concentrated heat input and long duration make the grinding wheels prone to bending, twisting, and tooth pitch misalignment, resulting in high costs for subsequent straightening and machining.
[0004] Conventional laser cladding features a narrow heat-affected zone and high metallurgical bonding strength. However, if conventional laser cladding is processed using only fixed power, scanning speed, and powder feed rate, it is still difficult to adapt to the complex tooth profiles of grinding discs in a pulping machine. When the width of the bearing zone at the tooth tip is narrow, heat input per unit area tends to concentrate; when there is an inclination in the transition zone on the tooth side, molten metal tends to flow along the tooth side; and when the cooling airflow is too strong, microcracks may occur inside the metallurgical bond cladding layer due to uneven release of thermal stress. Different grinding teeth exhibit variations in tooth surface wear, corrosion marks, matrix hardness, and tooth pitch deviation. A single process window cannot stably balance the continuity, thickness uniformity, metallurgical bonding strength, heat-affected zone depth, and tooth pitch accuracy of the metallurgical bond cladding layer. Summary of the Invention
[0005] The purpose of this invention is to provide a method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding mill grinding discs, which solves the technical problems of insufficient wear-resistant layer bonding strength, difficulty in controlling tooth profile thermal deformation, uneven thickness of cladding layer in tooth side transition zone, microcracks induced by rapid cooling, and easy impact on the toughness of the matrix core in conventional surface strengthening treatment of grinding mill grinding discs.
[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for laser cladding of wear-resistant and surface-hardening treatments on grinding discs of a pulper includes the following steps:
[0008] Step S1: Obtain data on tooth surface morphology, tooth pitch deviation, matrix hardness, and corrosion traces of the grinding wheel teeth of the refining machine, and generate local cladding areas and thermally sensitive boundaries;
[0009] Step S2: Calculate the tooth surface heat input window and powder gradient scheme based on the local cladding area and the thermal boundary, and use the tooth surface heat input window as a linkage constraint of laser power, scanning speed and powder feeding amount;
[0010] Step S3: Following the partitioned scanning path that expands from the tooth tip bearing zone to the tooth side transition zone, laser co-melt is performed on the high-hardness alloy powder and the surface of the ground tooth to form a metallurgical bonding cladding layer.
[0011] Step S4: Collect the molten pool temperature, molten channel height and tooth pitch offset status, and use the molten pool status to reverse correct the partitioned scanning path, tooth surface heat input window and powder gradient scheme until the metallurgical bonding cladding layer is continuous and the thermally sensitive boundary does not cross the boundary.
[0012] Step S5: Perform surface finishing, hardened layer inspection, and tooth profile verification on the cladding-coated grinding teeth to obtain wear-resistant reinforced grinding discs.
[0013] Furthermore, in step S1, the grinding wheels of the polishing machine undergo degreasing, derusting, oxide layer removal, and tooth surface roughening treatment. The tooth surface roughness after roughening is used as a criterion for judging powder adhesion stability and is input into the local cladding area generation process. The tooth surface morphology is used to determine the location of the tooth tip bearing zone, tooth side transition zone, and tooth root avoidance zone; the tooth pitch deviation is used to determine the allowable deformation of the cladding process; the matrix hardness is used to determine the core bearing capacity of the matrix; and the corrosion trace data is used to determine the local reinforcement range.
[0014] Furthermore, the thermally sensitive boundary is a composite process boundary that incorporates geometric positional constraints and thermal deformation constraints, generated jointly by the tooth tip width, the angle between the surface normal of the tooth flank transition zone and the direction of gravity, the location of the tooth root avoidance zone, the tooth pitch deviation, and the matrix hardness. It is used to limit the range of thermal influence that can be transmitted to the core of the matrix during laser co-melting. The smaller the tooth tip width, the smaller the heat dissipation area of the tooth tip bearing zone, and the closer the thermally sensitive boundary is to the tooth surface; the larger the tooth pitch deviation, the smaller the allowable additional thermal deformation, and the narrower the heat input window on the tooth surface; the higher the matrix hardness, the more sensitive the matrix is to the microstructural changes caused by thermal cycling, and the lower the upper limit of the heat input window on the tooth surface.
[0015] Furthermore, the tooth surface heat input window includes the tooth surface heat input index and a set of parameters constrained by this index, including laser power, scanning speed, and powder feed rate. The tooth surface heat input index characterizes the laser energy borne per unit tooth surface area and the degree of tooth profile thermal sensitivity. The tooth surface heat input index is obtained by dividing the laser power by the product of the scanning speed and the spot width, and then multiplying by the tooth profile thermal sensitivity coefficient. When the tooth surface heat input index is too low, the high-hardness alloy powder and the ground tooth surface cannot be fully fused, and the metallurgical bonding cladding layer is prone to incomplete fusion or porosity; when the tooth surface heat input index is too high, the thermal influence depth of the tooth root avoidance zone increases, and the tooth pitch offset increases. For grinding teeth of small and medium-sized paper mill grinding discs, the tooth surface heat input index can be controlled between 35 J / mm² and 120 J / mm². For example, when the laser power is 960 W, the scanning speed is 6 mm / s, the spot width is 3 mm, and the tooth profile thermal sensitivity coefficient is 1.2, the tooth surface heat input index is 64 J / mm², which is within the aforementioned control range.
[0016] Furthermore, the powder gradient scheme includes the powder ratio for the tooth tip bearing zone and the powder ratio for the tooth flank transition zone. The powder ratio for the tooth tip bearing zone is used to improve the hardness and abrasive wear resistance of the bearing surface, while the powder ratio for the tooth flank transition zone is used to improve the toughness and interfacial transition stability of the metallurgical bonding cladding layer. The high-hardness alloy powder is selected from nickel-based alloy powder, cobalt-based alloy powder, nickel-based alloy powder with added tungsten carbide hard particles, or cobalt-based alloy powder with added chromium carbide hard particles.
[0017] Furthermore, the zonal scanning path includes a tooth tip bearing zone scanning section, a tooth flank transition zone scanning section, and an end buffer scanning section. The tooth tip bearing zone scanning section is used to form the main wear-resistant bearing surface, the tooth flank transition zone scanning section is used to form a continuously transitioning wear-resistant side surface, and the end buffer scanning section is used to reduce the risk of buildup and cracking caused by the unsteady molten pool at the end of the ground tooth. The zonal scanning path extends from the tooth tip bearing zone to the tooth flank transition zone, allowing the tooth tip bearing zone to first obtain a stable metallurgical bonding cladding layer, and then the tooth flank transition zone to take over the transition of the molten pool edge.
[0018] Furthermore, in step S4, the feedback correction amount is formed based on the weighted sum of the normalized molten pool temperature deviation, molten channel height deviation, and tooth pitch offset. The molten pool temperature deviation originates from the difference between the molten pool temperature and the target temperature range; the molten channel height deviation originates from the difference between the molten channel height and the target metallurgical bonding cladding layer thickness; and the tooth pitch offset originates from the difference between the tooth pitch reference before cladding and the tooth pitch measurement value during cladding. When the feedback correction amount increases, the feedback control process simultaneously reduces the laser power, increases the scanning speed, or reduces the powder feed; when the feedback correction amount decreases, the feedback control process allows a return to a higher energy input state within the tooth surface heat input window. In claim 1, "until the metallurgical bonding cladding layer is continuous and the thermosensitive boundary has not been crossed" is the core termination criterion, while the molten channel height deviation being within the set height range, the final tooth pitch offset being within the set tooth profile verification range, and the thermally affected depth of the tooth root avoidance zone not exceeding the thermosensitive boundary limit are auxiliary termination criteria.
[0019] Furthermore, in step S3, when laser co-melting the high-hardness alloy powder and the surface layer of the ground tooth according to the partitioned scanning path expanding from the tooth tip bearing zone to the tooth side transition zone, an accompanying cooling gas flow is applied to the tail of the molten pool. The cooling flow rate of the accompanying cooling gas flow is dynamically generated based on the weighted sum of the tooth profile thermal sensitivity coefficient and the molten pool temperature deviation, and a basic cooling flow rate is set as a lower limit. The cooling flow rate satisfies the following:
[0020]
[0021] in, The cooling flow rate accompanying the cooling airflow, Based on the basic cooling flow rate, The first flow gain coefficient, This is the second flow gain coefficient. The thermal sensitivity coefficient of the tooth profile. This is the deviation of the molten pool temperature; when hour, ;when hour, ; , , , The units are all L / min. Dimensionless The temperature deviation is expressed in units. For example, if the base cooling flow rate is 15 L / min, the tooth profile thermistor is 1.1, and the molten pool temperature is 215°C higher than the target temperature range, then if 50°C is used as a temperature deviation unit, the molten pool temperature deviation is 4.3. The first flow gain coefficient is taken as 12.5 L / min, and the second flow gain coefficient is taken as 4.2 L / min, resulting in a weighted sum of 31.81 L / min. The accompanying cooling flow rate can be taken as 32 L / min. The first and second flow gain coefficients are calibrated based on historical machining records of the same specification of gear, ensuring that the accompanying cooling flow creates different cooling intensities between the tooth tip bearing zone and the tooth flank transition zone.
