A titanium felt self-supporting anode containing iridium manganese active layer, membrane electrode assembly and preparation method and application thereof
By preparing a uniform iridium-manganese active layer on a titanium felt self-supporting anode and setting an independent Nafion ionomer layer on the surface of the proton exchange membrane, the problem of insufficient contact between the self-supporting anode and the proton exchange membrane was solved, improving the electrolysis performance and stability of proton exchange membrane water electrolysis for hydrogen production and reducing the amount of iridium used.
Patent Information
- Application Number
- CN202611512947.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the physical differences between the self-supporting anode and the proton exchange membrane lead to insufficient interfacial contact, resulting in high proton conduction impedance, which affects the electrolysis performance and long-term operational stability of proton exchange membrane water electrolysis for hydrogen production.
A self-supporting anode preparation method using titanium felt containing an iridium-manganese active layer was adopted. The titanium felt was treated with oxalic acid and coated with an iridium-manganese precursor solution, followed by calcination to form a uniform active layer. This active layer was then combined with a catalyst-free Nafion ionomer layer and hot-pressed onto the surface of a proton exchange membrane to establish a continuous proton conduction channel.
Stable contact between the self-supporting anode and the proton exchange membrane was achieved, reducing the interfacial proton conduction impedance, improving the electrolytic performance and long-term operational stability of the membrane electrode assembly, reducing the amount of iridium used, and balancing catalytic activity and economy.
Smart Images

Figure CN123153076A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of proton exchange membrane water electrolysis for hydrogen production technology, specifically to a titanium felt self-supporting anode containing an iridium-manganese active layer, a membrane electrode assembly, its preparation method, and its application. Background Technology
[0002] Proton exchange membrane (PEM) water electrolysis for hydrogen production boasts advantages such as high current density, rapid start-up and shutdown response, and high hydrogen purity, making it a crucial technological route for large-scale green hydrogen production. However, the anode operates in a strongly acidic, high-potential oxygen evolution environment, placing high demands on the activity and stability of the catalytic material, as well as the integration between the catalytic layer and the porous transport structure. Currently, iridium-based materials remain the only acidic oxygen evolution catalyst with practical application potential, but iridium resources are scarce and expensive, directly limiting the large-scale application of PEM electrolyzers. Therefore, how to maintain the activity and long-term operational stability of the catalytic layer while reducing iridium usage is a core issue that urgently needs to be addressed in this field.
[0003] Traditional membrane electrode assembly (MEA) fabrication often employs a catalyst coating process, where the catalyst is formulated into a slurry containing ionomers and then coated onto a proton exchange membrane or porous transport layer. In this process, the ionomers function as both proton conductors and binders within the catalyst layer, and their amount and distribution significantly impact electrolysis performance. Insufficient ionomers lead to decreased proton conductivity, while excessive ionomers occupy too much volume, increasing oxygen transport resistance and the contact resistance between the catalyst layer and the porous transport layer. More importantly, the slurry coating method relies primarily on physical adhesion between the catalyst layer and the substrate. During long-term operation of the electrolyzer, the intense oxygen evolution reaction on the anode side, accompanied by the generation and desorption of numerous bubbles, can easily cause the catalyst layer to detach from the substrate surface, resulting in a rapid decline in electrolysis performance. Researchers have explored various improvement methods to address this issue.
[0004] Patent CN112647086A discloses a titanium fiber felt anode diffusion layer for PEM water electrolysis cells and its preparation method. The method employs an impregnation-calcination method to prepare a catalytic protective coating on the surface of the titanium fiber felt. During calcination, a solid solution structure is formed between the substrate and the coating, effectively improving the stability of the catalytic layer. However, the catalytic activity of the catalytic layer obtained solely through the impregnation method is relatively limited, and the bonding strength between the catalytic layer and the substrate still needs further improvement.