[0022] Furthermore, when the zonal scanning path is in the tooth flank transition zone scanning section, a transverse high-frequency oscillation is applied to the laser beam. The amplitude of the transverse high-frequency oscillation increases with the angle between the surface normal of the tooth flank transition zone and the direction of gravity. The amplitude of the transverse high-frequency oscillation is obtained by multiplying the preset maximum oscillation amplitude by the sine of the angle between the surface normal of the tooth flank transition zone and the direction of gravity, and then adding the minimum basic oscillation amplitude. The transverse high-frequency oscillation is applied to the laser beam through a two-dimensional galvanometer system, causing the laser beam to form a transverse energy distribution in the tooth flank transition zone scanning section. The transverse energy distribution is used to suppress the flow of molten metal along the tooth flank transition zone and to make the hard particles more uniformly distributed in the metallurgical bonding cladding layer. For example, when the angle between the surface normal of the tooth flank transition zone and the direction of gravity is 65°, the preset maximum oscillation amplitude is 2.0 mm, and the minimum basic oscillation amplitude is 0.5 mm, the oscillation amplitude can be 2.31 mm, and the oscillation frequency of the transverse high-frequency oscillation can be 150 Hz.
[0023] Furthermore, while applying a cooling gas flow to the tail of the molten pool, a follower-driven defocused laser beam is applied behind the cooling gas flow to form an in-situ tempering zone. The follower-driven defocused laser beam moves synchronously with the laser cladding head and continuously covers the in-situ tempering zone behind the tail of the molten pool. Acoustic emission signal characteristic parameters of the in-situ tempering zone are collected by a piezoelectric ceramic sensor. These acoustic emission signal characteristic parameters include the acoustic emission energy accumulation rate and the high-frequency pulse count. The acoustic emission energy accumulation rate is the cumulative characteristic quantity obtained by integrating the acoustic emission envelope amplitude over a fixed statistical period. The incident angle of the cooling gas flow and the tempering power of the follower-driven defocused laser beam are adjusted in real time in coordination with the acoustic emission energy accumulation rate and the angle between the surface normal of the tooth flank transition zone and the direction of gravity. The incident angle of the cooling gas flow satisfies:
[0024]
[0025] in, The incident angle of the accompanying cooling airflow, Let the initial incident angle be , This is the included angle compensation coefficient. The cumulative rate of acoustic emission energy is obtained by integrating the acoustic emission envelope amplitude over a fixed statistical period. To preset the acoustic emission energy threshold, The angle between the normal to the surface of the tooth flank transition zone and the direction of gravity. It is the natural logarithm function. The cosine function is calculated in degrees; the units of the incident angle, initial incident angle, angle compensation coefficient, and angle between the surface normal of the tooth flank transition zone and the direction of gravity are all °; the units of the acoustic emission energy accumulation rate and the preset acoustic emission energy threshold are both mV·s; when the calculated incident angle of the accompanying cooling airflow exceeds the execution range of 40° to 60°, the adjacent boundary value of the execution range is taken.
[0026] Furthermore, when acquiring acoustic emission signal characteristic parameters of the in-situ tempering zone using a piezoelectric ceramic sensor, a high-frequency pulse count is used to trigger the pulse mode switching of the follow-up defocused laser beam. When the high-frequency pulse count exceeds the pulse threshold calibrated by historical machining records of the same specification grinding gear, the follow-up defocused laser beam switches from continuous output mode to pulse output mode. The pulse frequency of the follow-up defocused laser beam remains synchronized with the oscillation frequency of the transverse high-frequency oscillation, and the pulse duty cycle of the follow-up defocused laser beam decreases as the high-frequency pulse count increases. When the high-frequency pulse count is lower than or equal to the pulse threshold calibrated by historical machining records of the same specification grinding gear, the follow-up defocused laser beam maintains continuous output mode, and the pulse duty cycle of the follow-up defocused laser beam satisfies the following conditions:
[0027]
[0028] in, The pulse duty cycle of the follow-up defocused laser beam. To preset the maximum pulse duty cycle, This is the duty cycle attenuation coefficient. This refers to the high-frequency pulse count within a single statistical period. The unit statistical period pulse threshold is calibrated from the historical processing records of the same specification gear grinding; the pulse duty cycle of the follower defocused laser beam and the preset maximum pulse duty cycle are both in percentage; the duty cycle attenuation coefficient is in percentage / time; the high frequency pulse count and pulse threshold are both dimensionless count values; when the calculated pulse duty cycle of the follower defocused laser beam is higher than 80%, it is taken as 80%; when it is lower than 20%, it is taken as 20%.
[0029] Furthermore, this invention also provides a laser cladding wear-resistant enhancement and surface hardening treatment system for grinding mill tooth grinding discs. This system includes a tooth surface detection module, a process planning module, a powder supply module, a laser cladding module, a molten pool monitoring module, a feedback control module, an accompanying cooling module, a lateral oscillation module, an acoustic emission monitoring module, a follow-up tempering module, and a post-processing detection module. The tooth surface detection module outputs tooth surface state data; the process planning module outputs local cladding areas, thermally sensitive boundaries, tooth surface heat input windows, powder gradient schemes, and partitioned scanning paths; the powder supply module outputs high-hardness alloy powder; the laser cladding module forms a metallurgically bonded cladding layer; the molten pool monitoring module outputs the molten pool state; the feedback control module corrects process parameters; the accompanying cooling module outputs accompanying cooling airflow; the lateral oscillation module outputs the laser beam oscillation trajectory; the acoustic emission monitoring module outputs the acoustic emission energy accumulation rate and high-frequency pulse count; the follow-up tempering module outputs a follow-up defocused laser beam in continuous or pulsed mode; and the post-processing detection module outputs surface finishing results, hardened layer detection results, and tooth profile verification results.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] This invention acquires data on the tooth surface morphology, pitch deviation, matrix hardness, and corrosion traces of teeth ground by a grinding mill, generating localized cladding regions and thermosensitive boundaries. This allows laser cladding to target specific damage locations on the ground teeth, avoiding the deformation risks associated with treating the entire tooth and improving the targeted nature of surface strengthening. By calculating the tooth surface heat input window and powder gradient scheme based on the localized cladding regions and thermosensitive boundaries, and using the tooth surface heat input window as a constraint linking laser power, scanning speed, and powder feed rate, precise control of heat input per unit tooth surface area is achieved. This ensures sufficient co-fusion of high-hardness alloy powder with the tooth surface to form a metallurgically bonded cladding layer, while reducing the thermal influence depth and pitch offset in the tooth root avoidance zone, thus enhancing the bonding strength between the metallurgically bonded cladding layer and the tooth matrix. Laser co-fusion is performed according to a partitioned scanning path extending from the tooth tip bearing zone to the tooth side transition zone, allowing the tooth tip bearing zone to first form a continuous wear-resistant bearing surface, and then the tooth side transition zone to form a continuously transitioning wear-resistant side surface, improving the uniformity and continuity of the tooth surface cladding layer thickness. By collecting data on the molten pool temperature, molten channel height, and tooth pitch offset, a closed-loop feedback correction is formed, enabling the laser cladding process to adjust the partitioned scanning path, tooth surface heat input window, and powder gradient scheme according to the real-time status. This enhances the adaptability of process parameters to different grinding conditions and reduces the thickness difference of the tooth flank transition zone and the final tooth pitch offset.
[0032] This invention enhances heat dissipation in the rapid solidification zone by applying a cooling gas flow to the tail of the molten pool and incorporating transverse high-frequency oscillation in the scanning section of the tooth-side transition zone. This suppresses unilateral accumulation of molten metal along the tooth-side transition zone, reducing residual tensile stress and the risk of microcrack initiation within the cladding layer. Through coordinated control of acoustic emission monitoring and in-situ tempering with a follow-up defocused laser beam, active intervention in thermal stress release is achieved, improving the solidification microstructure, further reducing microcrack density, and enhancing the shear strength of the bonding interface. Attached Figure Description
[0033] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained from these drawings without creative effort.
[0034] Figure 1 This is a flowchart of the processing method of the present invention.
[0035] Figure 2 This is a flowchart of the sub-process of generating cooling flow rate and coordinating the incident angle with the cooling airflow in this invention.
[0036] Figure 3 This is a schematic diagram of the state after cladding according to the present invention. Detailed Implementation
[0037] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of the embodiments of the invention. Therefore, the drawings and description are considered to be exemplary in nature and not restrictive.
[0038] The following is in conjunction with the appendix Figures 1-2 The embodiments of the present invention will be described in detail below.
[0039] The present invention provides a method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding mill tooth plates. This method uses the tooth surface condition of the grinding mill tooth plate as input, local cladding areas and thermally sensitive boundaries as the basis for process planning, and the tooth surface heat input window, powder gradient scheme, and zoned scanning path as the laser eutectic control objects. The molten pool temperature, molten channel height, and tooth pitch offset are used as feedback inputs to form a metallurgically bonded cladding layer between high-hardness alloy powder and the surface of the ground tooth. This metallurgically bonded cladding layer improves the hardness, pitting resistance, tensile strength, and abrasive wear resistance of the ground tooth surface, while maintaining the original toughness of the tooth matrix core.
[0040] Specifically, the steps include the following:
[0041] In step S1, the grinding teeth of the grinding mill disc to be treated undergo degreasing, rust removal, oxide layer removal, and tooth surface roughening treatment. Degreasing can be performed using an alkaline cleaning agent, rust removal can be performed using mechanical brushing or sandblasting, oxide layer removal can be performed using fine-grained abrasive belts, and the tooth surface roughness after roughening treatment can be controlled to Ra2.5μm to Ra5.0μm. Tooth surface roughness is used to improve the spreading stability of high-hardness alloy powder before laser co-melting and reduce abrupt changes in melt channel height caused by local powder accumulation.
[0042] The tooth surface inspection module acquires a tooth surface morphology coordinate matrix along the radial direction of the grinding disc. This matrix is used to identify the tooth tip bearing zone, tooth flank transition zone, tooth root avoidance zone, and end region. Tooth pitch deviation is obtained by comparing the tooth pitch reference value before cladding with the current measured value. Matrix hardness is obtained by hardness testing on the non-working surface or outer area of the tooth root. Corrosion trace data is obtained through tooth surface image grayscale, pitting number, and pitting depth. Tooth surface morphology, tooth pitch deviation, matrix hardness, and corrosion trace data are collectively input into the process planning module.
[0043] The process planning module generates local cladding zones based on tooth surface wear depth, pitting distribution, and scratch distribution. These local cladding zones prioritize covering the wear concentration areas of the tooth tip bearing zone, the erosion concentration areas of the tooth side transition zone, and the local pitting concentration areas. The local cladding zones do not cover the tooth root avoidance areas that do not require reinforcement, thus eliminating the need for overall heat treatment of the entire tooth during grinding in the refiner, thereby reducing the risk of overall deformation.
[0044] In step S2, the process planning module generates a thermally sensitive boundary based on the tooth tip width, the angle between the surface normal of the tooth flank transition zone and the direction of gravity, the location of the tooth root avoidance zone, the tooth pitch deviation, and the matrix hardness. The thermally sensitive boundary is a composite process boundary that includes both geometric position constraints and thermal deformation constraints. It is used to limit the range of thermal influence that can be transmitted to the core of the matrix during laser co-melting and the upper limit of the allowable tooth pitch deviation. The smaller the tooth tip width, the smaller the heat dissipation area of the tooth tip bearing zone, and the closer the thermally sensitive boundary is to the tooth surface; the larger the tooth pitch deviation, the smaller the allowable additional thermal deformation, and the narrower the heat input window on the tooth surface; the higher the matrix hardness, the more sensitive the matrix is to the microstructure changes caused by thermal cycling, and the lower the upper limit of the heat input window on the tooth surface.
[0045] The tooth surface heat input window includes the tooth surface heat input index and a set of parameters constrained by this index, including laser power, scanning speed, and powder feed rate. The tooth surface heat input index characterizes the laser energy borne per unit tooth surface area and the tooth profile thermal sensitivity. The tooth surface heat input index is obtained by dividing the laser power by the product of the scanning speed and the spot width, and then multiplying by the tooth profile thermal sensitivity coefficient. When the tooth surface heat input index is too low, the high-hardness alloy powder and the ground tooth surface cannot fully co-melt, and the metallurgical bonding cladding layer is prone to incomplete fusion or porosity. When the tooth surface heat input index is too high, the thermal influence depth of the tooth root avoidance zone increases, and the tooth pitch offset increases. For grinding teeth of small and medium-sized paper mill grinding discs, the tooth surface heat input index can be controlled between 35 J / mm² and 120 J / mm².
[0046] For example, when the laser power is 960W, the scanning speed is 6mm / s, the spot width is 3mm, and the tooth profile thermal sensitivity coefficient is 1.2, the tooth surface heat input index is 64J / mm², which is within the aforementioned control range.
[0047] The powder gradient scheme is generated according to different tooth surface parts in the local cladding area. The tooth tip bearing zone bears the main extrusion and shear forces. The powder composition for the tooth tip bearing zone can be a mixture of nickel-based alloy powder and tungsten carbide hard particles, with the tungsten carbide hard particle mass ratio ranging from 25% to 40%. The tooth side transition zone is affected by slurry erosion and molten pool flow. The powder composition for the tooth side transition zone can reduce the mass ratio of hard particles and increase the mass ratio of nickel-based alloy powder or cobalt-based alloy powder. The powder particle size can be 45μm to 105μm, and the powder feed rate can be 8g / min to 18g / min.
[0048] In step S3, the laser cladding module performs laser co-fusion according to a partitioned scanning path that extends from the tooth tip bearing zone to the tooth side transition zone. The partitioned scanning path includes a tooth tip bearing zone scanning section, a tooth side transition zone scanning section, and an end buffer scanning section. The tooth tip bearing zone scanning section extends radially along the grinding disc of the grinding mill, allowing a continuous metallurgical bonding cladding layer to form on the tooth tip bearing zone first. The tooth side transition zone scanning section extends along the inclined surface of the tooth side, ensuring a continuous overlap between the molten pool of the tooth side transition zone and the edge of the molten pool of the tooth tip bearing zone. The end buffer scanning section uses a lower scanning speed or a lower powder feed rate to prevent excessive accumulation of the metallurgical bonding cladding layer at the end of the ground tooth.
[0049] A laser beam instantaneously fused high-hardness alloy powder with the extremely thin surface layer of the ground tooth. After melting, the high-hardness alloy powder and the surface metal of the ground tooth form a common molten pool. Upon solidification, this pool forms a metallurgically bonded cladding layer. Due to the short duration of the laser heat source, the heat-affected zone is concentrated near the tooth surface, allowing the core of the ground tooth matrix to maintain its original toughness. The target thickness of the metallurgically bonded cladding layer can range from 0.3 mm to 1.2 mm, with a single-pass overlap rate of 30% to 50%. After cladding, the hardness of the tooth tip bearing zone can reach HRC50 to 70.
[0050] When the scanning path is in the tooth tip bearing zone, the laser cladding module prioritizes ensuring the continuity of the metallurgical bonding cladding layer and the hardness of the tooth tip bearing zone. When the scanning path is in the tooth side transition zone, the laser cladding module reduces the heat input per unit area and improves the lateral spread of the molten pool through transverse high-frequency oscillation. The transverse high-frequency oscillation is applied by a two-dimensional galvanometer system, and the oscillation frequency can be from 80Hz to 200Hz. The larger the angle between the surface normal of the tooth side transition zone and the direction of gravity, the stronger the tendency of the molten metal to flow along the tooth side transition zone, and the larger the oscillation amplitude of the transverse high-frequency oscillation. The oscillation amplitude of the transverse high-frequency oscillation is obtained by multiplying the preset maximum oscillation amplitude by the sine of the angle between the surface normal of the tooth side transition zone and the direction of gravity, and then adding the minimum basic oscillation amplitude. The transverse high-frequency oscillation creates an alternating flow field inside the molten pool, which can improve the uniformity of hard particle distribution and reduce the thickness variation of the metallurgical bonding cladding layer in the tooth side transition zone.
[0051] When the grinding discs of the pulp mill are in high-consistency pulping conditions or when the tooth tip width is narrow, an accompanying cooling airflow is applied to the tail of the molten pool by the accompanying cooling module. This accompanying cooling airflow directly acts on the rapid solidification zone behind the molten pool, increasing the heat dissipation intensity of the rapid solidification zone. The spray position of the accompanying cooling airflow can be 3mm to 5mm behind the tail of the molten pool, and the spray direction can be towards the surface of the metallurgical bonding cladding layer. The supply pressure of the accompanying cooling airflow can be 0.2MPa to 0.6MPa. The cooling flow rate is dynamically generated based on the weighted sum of the tooth profile thermal sensitivity coefficient and the molten pool temperature deviation, with a base cooling flow rate set as a lower limit. The cooling flow rate satisfies the following:
[0052]
[0053] in, The cooling flow rate accompanying the cooling airflow, Based on the basic cooling flow rate, The first flow gain coefficient, This is the second flow gain coefficient. The thermal sensitivity coefficient of the tooth profile. This is the deviation of the molten pool temperature; when hour, ;when hour, ; , , , The units are all L / min. Dimensionless The deviation is expressed in units of temperature deviation. For example, if the tooth-shaped thermistor coefficient is 1.1 and the molten pool temperature is 215°C higher than the target temperature range, and 50°C is taken as a temperature deviation unit, then the molten pool temperature deviation is 4.3; if the first flow gain coefficient is taken as 12.5L / min, the second flow gain coefficient is taken as 4.2L / min, and the basic cooling flow rate is 15L / min, then the sum of the weighted components is 31.81L / min, and the cooling flow rate accompanying the cooling airflow can be taken as 32L / min.
[0054] In step S4, the molten pool monitoring module continuously collects the molten pool temperature, melt channel height, and tooth pitch offset. The molten pool temperature can be collected by the infrared thermometry unit, the melt channel height by the laser profile measurement unit, and the tooth pitch offset by the tooth profile measurement unit. The molten pool temperature is used to determine whether the high-hardness alloy powder and the surface of the ground tooth are fully eutectic, the melt channel height is used to determine whether the thickness of the metallurgical bonding cladding layer is stable, and the tooth pitch offset is used to determine whether the heat input causes geometric errors in the grinding teeth.
[0055] The feedback control module normalizes the deviations in molten pool temperature, molten channel height, and tooth pitch offset to form a feedback correction value. This correction value is used to reverse-correct the zonal scanning path, tooth surface thermal input window, and powder gradient scheme. If the molten pool temperature is higher than the target temperature range and the tooth pitch offset increases, the feedback control module reduces the laser power, increases the scanning speed, and decreases the powder feed rate. If the molten channel height is lower than the target metallurgical bonding cladding thickness and the molten pool temperature is within the target temperature range, the feedback control module allows for an increase in the powder feed rate or a decrease in the scanning speed. If the thermal impact depth of the tooth root avoidance zone approaches the depth defined by the thermosensitive boundary, the feedback control module shortens the current continuous scanning length of the tooth surface and switches to an intermittent skip-tooth thermal equalization sequence.