[0005] Patent CN120818840A discloses a self-supporting anode electrode for PEM water electrolysis. This electrode uses a porous titanium substrate as a carrier, and the catalyst layer material has the general formula M1aM2bOx, where M1 is Ir and M2 can be various metal elements such as Mn. The preparation method employs a two-step process combining electrodeposition and impregnation-calcination. This approach achieves a tight bond between the catalyst and the substrate through electrochemical bonding, avoiding the interfacial resistance and detachment problems caused by binders in powdered catalysts. The corrosion resistance and mechanical strength of the titanium fiber felt further enhance the stability of the catalyst layer under long-term operation. However, while this self-supporting anode solves the catalyst detachment problem, its rigid porous structure differs significantly in physical properties from the flexible and dense proton exchange membrane. When the self-supporting anode is directly pressed into contact with the proton exchange membrane, the actual contact area between the two is limited, resulting in significant contact resistance at the interface.
[0006] Patent CN120033254A discloses a proton exchange membrane fuel cell with direct addition of ionomers and its preparation method. This method involves directly coating a Nafion solution onto the surface of a Pt / C catalyst layer on carbon paper, allowing the Nafion to penetrate into the macropores within the catalyst layer. This aims to reduce direct contact between the ionomers and the Pt surface, thereby preventing catalyst poisoning. While this approach has achieved good results in fuel cell systems, the ionomers penetrate into the interior of the catalyst layer, and the application is to a powdered catalyst layer on the cathode side. It does not address the interface construction between the self-supporting anode and the proton exchange membrane.
[0007] In summary, while existing technologies have made significant progress in the construction of self-supporting anodes, effectively improving the bonding stability between the catalyst layer and the substrate, an effective solution is still lacking for the problem of how to form a stable, low-impedance proton conduction interface between the self-supporting anode and the proton exchange membrane. The physical mismatch between the rigid porous characteristics of the self-supporting anode and the flexible and dense characteristics of the proton exchange membrane leads to insufficient interfacial contact after hot-pressing integration, resulting in discontinuous proton conduction channels and severely limiting the practical application effect of self-supporting anodes in PEM water electrolyzers.
[0008] Therefore, there is an urgent need for a membrane electrode assembly and its preparation method that can effectively bridge the self-supporting anode and the proton exchange membrane and establish a continuous proton conduction channel between them, so as to simultaneously achieve high stability and low interfacial impedance of the catalyst layer. Summary of the Invention
[0009] This invention addresses the problems existing in the prior art by providing a titanium felt self-supporting anode containing an iridium-manganese active layer, a membrane electrode assembly, its preparation method, and its application. It aims to solve the problems of insufficient interfacial contact and high proton conduction impedance between the self-supporting anode and the proton exchange membrane due to differences in physical properties. While maintaining a strong bond between the catalytic layer and the titanium felt substrate and reducing the amount of iridium used, it improves the interfacial proton conduction between the self-supporting anode and the proton exchange membrane, thereby enhancing the electrolytic performance and long-term operational stability of the membrane electrode assembly.
[0010] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of this invention provides a method for preparing a titanium felt self-supporting anode containing an iridium-manganese active layer, comprising the following steps: (i) The titanium felt is washed in an oxalic acid solution to obtain titanium felt treated with oxalic acid; (ii) Dissolve the iridium salt and manganese salt in a mixed solvent of ethanol and deionized water to obtain an iridium-manganese precursor solution; (iii) The iridium-manganese precursor solution is coated onto the surface of the titanium felt treated with oxalic acid, dried and then calcined. After calcination and cooling, the titanium felt is washed with deionized water and dried to obtain the titanium felt self-supporting anode with the iridium-manganese active layer.
[0011] Further, in step (i), the temperature of the oxalic acid solution is 60~80℃.
[0012] Further, in step (ii), the iridium salt is one or more of iridium trichloride, iridium tetrachloride, ammonium chloroiridate, iridium acetate, and iridium nitrate; the manganese salt is one or more of manganese acetate, manganese chloride, manganese sulfate, and manganese nitrate.
[0013] Further, in step (ii), the mass ratio of the iridium salt to the manganese salt is 1:0.5~2.
[0014] Further, in step (ii), the volume ratio of ethanol to deionized water is 1:0.5~2.
[0015] Furthermore, in step (iii), the coating is performed in multiple coats, with each coat dried under an infrared drying lamp for 2-3 minutes before the next coat is applied.
[0016] Further, in step (iii), the iridium loading in the iridium-containing manganese active layer is 0.2~0.8 mg / cm³. 2 .
[0017] Further, in step (iii), the calcination is carried out in an air atmosphere, the calcination temperature is 300~400℃, the heating rate is 4~6℃ / min, and the holding time is 1~3 h.
[0018] A second aspect of the present invention provides a titanium felt self-supporting anode containing an iridium-manganese active layer, which is prepared using the above-described method for preparing a titanium felt self-supporting anode containing an iridium-manganese active layer.
[0019] This invention first treats titanium felt with oxalic acid solution at 60-80℃. This removes the oxide layer and oil from the fiber surface and creates a micro-rough structure on the titanium fiber surface, introducing oxygen-containing functional groups. This provides a foundation for the uniform spreading of the precursor solution and the firm adhesion of the subsequent active layer. The precursor solution is applied through multiple coatings, each followed by infrared drying, allowing the iridium-manganese salt to be deposited layer by layer on the titanium fiber skeleton. This avoids localized accumulation and uneven distribution caused by excessive coating in a single step, and facilitates the formation of a uniform and continuous coating of the active layer on the three-dimensional porous skeleton surface of the titanium felt. The calcination temperature is controlled at 300-400℃, which allows the precursor salt to fully decompose and oxidize into iridium-manganese oxide while preventing excessive oxidation of the titanium felt surface at high temperatures, thus avoiding the formation of a thick insulating TiO2 layer. This maintains good electronic conductivity between the active layer and the titanium substrate. The self-supporting anode prepared by this invention has an iridium-manganese active layer uniformly distributed on the surface of titanium fibers. When this anode is hot-pressed into contact with the Nafion ionomer layer on the proton exchange membrane, the active layer can form a relatively uniform contact with the Nafion layer across the entire outer surface of the titanium felt skeleton, rather than just at local protrusions. This facilitates the establishment of a uniformly distributed proton conduction channel between the self-supporting anode and the proton exchange membrane. Compared with the two-step method of electrodeposition combined with impregnation and calcination, the preparation method of this invention is simpler, and the iridium-manganese element distribution in the active layer is more uniform, which is beneficial for maintaining catalytic activity at a lower iridium content.
[0020] A third aspect of the present invention provides a membrane electrode assembly, comprising carbon paper, a Pt / C cathode catalyst layer, a proton exchange membrane, a Nafion (perfluorosulfonic acid) ionomer layer, and an iridium-manganese-containing active layer, stacked sequentially. The Pt / C cathode catalyst layer is disposed on a first surface of the proton exchange membrane, and the Nafion ionomer layer is disposed on a second surface of the proton exchange membrane. The carbon paper is in contact with the Pt / C cathode catalyst layer, and the titanium felt self-supporting anode is in contact with the Nafion ionomer layer. The Nafion ionomer layer is an independent layer without a catalyst.
[0021] Furthermore, the Nafion ionomer layer is formed by coating the second surface of the proton exchange membrane with a diluted Nafion solution.
[0022] The self-supporting titanium felt anode is a rigid porous structure, while the proton exchange membrane is a flexible, dense film. When the two are directly hot-pressed, the actual contact only occurs in a localized area where the titanium fibers and the membrane surface are close together. Numerous microscopic voids exist between the titanium felt pores and the membrane surface, making it difficult for protons to effectively conduct. This invention pre-forms a catalyst-free Nafion ionomer layer on the surface of the proton exchange membrane. During hot pressing, this layer softens and fills the microscopic voids between the titanium felt fibers and the membrane, allowing the proton conduction channel to extend continuously from the proton exchange membrane through the Nafion layer to the iridium-manganese-containing active layer on the titanium felt surface, thereby reducing the interfacial proton conduction impedance. Unlike the conventional practice of mixing Nafion with a catalyst to form a slurry, the Nafion layer in this invention is catalyst-free and exists independently between the membrane and the self-supporting anode. Unlike a mixed slurry, it does not encapsulate the ionomer around the catalyst particles, thus avoiding large-area coverage of the active sites inside the catalyst layer while establishing an interfacial proton conduction channel. Compared with coating the surface of the catalyst layer with Nafion to allow it to penetrate into the interior of the catalyst layer, the Nafion layer of the present invention does not penetrate into the internal pores of the titanium felt. Instead, it forms a continuous proton conduction thin layer mainly in the interface region between the membrane and the titanium felt surface. This ensures the proton transport efficiency at the interface and avoids the large amount of ionomers entering the interior of the titanium felt, blocking the porous transport channels and affecting oxygen exhaust.