[0056] The core termination criteria for closed-loop correction are: continuous metallurgical bonding cladding layer and no breach of the thermosensitive boundary. Secondary termination criteria include: the deviation of the melt channel height within the height range determined by process calibration; the thermally affected depth of the tooth root avoidance zone not exceeding the depth limit of the thermosensitive boundary; and the final offset of the tooth pitch within the tooth profile verification range determined by process calibration. After the closed-loop correction meets the termination criteria, the laser cladding module completes the processing of the current local cladding area and writes the final processing parameters into the historical processing record of the same specification grinding teeth for subsequent process calibration of the same specification grinding teeth.
[0057] In step S5, the ground teeth after cladding undergo surface finishing, hardened layer inspection, and tooth profile verification. Surface finishing includes removing local spatter, smoothing the tooth tip bearing zone, and trimming the edges of the tooth flank transition zone. Hardened layer inspection includes testing the hardness of the metallurgical bond cladding layer, the thickness of the metallurgical bond cladding layer, detecting cracks at the metallurgical bond interface, and testing the depth of the heat-affected zone. Tooth profile verification includes verifying the tooth pitch, tooth flank profile, and tooth tip width. If the results of the hardened layer inspection or tooth profile verification do not meet the qualification conditions determined by the process calibration, the post-processing inspection module will send the inspection results back to the process planning module, causing the process planning module to regenerate the tooth surface heat input window and partition scanning path for the next tooth surface.
[0058] To facilitate a better understanding of the present invention by those skilled in the art, the present invention will be further illustrated below with reference to specific implementation examples.
[0059] Example 1: A grinding wheel tooth for a paper mill was selected. The tooth tip width was 3.0 mm, the tooth pitch deviation before cladding was 0.04 mm, the matrix hardness was HRC36, and the tooth surface had pitting and slight scratches. The grinding wheel was subjected to degreasing, derusting, oxide layer removal, and tooth surface roughening treatment. The surface roughness after roughening treatment was Ra3.2 μm. The tooth surface detection module collected the tooth surface morphology coordinate matrix, tooth pitch deviation, matrix hardness, and corrosion trace data. The process planning module generated a local cladding area covering the tooth tip bearing zone and the local tooth side transition zone, and generated a heat-sensitive boundary that avoids the tooth root avoidance zone.
[0060] The process planning module generates a tooth surface heat input window based on the local cladding area and thermistor boundary. The laser power is set to 960W, the scanning speed to 6mm / s, the spot width to 3mm, the tooth profile thermistor coefficient to 1.2, and the tooth surface heat input index to 64J / mm². The powder gradient scheme uses a mixture of nickel-based alloy powder and tungsten carbide hard particles. The tungsten carbide hard particle mass ratio in the tooth tip bearing zone is 30%, and in the tooth side transition zone it is 18%. The powder particle size ranges from 45μm to 105μm, and the powder feed rate is 12g / min.
[0061] The laser cladding module first performs laser co-fusion along the tooth tip bearing zone scanning section, and then performs continuous overlapping along the tooth side transition zone scanning section. The molten pool monitoring module collects the molten pool temperature and molten channel height, while the tooth profile measurement unit collects the tooth pitch offset. During processing, the molten pool temperature is maintained between 1450°C and 1580°C, the molten channel height is controlled between 0.55mm and 0.70mm, and the tooth pitch offset is less than 0.04mm. The feedback control module generates a feedback correction amount based on the weighted sum of the molten pool temperature deviation, molten channel height deviation, and tooth pitch offset. When the molten channel height is higher than the target metallurgical bonding cladding layer thickness, the feedback control module reduces the powder feed rate from 12g / min to 10g / min and increases the scanning speed from 6mm / s to 6.5mm / s.
[0062] See Figure 3 After processing, the clad teeth underwent surface finishing, hardened layer inspection, and tooth profile verification. The test results showed that the average thickness of the metallurgical bonding cladding layer was 0.62 mm, the hardness of the tooth tip bearing zone was HRC61, the heat-affected zone depth of the tooth root avoidance area was 0.48 mm, and the final tooth pitch offset was 0.03 mm. No continuous cracks were found at the metallurgical interface, and the metallurgical bonding cladding layer effectively covered the wear concentration area of the tooth tip bearing zone and the erosion concentration area of the tooth side transition zone.
[0063] Example 2: Based on Example 1, a laser cladding system for wear-resistant enhancement and surface hardening treatment of grinding mill tooth discs is configured. The tooth surface inspection module includes a 3D contour acquisition unit, a tooth pitch measurement unit, a hardness acquisition unit, and a corrosion image acquisition unit. The 3D contour acquisition unit outputs the tooth surface morphology coordinate matrix, the tooth pitch measurement unit outputs the tooth pitch deviation, the hardness acquisition unit outputs the matrix hardness, and the corrosion image acquisition unit outputs corrosion trace data. The process planning module generates local cladding areas, thermally sensitive boundaries, tooth surface thermal input windows, powder gradient schemes, and zoned scanning paths based on the tooth surface morphology coordinate matrix, tooth pitch deviation, matrix hardness, and corrosion trace data.
[0064] The powder supply module includes a dual-hopper powder feeding mechanism, which stores nickel-based alloy powder and nickel-based mixed powder containing tungsten carbide hard particles, respectively. The powder supply module adjusts the powder feeding ratio of the two hoppers according to a powder gradient scheme, ensuring a higher proportion of hard particles in the tooth tip bearing zone and a higher proportion of nickel-based alloy in the tooth side transition zone. The laser cladding module includes a laser cladding head, which receives the partitioned scanning path and the tooth surface heat input window, and performs laser co-melting along the partitioned scanning path.
[0065] The accompanying cooling module includes a coaxial annular cooling nozzle. This nozzle is positioned behind the laser cladding head, with the cooling gas outlet facing the rapid solidification zone at the tail of the molten pool. The cooling medium can be nitrogen or liquid nitrogen vaporized cold gas. Under certain processing conditions, the distance between the cooling gas outlet and the tail of the molten pool is 4 mm, the accompanying cooling gas supply pressure is 0.4 MPa, and the basic cooling flow rate is 15 L / min. When the molten pool temperature deviation increases and the tooth profile thermistoricity is high, the cooling flow rate is increased to 32 L / min. The accompanying cooling gas increases the heat transfer intensity in the rapid solidification zone, allowing heat to be promptly removed from the surface of the metallurgical bonding cladding layer, thus reducing the depth of the heat-affected zone in the tooth root avoidance area.
[0066] The lateral oscillation module includes a two-dimensional galvanometer system. This system receives the angle between the surface normal of the tooth flank transition zone and the direction of gravity, and applies a high-frequency lateral oscillation to the laser beam during the scanning section of the tooth flank transition zone. With a 65° angle between the surface normal and the direction of gravity, a preset maximum oscillation amplitude of 2.0 mm, and a minimum basic oscillation amplitude of 0.5 mm, the oscillation amplitude is calculated by multiplying the preset maximum oscillation amplitude by the sine of the 65° angle and then adding the minimum basic oscillation amplitude. Multiplying 2.0 mm by 0.9063 and adding 0.5 mm yields a lateral high-frequency oscillation amplitude of 2.31 mm. The oscillation frequency is 150 Hz. This lateral high-frequency oscillation distributes laser energy laterally across the tooth flank transition zone, reducing thickness unevenness caused by unidirectional flow of molten metal along the transition zone.
[0067] Example 3: Based on Example 1, the grinding wheel teeth of the pulper were used in a pulping process involving both mortar and weakly corrosive slurry. The tooth surface detection module identified a continuous wear band on the tooth tip bearing zone, slurry erosion grooves on the tooth side transition zone, and no obvious cracks in the tooth root avoidance zone. The process planning module limited the local cladding area to the tooth tip bearing zone and the tooth side transition zone, and the thermally sensitive boundary avoided the tooth root avoidance zone. In the powder gradient scheme, the tooth tip bearing zone used a mixture of nickel-based alloy powder and tungsten carbide hard particles, while the tooth side transition zone used a mixture of nickel-based alloy powder and a lower mass percentage of tungsten carbide hard particles.
[0068] During the processing, the laser cladding module performs the scanning in the following order: tooth tip bearing zone scanning section, tooth side transition zone scanning section, and end buffer scanning section. The molten pool monitoring module detected an increase in the molten pool height deviation in the tooth side transition zone scanning section. The feedback control module reduced the powder feed rate and increased the scanning speed, restoring the metallurgical bonding cladding layer thickness in the tooth side transition zone to the target range. After processing, the tooth tip bearing zone hardness was HRC63, the tooth side transition zone hardness was HRC58, the metallurgical bonding cladding layer thickness range was 0.12 mm, and the final tooth pitch offset was 0.03 mm.
[0069] Example 3 illustrates that in pulping conditions involving both mortar and weakly corrosive slurry, a continuous data flow is formed between the local cladding area, the thermosensitive boundary, the tooth surface heat input window, the powder gradient scheme, and the partitioned scanning path. The local cladding area defines the processing range, the thermosensitive boundary defines the heat-affected zone, the tooth surface heat input window defines the laser power, scanning speed, and powder feed rate, the powder gradient scheme defines the powder ratio for different tooth surface areas, the partitioned scanning path defines the laser co-melting sequence, and the molten pool state feedback is used to correct the aforementioned process parameters. This closed-loop data flow enables the pulper grinding discs to achieve a wear-resistant and reinforced tooth surface while maintaining the toughness of the matrix core.