[0023] Furthermore, the carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer, and titanium felt self-supporting anode are hot-pressed together into an integral structure.
[0024] A fourth aspect of the present invention provides a method for preparing the above-mentioned membrane electrode assembly, comprising the following steps: (1) Pt / C catalyst is prepared into a slurry and coated onto the first surface of the proton exchange membrane to form a Pt / C cathode catalyst layer; a diluted Nafion solution is coated onto the second surface of the proton exchange membrane to form an independent Nafion ionomer layer without catalyst; (2) The carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer and titanium felt self-supporting anode containing iridium and manganese active layer are stacked in the order of carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer and titanium felt self-supporting anode containing iridium and manganese active layer, so that the carbon paper is in contact with the Pt / C cathode catalyst layer and the titanium felt self-supporting anode containing iridium and manganese active layer is in contact with the Nafion ionomer layer. (3) The laminate obtained in step (2) is hot-pressed to obtain the membrane electrode assembly.
[0025] Further, in step (1), the diluted Nafion solution is obtained by diluting the Nafion stock solution with a mixed solvent of water and isopropanol, and the concentration of the diluted Nafion solution is 0.5~2 wt%.
[0026] Furthermore, in step (1), the thickness of the Nafion ionomer layer is 1~5 μm.
[0027] Furthermore, in step (3), the temperature of the hot pressing is 120~140℃.
[0028] A fifth aspect of the present invention provides a proton exchange membrane water electrolyzer, which includes the membrane electrode assembly described in the present invention, wherein the titanium felt self-supporting anode containing an iridium-manganese active layer is located on the anode side, and the Pt / C cathode catalyst layer and the carbon paper are located on the cathode side.
[0029] The sixth aspect of the present invention provides a method for producing hydrogen by water electrolysis, which uses the proton exchange membrane water electrolysis cell described in the present invention to electrolyze water and obtain hydrogen from the cathode side.
[0030] Compared with the prior art, the present invention has the following beneficial effects: This invention achieves a synergistic improvement in catalytic layer stability, interfacial proton conduction, and electrolysis performance through the coordinated fabrication of a self-supporting anode and the structural design of the membrane electrode assembly. The self-supporting anode is prepared using a one-step method of coating a precursor solution followed by calcination. The active layer is uniformly distributed on the surface of the titanium felt and firmly bonded to the substrate, making it less prone to detachment during long-term oxygen evolution operation. Furthermore, the synergistic effect of manganese reduces the amount of iridium required, balancing catalytic activity and economy. In the membrane electrode assembly, a Pt / C cathode catalyst layer and an independent Nafion ionomer layer are respectively disposed on both sides of the proton exchange membrane. The latter, after hot pressing, fills the microscopic voids between the self-supporting anode and the membrane, establishing a continuous proton conduction channel. This ensures stable contact between the rigid porous structure of the self-supporting anode and the flexible, dense surface of the proton exchange membrane, avoiding the proton conduction obstruction caused by insufficient interfacial contact in traditional structures. Simultaneously, this Nafion layer is independent of the catalyst layer, does not encapsulate the Ir-Mn active sites inside the titanium felt, and does not block the porous transport channels. Thus, while improving interfacial proton conduction, it retains the intrinsic activity and mass transfer performance of the catalyst layer. Therefore, the membrane electrode assembly provided by this invention exhibits a lower electrolyzer voltage and good long-term operational stability, providing a technical solution for proton exchange membrane water electrolysis hydrogen production that combines performance and process feasibility. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the structure of the membrane electrode assembly of the present invention and a schematic diagram of the preparation process of the titanium felt self-supporting anode containing an iridium-manganese active layer.
[0032] Figure 2The images show the surface morphology and elemental distribution of the titanium felt self-supporting anode with an iridium-manganese active layer obtained in Example 1. (a) is a low-magnification scanning electron microscope (SEM) image, (e) is a high-magnification SEM image, and (b) to (d) are elemental distribution diagrams of Ti, Ir, and Mn, respectively.
[0033] Figure 3 The graphs shown are the oxygen evolution reaction performance test results of the self-supported anodes obtained in Examples 1, 1, 2 and 6, where (a) is the polarization curve, (b) is the electrochemical impedance spectroscopy, and (c) is the Tafel slope diagram.
[0034] Figure 4 The self-supporting anodes obtained in Example 1, Comparative Example 2, and Comparative Example 6 were tested at 100 mA cm⁻¹. -2 Graph of constant current stability test under current density.
[0035] Figure 5 The self-supporting anode obtained in Example 1 at 10 mA cm -2 Graph of constant current stability test under current density.
[0036] Figure 6 The figures show the single-cell performance test results of the membrane electrode assemblies obtained in Examples 2, 3-5, and 7-9, where (a) is the polarization curve and (b) is the 500 mA cm⁻¹ curve. -2 Graph of constant current stability test under current density.
[0037] Figure 7 The membrane electrode assembly obtained in Example 2 was measured at 1 A cm. -2 Graph of constant current stability test under current density.
[0038] Figure 8 The images show the single-cell electrochemical impedance spectroscopy and relaxation time distribution of the membrane electrode assembly obtained in Examples 2, 5, 8 and 9, where (a) is the electrochemical impedance spectroscopy and (b) is the relaxation time distribution of Examples 2 and 5. Detailed Implementation
[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise specified, the raw materials used in the embodiments are all commercially available products.
[0040] Figure 1This is a schematic diagram of the structure of the membrane electrode assembly of the present invention and a schematic diagram of the fabrication process of the titanium felt self-supporting anode containing an iridium-manganese active layer. In the figure, the membrane electrode assembly, from left to right, includes carbon paper, a Pt / C cathode catalyst layer, a proton exchange membrane, a Nafion ionomer layer, and a titanium felt self-supporting anode containing an iridium-manganese active layer. The Pt / C cathode catalyst layer is disposed on the left side of the proton exchange membrane, and the Nafion ionomer layer is disposed on the right side; the carbon paper is in contact with the Pt / C cathode catalyst layer, and the titanium felt self-supporting anode containing the iridium-manganese active layer is in contact with the Nafion ionomer layer. Figure 1 The upper right side shows the preparation process of the titanium felt self-supporting anode with an iridium-manganese active layer: manganese salt and iridium salt are mixed to form a precursor solution, which is coated on the pretreated titanium felt surface. After drying and calcination, the titanium felt self-supporting anode with an iridium-manganese active layer is obtained.
[0041] Example 1 This embodiment provides a titanium felt self-supporting anode containing an iridium-manganese active layer, the preparation method of which is as follows: (i) Take 2×2 cm 2 Titanium felt is washed in an oxalic acid solution at 70°C to obtain oxalic acid-treated titanium felt.
[0042] (ii) Iridium trichloride and manganese acetate are dissolved in a mixed solvent of ethanol and deionized water in a mass ratio of 1:1 to obtain an iridium-manganese precursor solution.
[0043] (iii) The iridium-manganese precursor solution was coated onto the oxalic acid-treated titanium felt surface obtained in step (i). This coating was repeated three times, with each coating followed by drying under an infrared drying lamp for 2 minutes before the next coating. After coating, the titanium felt was placed in air and heated to 350°C at a rate of 5°C / min, held at that temperature for 2 hours, calcined, and then cooled to room temperature in the furnace. It was then washed with deionized water and dried to obtain a self-supporting titanium felt anode with an iridium-manganese active layer, wherein the iridium loading was 0.4 mg / cm³. 2 .