[0070] Example 4: When grinding wheels in a pulp mill are operating under high-consistency pulping conditions, the tooth surface experiences high levels of mechanical impact and slurry erosion stress. Metallurgical bonding cladding layers relying solely on natural cooling are prone to residual tensile stress during rapid solidification due to microstructural transformation and temperature gradients. High-carbon, high-tungsten content, high-hardness alloy powders, when affected by gravity in the tooth flank transition zone, are prone to uneven thickness of the metallurgical bonding cladding layer and heat overload in the tooth root avoidance zone. Example 4 addresses this by controlling the heat dissipation intensity in the rapid solidification zone through accompanying cooling airflow, and improving the flow state driven by lateral high-frequency oscillation to reduce the accumulation of residual tensile stress and the risk of tooth flank shape collapse.
[0071] The pretreatment stage includes degreasing, rust removal, oxide layer removal, and tooth surface roughening. The tooth surface inspection module collects the tooth surface morphology coordinate matrix radially along the grinding disc of the refiner. The tooth tip width of a high-consistency refiner grinding disc was measured to be 2.5 mm, the angle between the surface normal of the tooth flank transition zone and the direction of gravity was 65°, and the base material was 17-4PH precipitation-hardening stainless steel. The process planning module generates local cladding areas and thermally sensitive boundaries based on the tooth pitch deviation. The process planning module determines that the tooth tip width is within a narrow range, the tooth profile has a high thermal sensitivity coefficient, and traditional natural cooling methods are insufficient to dissipate the heat generated by laser co-melting in a timely manner.
[0072] To reduce heat accumulation in the rapid solidification zone, a coaxial annular cooling nozzle is installed behind the laser cladding head in the processing system. The cooling medium is a vaporized liquid nitrogen gas stream with a purity of 99.99%. This cooling gas stream directly acts on the rapid solidification zone 3mm to 5mm behind the molten pool. The cooling flow rate is dynamically adjusted based on the heat input window on the tooth surface and the state of the molten pool. The supply pressure of the cooling gas stream is 0.4MPa. Calibration tests were conducted with a first flow gain coefficient of 12.5L / min, a second flow gain coefficient of 4.2L / min, and a base cooling flow rate of 15L / min. When the laser beam reaches the tooth tip bearing zone, the temperature deviation of the molten pool increases due to the limited convection area at the tooth tip, and the cooling flow rate of the accompanying cooling gas stream increases from the base value of 15L / min to 32L / min. Forced convection cooling removes heat from the surface of the metallurgical bonding cladding layer, increasing the temperature gradient at the solidification interface front, achieving a cooling rate of 10000°C / s. A higher cooling rate can suppress the growth of primary carbide grains, promote microstructure refinement, thereby reducing residual tensile stress and the risk of microcrack initiation.
[0073] When transitioning to the tooth flank transition zone scanning section, the gravitational component affects the fluid balance of the molten pool. Molten metal on the 65° inclined plane tends to flow along the tooth width, easily leading to the risk of thermal boundary overflow in the tooth root avoidance zone. The laser cladding module activates the two-dimensional galvanometer system, applying transverse high-frequency oscillation to the laser beam. With a preset maximum oscillation amplitude of 2.0 mm and a minimum basic oscillation amplitude of 0.5 mm, and an angle of 65° between the surface normal of the tooth flank transition zone and the direction of gravity, the oscillation amplitude is calculated by multiplying the preset maximum oscillation amplitude by the sine of the 65° angle and then adding the minimum basic oscillation amplitude. Multiplying 2.0 mm by 0.9063 and adding 0.5 mm yields a transverse high-frequency oscillation amplitude of 2.31 mm. The oscillation frequency of the transverse high-frequency oscillation is 150 Hz. The high-frequency oscillating laser beam excites alternating Marangoni convection within the molten pool. The surface tension gradient generated by the alternating flow field creates a transverse spreading effect opposite to the direction of metal droplet descent, reducing the risk of molten metal unilateral accumulation. The high-hardness alloy powder ejected from the powder supply module is fully melted under the irradiation of the oscillating beam, and the hard tungsten carbide particles are distributed in the nickel-based solid solution, reducing the accumulation of bottom particles caused by gravity sedimentation.
[0074] The physical metallurgical process continues. The molten pool monitoring module provides feedback on the molten pool temperature and molten channel height status 1000 times per second. The feedback control module generates a feedback correction value based on the weighted sum of the molten pool temperature deviation, molten channel height deviation, and tooth pitch offset, and finely adjusts the scanning speed and laser power in real time according to the feedback correction value. When the process reaches the end-of-grind buffer scanning section, the cooling airflow is delayed and shut off for 3 seconds to keep the solidified structure of the unsteady molten pool at the end close to that of the middle section. During multi-tooth continuous machining, an intermittent skip-tooth thermal equalization sequence is used to reduce thermal coupling conduction between adjacent grinding teeth.
[0075] After processing, the material is fed into a coordinate measuring machine and an X-ray diffractometer for hardened layer detection and tooth profile verification. The process described in Example 4 is compared with a linear scanning process without accompanying cooling airflow and without lateral high-frequency oscillation, and the results are shown in Table 1.
[0076] Table 1 is a comparison table of the surface strengthening properties of grinding teeth of high-consistency refiners;
[0077]
[0078] The results listed in Table 1 demonstrate that, in Example 4, the combination of accompanying cooling airflow and transverse high-frequency oscillation reduced the depth of the heat-affected zone in the tooth root avoidance area to 0.35 mm, changed the residual stress of the metallurgical bonding cladding layer from tensile stress to compressive stress, reduced the average carbide grain size from 12.5 μm to 3.2 μm, and reduced the thickness variation of the metallurgical bonding cladding layer in the tooth side transition zone from 0.45 mm to 0.08 mm. These results reflect the controlling effect of the accompanying cooling airflow on the heat-affected zone and residual stress state, as well as the improving effect of transverse high-frequency oscillation on the spread and thickness uniformity of the molten pool in the tooth side transition zone. The repaired high-consistency refiner grinding teeth can be used in papermaking pulping processes involving both high-frequency shearing and corrosive wear, and reduce the need for large-scale secondary machining and shaping.
[0079] Example 5: Based on Example 4, further optimization is performed. In this example, the dynamic evolution of thermal stress is further controlled. While the accompanying cooling airflow can refine the average grain size of carbides, forced convection cooling, while increasing the temperature gradient at the solidification interface, can also lead to the initiation of micro-cleavage cracks within the metallurgical bonding cladding layer during the rapid cooling and contraction phase due to the difference in linear expansion coefficients between the tungsten carbide hard particles and the nickel-based solid solution in the high-hardness alloy powder. The microcrack initiation induced by localized strong cooling exhibits acoustic release characteristics. This example introduces a stress active intervention mechanism coupled with acoustic emission monitoring and in-situ tempering using a follow-up defocused laser beam to reduce the risk of uncontrollable thermal stress release in the tooth flank transition zone under high-concentration polishing conditions.
[0080] The processing system integrates a follow-up defocused laser beam emitting component 15mm behind the laser cladding head. This component moves synchronously with the laser cladding head, ensuring the center of the laser beam remains 15mm behind the molten pool. The beam area is set to 4 to 6 times the focal area of the laser cladding head. This follow-up defocused laser beam is not used to melt high-hardness alloy powder; instead, it injects secondary heat into the metallurgical bonding cladding layer, which has just undergone forced cooling with accompanying airflow. This creates an in-situ tempering zone behind the rapid solidification zone, maintaining a temperature between 450°C and 600°C. The accompanying cooling airflow nozzle is a two-axis servo motor-driven omnidirectional nozzle, capable of changing the incident angle of the accompanying cooling airflow irradiating the in-situ tempering zone according to CNC commands. A piezoelectric ceramic sensor is positioned on the non-machined end face of the grinding wheel of the polishing machine. The sensor surface is coated with a high-temperature resistant acoustic coupling agent and subjected to a constant preload. The data acquisition card continuously reads the raw voltage signal output by the piezoelectric ceramic sensor at a sampling rate of 2MHz.
[0081] After the hardware system is deployed, the signal processing and physical field linkage control phase begins. A digital bandpass filter removes mechanical vibration noise below 100kHz and electromagnetic interference noise above 800kHz from the original voltage signal. An envelope detection algorithm converts the filtered high-frequency voltage signal into an acoustic emission energy accumulation rate over a fixed statistical period of 0.2s. The acoustic emission energy accumulation rate is a cumulative characteristic obtained by integrating the acoustic emission envelope amplitude over the fixed statistical period, characterizing the change in elastic strain energy released by lattice dislocation slip and microcrack propagation. A threshold cross-detection algorithm counts high-frequency pulses whose amplitude exceeds a preset baseline; the high-frequency pulse count corresponds to the frequency of brittle phase fracture events. The process planning module inputs the acoustic emission energy accumulation rate into the incident angle correction process. The initial incident angle is set to 45°, the angle compensation coefficient is set to 12.5°, the preset acoustic emission energy threshold is calibrated to 150mV·s, and the incident angle execution range accompanied by cooling airflow is set to 40° to 60°. When the calculated incident angle of the accompanying cooling airflow exceeds the incident angle execution range, the feedback control module drives the universal nozzle according to the adjacent boundary value of the incident angle execution range.