[0044] Figure 2 The images show the surface morphology and elemental distribution of the titanium felt self-supporting anode with an iridium-manganese active layer obtained in Example 1. Image (a) is a low-magnification scanning electron microscope (SEM) image, image (e) is a high-magnification SEM image, and images (b)-(d) are elemental distribution maps of Ti, Ir, and Mn, respectively. The self-supporting anode obtained in Example 1 was characterized using scanning electron microscopy, and its surface elemental distribution was determined by energy dispersive spectroscopy (EDS). Figure 2 (a) It can be seen that the titanium felt has a complete fiber skeleton structure, and the fiber surface is covered by an active layer; from Figure 2 (e) It can be seen that a relatively uniform active layer has formed on the surface of the titanium fiber; from Figure 2As can be seen from (b) to (d), Ti is uniformly distributed on the fiber skeleton, and Ir and Mn are uniformly anchored on the surface of the titanium fiber without obvious agglomeration or local enrichment. These results indicate that the iridium-manganese active layer obtained by the method of this invention is uniformly distributed on the surface of the titanium felt and has good adhesion to the titanium substrate.
[0045] Example 2 This embodiment provides a membrane electrode assembly, the preparation method of which is as follows: (1) Pt / C catalyst is mixed with isopropanol to prepare Pt / C slurry. The Pt / C slurry is sprayed onto the first surface of the proton exchange membrane (N115) to form a Pt / C cathode catalyst layer. The Nafion stock solution is diluted with a mixed solvent of water and isopropanol at a mass ratio of 1:2 to a concentration of 1 wt%. The diluted Nafion solution is sprayed onto the second surface of the proton exchange membrane to form an independent Nafion ionomer layer without catalyst. The thickness of the Nafion ionomer layer is 2 μm.
[0046] (2) The carbon paper, the Pt / C cathode catalyst layer obtained in step (1), the proton exchange membrane, the Nafion ionomer layer and the titanium felt self-supporting anode containing the iridium-manganese active layer obtained in Example 1 are stacked in that order, so that the carbon paper is in contact with the Pt / C cathode catalyst layer and the titanium felt self-supporting anode containing the iridium-manganese active layer is in contact with the Nafion ionomer layer.
[0047] (3) Place the laminate obtained in step (2) in a hot press and hot press at 135°C to obtain the membrane electrode assembly.
[0048] Example 3 This embodiment provides a method for producing hydrogen by water electrolysis, using the membrane electrode assembly obtained in Example 2. The specific method is as follows: The membrane electrode assembly obtained in Example 2 was installed in a proton exchange membrane water electrolyzer. The titanium felt self-supporting anode containing an iridium-manganese active layer was located on the anode side, and the Pt / C cathode catalyst layer and the carbon paper were located on the cathode side. Water was supplied to the anode side of the proton exchange membrane water electrolyzer. At 80°C, an electrolysis voltage was applied between the anode side and the cathode side, causing the water to undergo an oxygen evolution reaction on the anode side to generate oxygen and protons. The protons were conducted to the cathode side through the Nafion ionomer layer and the proton exchange membrane, where a hydrogen evolution reaction occurred to generate hydrogen gas. Hydrogen gas was obtained from the cathode side.
[0049] Comparative Example 1 This comparative example provides a pure Ir self-supporting anode, the preparation method of which is as follows: (i) Take 2×2 cm 2Titanium felt is washed in an oxalic acid solution at 70°C to obtain oxalic acid-treated titanium felt.
[0050] (ii) Dissolve iridium trichloride in a mixed solvent of ethanol and deionized water in a volume ratio of 1:1 to obtain an iridium-containing precursor solution.
[0051] (iii) The iridium-containing precursor solution obtained in step (ii) is coated onto the oxalic acid-treated titanium felt surface obtained in step (i). This coating is repeated three times, with each coating followed by drying under an infrared drying lamp for 2 minutes before the next coating. After coating, the titanium felt is placed in air and heated to 350°C at a rate of 5°C / min, held at that temperature for 2 hours, calcined, and then cooled to room temperature in the furnace. It is then washed with deionized water and dried to obtain a pure Ir self-supporting anode with an iridium loading of 0.4 mg / cm³. 2 .