[0082] The angle between the surface normal of the tooth flank transition zone and the direction of gravity was measured to be 65°. During laser eutectic melting in the scanning section of the tooth flank transition zone, the sedimentation of tungsten carbide hard particles led to an increase in local brittleness. The piezoelectric ceramic sensor detected an increase in the acoustic emission energy accumulation rate from 90 mV·s to 320 mV·s. The incident angle correction process calculated a new incident angle of 51.03° for the accompanying cooling gas flow. A servo motor drove the omnidirectional nozzle to deflect the incident angle from 45° to 51.03°. With the increased incident angle, the stagnation point of the accompanying cooling gas flow on the surface of the metallurgical bonding cladding layer shifted backward, reducing the gas flow adhesion effect and causing the peak region of the forced convection heat transfer coefficient to deviate from the sensitive region for microcrack initiation. The shift in the stagnation point weakened the temperature gradient driving force at the crack tip. The tempering power of the follow-up defocused laser beam was simultaneously increased from 200 W to 350 W. After absorbing the energy of the servo-driven defocused laser beam in the in-situ tempering zone, supersaturated dissolved carbon atoms precipitate from the martensitic structure, the residual austenite decomposes, and the lattice distortion energy is released gradually. The thermal stress release process is controlled in a closed loop by acoustic emission monitoring and the in-situ tempering mechanism.
[0083] To verify the role of the piezoelectric ceramic sensor in monitoring the acoustic emission energy accumulation rate and adjusting the injection angle of the accompanying cooling gas flow, two sets of grinding discs of the same specifications were processed using the processes of Example 5 and Example 4. X-ray non-destructive testing equipment and ultrasonic scanning microscopy were used to extract data on the microcrack density and residual stress distribution inside the metallurgical bonding cladding layer, and the performance comparison results listed in Table 2 were obtained.
[0084] Table 2 is a comparison table of the performance of in-situ tempering and dynamic adjustment of incident angle;
[0085]
[0086] The results listed in Table 2 show that by adjusting the injection angle of the accompanying cooling gas flow in real time based on the acoustic emission energy accumulation rate and the angle between the surface normal of the tooth flank transition zone and the direction of gravity, and by introducing a follow-up defocused laser beam, the microcrack density can be reduced from 3.2 cracks / cm² to 0.4 cracks / cm². After adjusting the residual compressive stress from -185MPa to -85MPa, the local stress concentration caused by excessive high pressure stress is reduced, and the interface shear strength is increased to 560MPa. Example 5 can reduce the risk of microcracks caused by deep hardening.
[0087] Example 6: Based on Example 5, further control was implemented for the micro-segregation of the solid-liquid phases at the solidification front of the molten pool under transverse high-frequency oscillation. Transverse high-frequency oscillation improves molten pool spreading in the tooth-side transition zone, but the oscillation causes periodic fluctuations in the laser energy input, resulting in a continuous oscillation in the ratio of the temperature gradient to the solidification rate at the solid-liquid interface. Since the high-hardness alloy powder contains various refractory metal elements, interface oscillation easily induces localized supercooling, forming coarse columnar dendrites accompanied by shrinkage cavities. The high-frequency pulse count captured by the piezoelectric ceramic sensor can reflect the acoustic characteristics of the tearing of low-melting-point eutectic at the columnar dendrite grain boundaries. This example establishes a synchronization mechanism between the temporal output mode of the follow-up defocused laser beam and the frequency domain characteristics of the transverse high-frequency oscillation.
[0088] High-frequency pulse counting is used to trigger the pulse mode switching of the follow-up defocused laser beam. The pulse threshold per unit statistical period calibrated from the historical processing records of the same specification grinding teeth is 50 times within a 1-second statistical period. The laser cladding head performs laser co-melting in the scanning section of the tooth side transition zone, and the lateral oscillation module applies a 150Hz lateral high-frequency oscillation to the laser beam. The piezoelectric ceramic sensor continuously outputs high-frequency pulse counts. When the powder feed rate fluctuates instantaneously in a local area or the molten pool is deflected by the gravitational component, the solid-liquid interface front-side feeding is insufficient, and the high-frequency pulse count increases to 120 times within a 1-second statistical period. After the high-frequency pulse count exceeds the pulse threshold, the feedback control module triggers the follow-up tempering module to switch, and the follow-up defocused laser beam switches from continuous output mode to pulse output mode; when the high-frequency pulse count is lower than or equal to the pulse threshold, the feedback control module keeps the follow-up defocused laser beam in continuous output mode.
[0089] The pulse frequency of the follow-up defocused laser beam is locked at 150Hz by a hardware phase-locked loop, and the pulse frequency is synchronized with the oscillation frequency of the transverse high-frequency oscillation. The preset maximum pulse duty cycle is set to 80%, the duty cycle attenuation coefficient is set to 0.4% / cycle, and the pulse duty cycle execution range of the follow-up defocused laser beam is set to 20% to 80%. Substituting 120 high-frequency pulse counts and 50 pulse thresholds into the pulse duty cycle relationship, the pulse duty cycle of the follow-up defocused laser beam is calculated to decrease from 80% to 52%. The follow-up defocused laser beam acts on the surface of the in-situ tempering zone at a frequency of 150Hz and a duty cycle of 52%. When the calculated pulse duty cycle of the follow-up defocused laser beam is lower than 20%, the feedback control module drives the follow-up tempering module at 20%; when the calculated pulse duty cycle of the follow-up defocused laser beam is higher than 80%, the feedback control module drives the follow-up tempering module at 80%.
[0090] When a high-frequency pulsed beam acts on the surface of the in-situ tempering zone, it generates micro-thermo-elasto-plastic disturbances on the surface of the metallurgical bonding cladding layer. The frequency of these micro-thermo-elasto-plastic disturbances is the same as the frequency of the solidification oscillations induced by the transverse high-frequency oscillations, and the two periodic actions work together at the tail of the molten pool. After the pulse duty cycle decreases, the instantaneous energy density of a single pulse increases, and the pulse energy can act near the solid-liquid interface, thereby interfering with the directional growth of the primary columnar dendrite network. The disturbed dendrite arms enter the interior of the molten pool and act as new nucleation sites, causing the columnar crystals to transform into equiaxed crystals. The equiaxed crystal structure reduces the continuous low-melting-point eutectic film at grain boundaries, reducing the continuity of microcracks along the grain propagation path. As the proportion of equiaxed crystals increases, grain boundary tearing events decrease, and the high-frequency pulse count monitored by the piezoelectric ceramic sensor gradually falls below the pulse threshold. The feedback control module controls the follow-up tempering module to switch the follow-up defocused laser beam back to continuous output mode, restoring the in-situ tempering function.
[0091] Metallographic sections were prepared from samples of the tooth flank transition zone after pulse mode switching. Dendritic morphology was observed using field emission scanning electron microscopy, and fatigue resistance was tested using a reciprocating friction and wear testing machine. The multidimensional physical field coupling verification data listed in Table 3 were obtained.
[0092] Table 3 shows the performance of pulse synchronization control and grain morphology transformation.
[0093]
[0094] The data listed in Table 3 illustrate that synchronizing the pulse frequency of the follow-up defocused laser beam with the transverse high-frequency oscillation frequency, and dynamically reducing the pulse duty cycle based on the high-frequency pulse count, can improve the ability to regulate the solidified structure. Micro-thermo-elastic-plastic perturbations induce a transformation of the solidified structure from columnar crystals to equiaxed crystals, increasing the equiaxed crystal volume percentage from 15% to 72%. The reciprocating fatigue life increases from 45,000 cycles to 112,000 cycles. The frequency coordination mechanism of acoustic emission monitoring, follow-up defocused laser beam, and transverse high-frequency oscillation disclosed in Example 6 improves the fatigue spalling resistance of the grinding disc teeth when dealing with alternating stresses caused by high-load operation of papermaking equipment.
[0095] Comparative Example 1: Comparative Example 1 and Example 1 use the same grinding mill grinding discs, the same high-hardness alloy powder, the same local cladding area, and the same pretreatment method. The difference is that Comparative Example 1 does not collect the molten pool temperature, molten channel height, and tooth pitch offset to form a closed-loop feedback. Instead, it uses a fixed laser power, a fixed scanning speed, and a fixed powder feed rate for continuous linear scanning.
[0096] In Comparative Example 1, the laser power was fixed at 960W, the scanning speed at 6mm / s, and the powder feed rate at 12g / min. When processing reached the transition zone scanning section on the tooth flank, the weld pool height locally increased, and the tooth pitch offset gradually increased. Because the weld pool temperature deviation, weld pool height deviation, and tooth pitch offset were not fed back to the tooth surface heat input window and the partitioned scanning path generation process, the laser cladding module could not promptly reduce the laser power, increase the scanning speed, or decrease the powder feed rate.
[0097] After processing, in Comparative Example 1, the average thickness of the metallurgical bonding cladding layer was 0.78 mm, the hardness of the tooth tip bearing zone was HRC57, the heat-affected zone depth of the tooth root avoidance zone was 0.86 mm, the final tooth pitch offset was 0.08 mm, and local melt channel buildup was observed in the tooth flank transition zone. Compared with Example 1, Comparative Example 1 only removed the closed-loop feedback correction process, while maintaining the same processing conditions except for the closed-loop feedback correction process. The results show that the closed-loop feedback correction process can reduce the depth of the heat-affected zone and the final tooth pitch offset, and improve the thickness stability of the metallurgical bonding cladding layer.