[0052] Comparative Example 2 This comparative example provides a commercial IrO2 self-supporting anode, the preparation method of which is as follows: Commercial IrO2 powder was mixed with isopropanol to prepare a slurry, which was then coated onto a 2×2 cm substrate. 2 The titanium felt surface was dried at room temperature to obtain a commercially available IrO2 self-supporting anode with an iridium loading of 0.4 mg / cm³. 2 .
[0053] Comparative Example 3 This comparative example provides a membrane electrode assembly, the preparation method of which is as follows: (1) A slurry was prepared by mixing commercial IrO2 powder with isopropanol and then coated onto a 2×2 cm plate. 2 The titanium felt surface was dried at room temperature to obtain a commercial IrO2 anode with an iridium loading of 0.4 mg / cm³. 2 .
[0054] (2) The Pt / C catalyst is prepared into a slurry and sprayed onto the first surface of the proton exchange membrane to form a Pt / C cathode catalyst layer; the Nafion stock solution is diluted with a mixed solvent of water and isopropanol at a mass ratio of 1:2 to a concentration of 1 wt%, and the resulting diluted Nafion solution is sprayed onto the second surface of the proton exchange membrane to form an independent Nafion ionomer layer without catalyst, the thickness of which is 2 μm.
[0055] (3) Stack carbon paper, Pt / C cathode catalyst layer obtained in step (2), proton exchange membrane, Nafion ionomer layer and commercial IrO2 anode obtained in step (1) in that order, so that the carbon paper is in contact with the Pt / C cathode catalyst layer and the commercial IrO2 anode is in contact with the Nafion ionomer layer; place the resulting stack in a hot press and hot press at 135°C to obtain the membrane electrode assembly.
[0056] Comparative Example 4 This comparative example provides a membrane electrode assembly, the preparation method of which is as follows: (1) A slurry was prepared by mixing commercial IrO2 powder with isopropanol and directly coated onto the second surface of a proton exchange membrane. The slurry was then dried at room temperature to form an anode catalyst layer, wherein the iridium loading was 0.4 mg / cm³. 2 .
[0057] (2) The Pt / C catalyst is prepared into a slurry and sprayed onto the first surface of the proton exchange membrane to form a Pt / C cathode catalyst layer.
[0058] (3) Stack carbon paper, Pt / C cathode catalyst layer obtained in step (2), proton exchange membrane and anode catalyst layer obtained in step (1) in that order, so that the carbon paper is in contact with the Pt / C cathode catalyst layer; place the resulting stack in a hot press and hot press at 135°C to obtain the membrane electrode assembly.
[0059] Comparative Example 5 This comparative example provides a membrane electrode assembly, the preparation method of which is as follows: (1) The Pt / C catalyst is prepared into a slurry and sprayed onto the first surface of the proton exchange membrane to form a Pt / C cathode catalyst layer.
[0060] (2) The carbon paper, the Pt / C cathode catalyst layer obtained in step (1), the proton exchange membrane and the titanium felt self-supporting anode containing the iridium-manganese active layer obtained in Example 1 are stacked in that order, so that the carbon paper is in contact with the Pt / C cathode catalyst layer and the titanium felt self-supporting anode containing the iridium-manganese active layer is in direct contact with the second surface of the proton exchange membrane.
[0061] (3) Place the laminate obtained in step (2) in a hot press and hot press at 135°C to obtain the membrane electrode assembly.
[0062] Comparative Example 6 This comparative example provides a self-supporting titanium felt anode containing an iridium-manganese active layer, the preparation method of which is as follows: (1) Take 2×2 cm 2 The titanium felt was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 10 min each, and then dried at 80℃ for 2 h.
[0063] (2) Dissolve manganese acetate and ammonium chloride in deionized water to prepare a metal ion electrodeposition solution, wherein the concentration of manganese acetate is 0.1 mol / L and the molar ratio of ammonium chloride to manganese ions is 2:1.
[0064] (3) The titanium felt obtained in step (1) is used as the working electrode, the platinum sheet as the counter electrode, and the saturated calomel electrode as the reference electrode. Constant potential deposition is carried out in the electrodeposition solution obtained in step (2). The deposition potential is 2.72 V and the deposition time is 180 s.