[0098] Comparative Example 2: Comparative Example 2 and Example 4 use the same grinding mill grinding disc, the same high-hardness alloy powder, the same accompanying cooling airflow, the same tooth surface heat input window, and the same partitioned scanning path. The difference is that Comparative Example 2 does not apply transverse high-frequency oscillation to the laser beam in the tooth side transition zone scanning section.
[0099] In Comparative Example 2, the angle between the surface normal of the tooth flank transition zone and the direction of gravity is 65°. The cooling flow rate accompanying the cooling airflow is still dynamically generated according to the weighted relationship between the tooth profile thermistor coefficient and the molten pool temperature deviation. The laser power, scanning speed, and powder feed rate are consistent with Example 4. Since no transverse high-frequency oscillation is applied, the laser energy is mainly distributed along the scanning centerline. After the molten pool is affected by the gravitational component in the tooth flank transition zone, it shows a tendency for insufficient spreading on one side and accumulation on the other side, resulting in a decrease in the uniformity of tungsten carbide hard particle distribution.
[0100] After processing, in Comparative Example 2, the thickness range of the metallurgical bonding cladding layer in the tooth flank transition zone was 0.31 mm, the final tooth pitch offset was 0.05 mm, the Vickers hardness of the metallurgical bonding cladding layer was 820 HV0.5, and the depth of the heat-affected zone in the tooth root avoidance area was 0.39 mm. Compared with Example 4, Comparative Example 2 only removed the transverse high-frequency oscillation, while retaining the accompanying cooling airflow. The results showed that the transverse high-frequency oscillation mainly improved the transverse spreading of the molten pool and the uniformity of hard particle distribution in the tooth flank transition zone, and together with the accompanying cooling airflow, improved the tooth profile stability under high-consistency grinding conditions.
[0101] Comparative Example 3: Comparative Example 3 and Example 5 use the same grinding mill grinding disc, the same high-hardness alloy powder, the same accompanying cooling airflow, and the same transverse high-frequency oscillation. The difference is that Comparative Example 3 does not collect acoustic emission signal characteristic parameters, does not apply a follow-up defocused laser beam to form an in-situ tempering zone, and the incident angle of the accompanying cooling airflow remains unchanged at 45°.
[0102] In Comparative Example 3, after laser co-melting, the accompanying cooling gas flow continuously acts on the rapid solidification zone at the tail of the molten pool. Because the risk of microcrack initiation was not identified through acoustic emission energy accumulation rate, the stagnation point of the accompanying cooling gas flow on the surface of the metallurgical bonding cladding layer could not be moved backward, and the peak region of the forced convection heat transfer coefficient continuously covered the microcrack initiation sensitive area. Because no in-situ tempering zone for the follow-up defocused laser beam was set up, the rapidly solidified metallurgical bonding cladding layer could not obtain secondary heat input, resulting in insufficient release of local lattice distortion energy.
[0103] After processing, the peak acoustic emission energy accumulation rate in Comparative Example 3 was 485 mV·s, the microcrack density in the tooth flank transition zone was 3.2 cracks / cm², the residual stress at the corresponding location in the in-situ tempering zone was -185 MPa, and the shear strength of the bonding interface was 410 MPa. Compared with Example 5, Comparative Example 3 only removed acoustic emission monitoring, dynamic adjustment of the incident angle, and in-situ tempering with a follow-up defocused laser beam. The results show that the synergistic effect of the aforementioned three features can reduce the microcrack density and improve the shear strength of the bonding interface.
[0104] Comparative Example 4: Comparative Example 4 and Example 6 use the same grinding mill grinding disc, the same follow-up defocused laser beam, the same transverse high-frequency oscillation, and the same acoustic emission monitoring method. The difference is that the follow-up defocused laser beam in Comparative Example 4 always adopts a continuous output mode, does not switch the pulse output mode according to the high-frequency pulse count, and does not keep the pulse frequency of the follow-up defocused laser beam synchronized with the oscillation frequency of the transverse high-frequency oscillation.
[0105] In Comparative Example 4, the transverse high-frequency oscillation frequency remained at 150Hz. During the machining of the tooth flank transition zone, the average high-frequency pulse count was 85 times / s, higher than the pulse threshold calibrated from historical machining records of the same specification. Because the follow-up defocused laser beam maintained a continuous output mode, the in-situ tempering zone could only obtain a stable heat input and could not form periodic thermo-elastic-plastic disturbances synchronized with the transverse high-frequency oscillation frequency. Therefore, the primary columnar dendrite network near the solid-liquid interface was difficult to effectively disturb.
[0106] After processing, the dendrite morphology in Comparative Example 4 was mainly coarse columnar crystals, with equiaxed crystals accounting for 15% of the volume, and the cyclic fatigue life was 45,000 cycles. Compared with Example 6, Comparative Example 4 only removed the pulse mode switching and frequency synchronization control triggered by high-frequency pulse counting. The results showed that the pulse synchronization mode could increase the equiaxed crystal volume ratio and improve the fatigue resistance of the metallurgical bonding cladding layer under cyclic loads.
[0107] In practical implementation, the process parameters for the laser cladding wear-resistant enhancement and surface hardening treatment method for grinding mill teeth can be calibrated according to the specifications of the grinding teeth. For example, for grinding mill teeth with a tooth tip width of 2.8 mm, an angle of 55° between the surface normal of the tooth flank transition zone and the direction of gravity, and a target thickness of 0.60 mm for the metallurgical bonding cladding layer, after the tooth surface detection module collects the tooth surface morphology coordinate matrix, the process planning module determines the tooth tip bearing zone and the tooth flank transition zone as local cladding areas, and determines the outer edge of the tooth root avoidance zone as the thermally sensitive boundary. The laser power is set to 900 W, the scanning speed is set to 5 mm / s, the spot width is set to 3 mm, the tooth profile thermal sensitivity coefficient is 1.0, and the tooth surface heat input index is 60 J / mm². The powder supply module mixes nickel-based alloy powder with tungsten carbide hard particles and feeds them into the laser cladding head at a powder feeding rate of 11 g / min. When the molten pool monitoring module detects that the molten channel height is 0.08 mm higher than the target metallurgical bonding cladding thickness, the feedback control module increases the scanning speed to 5.5 mm / s and reduces the powder feed rate to 10 g / min. After processing, the average thickness of the metallurgical bonding cladding is 0.61 mm, the hardness of the tooth tip bearing zone is HRC60, and the final tooth pitch offset is 0.025 mm.
[0108] In other embodiments, the accompanying cooling airflow does not need to be continuously activated throughout the entire path. In the tooth tip bearing zone scanning section, if the molten pool temperature deviates significantly and the tooth profile has a high thermal sensitivity coefficient, the accompanying cooling module increases the cooling flow rate. In the tooth side transition zone scanning section, if the molten pool temperature is within the target temperature range, the accompanying cooling module reduces the cooling flow rate to allow the molten pool sufficient spreading time. In the end buffer scanning section, the accompanying cooling airflow is delayed and shut off to keep the end solidification structure similar to the middle solidification structure. The accompanying cooling airflow is controlled in the rapid solidification zone at the tail of the molten pool, avoiding direct impact on the central area of the powder feed bundle, thus reducing powder scattering and intermittent melt flow.
[0109] In other embodiments, the amplitude of the lateral high-frequency oscillation is determined by the angle between the normal to the tooth flank transition zone surface and the direction of gravity. When the angle between the normal to the tooth flank transition zone surface and the direction of gravity is small, the amplitude of the lateral high-frequency oscillation is small, and the laser beam is mainly used to ensure continuous overlap between the tooth flank transition zone and the tooth tip bearing zone. When the angle between the normal to the tooth flank transition zone surface and the direction of gravity is large, the amplitude of the lateral high-frequency oscillation increases, and the lateral energy distribution range of the laser beam expands, which is used to offset the thickness deviation caused by the molten metal flowing down along the tooth flank transition zone. The amplitude of the lateral high-frequency oscillation is obtained by multiplying the preset maximum oscillation amplitude by the sine of the angle between the normal to the tooth flank transition zone surface and the direction of gravity, and then adding the minimum basic oscillation amplitude. The oscillation amplitude is not less than the minimum basic oscillation amplitude to keep the keyhole of the molten metal pool stable and prevent local incomplete fusion due to excessively small oscillation amplitude.
[0110] In other embodiments, the acoustic emission monitoring module extracts the acoustic emission energy accumulation rate and high-frequency pulse count within a fixed statistical period. The fixed statistical period can be set to 0.1s to 1s. The acoustic emission energy accumulation rate reflects the degree of elastic strain energy release within the metallurgical bonding cladding layer after rapid solidification, while the high-frequency pulse count reflects the frequency of brittle phase fracture and grain boundary tearing events near the solid-liquid interface. When the acoustic emission energy accumulation rate increases, the feedback control module increases the tempering power of the follow-up defocused laser beam and drives the omnidirectional nozzle to increase the incident angle of the accompanying cooling airflow, causing the forced convection heat transfer peak region to deviate from the microcrack initiation sensitive region. When the high-frequency pulse count exceeds the pulse threshold, the follow-up tempering module switches to pulse output mode, causing the follow-up defocused laser beam to act on the in-situ tempering region at the same frequency as the transverse high-frequency oscillation.
[0111] The historical machining records of the same-specification grinding teeth in this invention include grinding tooth specifications, tooth tip width, the angle between the surface normal of the tooth flank transition zone and the direction of gravity, matrix hardness, powder type, laser power, scanning speed, powder feed rate, cooling flow rate, incident angle, oscillation amplitude, molten pool temperature, melt channel height, tooth pitch offset, acoustic emission energy accumulation rate, high-frequency pulse count, tempering power of the follow-up defocused laser beam, pulse duty cycle of the follow-up defocused laser beam, hardness of the metallurgical bonding cladding layer, thickness of the metallurgical bonding cladding layer, depth of the heat-affected zone, microcrack density, and crack detection results. These historical machining records are used to calibrate the tooth profile thermal sensitivity coefficient, target temperature range, melt channel height range, first flow rate gain coefficient, second flow rate gain coefficient, weight of feedback correction, preset acoustic emission energy threshold, angle compensation coefficient, pulse threshold, and duty cycle attenuation coefficient. The calibration process involves selecting multiple sets of grinding samples of the same specification and varying the laser power, scanning speed, powder feed rate, cooling flow rate, incident angle, and output parameters of the follow-up defocused laser beam. The evaluation indicators are the thickness range of the metallurgical bonding cladding layer, the final tooth pitch offset, the depth of the heat-affected zone, the microcrack density, and the shear strength of the bonding interface. Iterative fitting yields calibration coefficients and thresholds, which are then recorded in the historical processing records of grinding samples of the same specification. Process calibration does not change the grinding material or the basic principle of laser cladding; rather, it feeds back the processing results of the previous grinding process to the processing parameters of the next grinding process, ensuring that the heat input, cooling intensity, tempering power, acoustic emission state, and tooth profile error converge tooth by tooth in batch grinding processes.
[0112] Through the above embodiments, this invention combines the local cladding area, thermistor boundary, tooth surface heat input window, powder gradient scheme, partitioned scanning path, molten pool state feedback, accompanying cooling airflow, lateral high-frequency oscillation, acoustic emission monitoring, and in-situ tempering with a follow-up defocused laser beam into a continuous process chain. The local cladding area defines the processing location, the thermistor boundary defines the heat-affected zone, the tooth surface heat input window defines the laser energy input, the powder gradient scheme defines the material microstructure, the partitioned scanning path defines the molten pool formation sequence, the molten pool state feedback defines the process correction direction, the accompanying cooling airflow defines the heat dissipation intensity of the rapid solidification zone, the lateral high-frequency oscillation defines the molten pool spreading state of the tooth flank transition zone, the acoustic emission monitoring defines the microcrack initiation and grain boundary tearing state, and the follow-up defocused laser beam in-situ tempering defines the thermal stress release and solidification microstructure transformation state. The aforementioned process chain can improve the surface hardness and wear resistance of the grinding wheel teeth while reducing tooth pitch deviation, uneven tooth flank thickness, excessive heat-affected zone depth, microcrack density, and the risk of metallurgical interface cracking.
[0113] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention.
[0114] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. It should be noted that any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for grinding mills, characterized in that, include: Data on tooth surface morphology, tooth pitch deviation, matrix hardness, and corrosion traces of grinding discs in a pulper are obtained to generate local cladding areas and thermally sensitive boundaries. The tooth surface heat input window and powder gradient scheme are calculated based on the local cladding area and the thermal boundary, and the tooth surface heat input window is used as a linkage constraint of laser power, scanning speed and powder feed rate. Following the partitioned scanning path that extends from the tooth tip bearing zone to the tooth side transition zone, high-hardness alloy powder and the surface of the ground tooth are laser-co-melted to form a metallurgical bonding cladding layer. Collect the molten pool temperature, molten channel height and tooth pitch offset status, and use the molten pool status to reverse correct the partitioned scanning path, tooth surface heat input window and powder gradient scheme until the metallurgical bonding cladding layer is continuous and the thermally sensitive boundary does not cross the boundary. After cladding, the surface of the ground teeth is finished, the hardened layer is inspected, and the tooth shape is verified to obtain wear-resistant and reinforced grinding discs.
2. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for polishing mills according to claim 1, characterized in that, Before obtaining data on tooth surface morphology, tooth pitch deviation, matrix hardness, and corrosion traces of the grinding wheel teeth, the grinding wheel teeth of the grinding machine are subjected to degreasing, derusting, oxide layer removal, and tooth surface roughening treatment. The tooth surface roughness after the tooth surface roughening treatment is used as a condition for judging powder adhesion stability and input into the local cladding area generation process.
3. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for pulpers according to claim 1, characterized in that, The thermally sensitive boundary is a composite process boundary that includes geometric position constraints and thermal deformation constraints, generated by the tooth tip width, the angle between the surface normal of the tooth flank transition zone and the direction of gravity, the position of the tooth root avoidance zone, the tooth pitch deviation, and the hardness of the matrix. It is used to limit the range of thermal influence that can be transmitted to the core of the matrix during laser co-melting.
4. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for pulpers according to claim 3, characterized in that, The tooth surface thermal input window includes the tooth surface thermal input index, which is obtained by dividing the laser power by the product of the scanning speed and the spot width, and then multiplying by the tooth profile thermal sensitivity coefficient. The tooth profile thermal sensitivity coefficient is determined by the tooth surface curvature, tooth tip width, and tooth pitch deviation. The tooth surface thermal input index is used to link and constrain the laser power, scanning speed, and powder feed rate.
5. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for pulpers according to claim 1, characterized in that, The powder gradient scheme includes the powder ratio of the tooth tip bearing zone and the powder ratio of the tooth side transition zone. The powder ratio of the tooth tip bearing zone has a higher mass ratio of hard particles than the powder ratio of the tooth side transition zone. The powder ratio of the tooth side transition zone has a higher mass ratio of nickel-based alloy or cobalt-based alloy than the powder ratio of the tooth tip bearing zone. This is used to improve the toughness and interface transition stability of the metallurgical bonding cladding layer in the tooth side transition zone.
6. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for polishing mills according to claim 1, characterized in that, The partitioned scanning path includes the tooth tip bearing zone scanning section, the tooth flank transition zone scanning section, and the end buffer scanning section. The scanning direction of the tooth tip bearing zone scanning section is radially extended along the grinding disc of the refiner, the scanning direction of the tooth flank transition zone scanning section is extended along the tooth flank inclined surface, and the scanning speed of the end buffer scanning section is lower than that of the tooth tip bearing zone scanning section.
7. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for polishing mills according to claim 1, characterized in that, When collecting data on molten pool temperature, molten channel height, and tooth pitch offset, the molten pool temperature is obtained from infrared thermometry data, the molten channel height is obtained from laser profile measurement data, and the tooth pitch offset is obtained from the difference between the tooth pitch reference before cladding and the tooth pitch measurement value during cladding.
8. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for polishing mills according to claim 1, characterized in that, When laser co-melting high-hardness alloy powder and the surface of the ground teeth according to the partitioned scanning path that expands from the tooth tip bearing zone to the tooth side transition zone, an accompanying cooling airflow is applied to the tail of the molten pool. The cooling flow rate of the accompanying cooling airflow is dynamically generated based on the weighted sum of the tooth profile thermal sensitivity coefficient and the temperature deviation of the molten pool. The first flow gain coefficient and the second flow gain coefficient are calibrated by the historical processing records of the same specification ground teeth.
9. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for pulpers according to claim 8, characterized in that, When the partitioned scanning path is in the tooth side transition zone scanning section, a transverse high-frequency oscillation is applied to the laser beam. The oscillation amplitude of the transverse high-frequency oscillation increases with the angle between the normal of the tooth side transition zone surface and the direction of gravity. The oscillation amplitude of the transverse high-frequency oscillation is obtained by multiplying the preset maximum oscillation amplitude by the sine value of the angle between the normal of the tooth side transition zone surface and the direction of gravity, and then adding the minimum basic oscillation amplitude. The transverse high-frequency oscillation is used to improve the transverse spreading of the molten pool in the tooth side transition zone and reduce the unilateral accumulation of molten metal along the tooth side transition zone.
10. The method for laser cladding wear-resistant enhancement and surface hardening treatment of grinding discs for pulpers according to claim 9, characterized in that, Simultaneously, a cooling gas flow is applied to the tail of the molten pool, while a follower-driven defocused laser beam is applied behind the cooling gas flow to form an in-situ tempering zone. The follower-driven defocused laser beam moves synchronously with the laser cladding head and continuously covers the in-situ tempering zone behind the tail of the molten pool. Acoustic emission signal characteristic parameters of the in-situ tempering zone are collected by a piezoelectric ceramic sensor. The acoustic emission signal characteristic parameters include the acoustic emission energy accumulation rate and the high-frequency pulse count. The incident angle of the cooling gas flow and the tempering power of the follower-driven defocused laser beam are adjusted in real time in coordination with the acoustic emission energy accumulation rate and the angle between the surface normal of the tooth flank transition zone and the direction of gravity. The incident angle of the cooling gas flow satisfies the following: in, The incident angle of the accompanying cooling airflow, Let the initial incident angle be , This is the included angle compensation coefficient. The cumulative rate of acoustic emission energy is obtained by integrating the acoustic emission envelope amplitude over a fixed statistical period. To preset the acoustic emission energy threshold, The angle between the normal to the surface of the tooth flank transition zone and the direction of gravity. It is the natural logarithm function. The cosine function is calculated in degrees; the units of the incident angle, initial incident angle, angle compensation coefficient, and angle between the surface normal of the tooth flank transition zone and the direction of gravity are all °; the units of the acoustic emission energy accumulation rate and the preset acoustic emission energy threshold are both mV·s; when the calculated incident angle of the accompanying cooling airflow exceeds the execution range of 40° to 60°, the adjacent boundary value of the execution range is taken.