[0065] (4) After rinsing the electrode obtained in step (3) with deionized water, place it in a muffle furnace and calcine it at 350°C for 3 h in an air atmosphere at a rate of 5°C / min. Then cool it to room temperature with the furnace to obtain the MnO2 / Ti electrode.
[0066] (5) Dissolve iridium trichloride in isopropanol to prepare an iridium salt impregnation solution with a concentration of 10 g / L.
[0067] (6) The MnO2 / Ti electrode obtained in step (4) was immersed in the iridium salt impregnation solution obtained in step (5) for 1 h, then dried at 80 °C for 1 h, and then placed in a muffle furnace and calcined at 350 °C for 3 h with the temperature increased at 5 °C / min. After cooling to room temperature in the furnace, a titanium felt self-supported anode containing an iridium-manganese active layer was obtained, with an iridium loading of 0.4 mg / cm³. 2 .
[0068] Comparative Example 7 This comparative example provides a membrane electrode assembly, which differs from Example 2 in that the titanium felt self-supporting anode with an iridium-manganese active layer obtained in Example 1 is replaced with the titanium felt self-supporting anode with an iridium-manganese active layer obtained in Comparative Example 6, while the rest is the same as in Example 2.
[0069] Comparative Example 8 This comparative example provides a membrane electrode assembly, which differs from Example 2 in that: a self-supporting titanium felt anode with an iridium-manganese active layer obtained in Example 1 is used, and it is immersed in a diluted Nafion solution. The diluted Nafion solution is prepared by diluting the Nafion stock solution with a mixed solvent of water and isopropanol at a mass ratio of 1:2 to a concentration of 1 wt%. After immersion, it is removed and dried at 60°C, so that Nafion fills the pores of the titanium felt and contacts the iridium-manganese active layer. The second surface of the proton exchange membrane does not have an independent Nafion ionomer layer. Everything else is the same as in Example 2.
[0070] Comparative Example 9 This comparative example provides a membrane electrode assembly, which differs from Example 2 in that: a titanium felt self-supporting anode with an iridium-manganese active layer obtained in Example 1 is used, and a diluted Nafion solution is coated on the surface of its iridium-manganese active layer. The diluted Nafion solution is obtained by diluting the Nafion stock solution with a mixed solvent of water and isopropanol at a mass ratio of 1:2 to a concentration of 1 wt%. After coating, it is dried to form a Nafion coating layer on the surface of the self-supporting anode; no independent Nafion ionomer layer is provided on the second surface of the proton exchange membrane; the rest is the same as in Example 2.
[0071] Performance testing I. Self-supporting anode performance test Electrochemical performance tests were performed on the self-supported anodes obtained in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 6. A three-electrode system was used in the tests on a Chenhua CHI 760E electrochemical workstation. The self-supported electrode obtained in each example or comparative example was used as the working electrode, a platinum sheet electrode as the counter electrode, and a saturated calomel electrode as the reference electrode. The electrolyte was a 0.5 mol / L sulfuric acid solution, and the test temperature was 25°C. The linear sweep voltammetry curves were performed at a scan rate of 2 mV / s with 85% manual compensation. In the galvanostatic test, a constant current was applied to the working electrode, and the voltage change over time was recorded.
[0072] Figure 3 The figures show the oxygen evolution reaction performance test results of the self-supported anodes obtained in Examples 1, 1, 2, and 6, where (a) is the polarization curve, (b) is the electrochemical impedance spectroscopy, and (c) is the Tafel slope diagram. Figure 3 (a) It can be seen that the self-supporting anode obtained in Example 1 is at 10 mA cm⁻¹ -2 and 100 mA cm -2 The overpotentials at 10 mA cm⁻¹ were 203 mV and 280 mV, respectively; those at Comparative Example 1 were 223 mV and 323 mV, respectively; those at Comparative Example 2 were 253 mV and 354 mV, respectively; and those at Comparative Example 6 were at 10 mA cm⁻¹. -2 The overpotential of Example 1 was 259 mV, which was significantly lower than that of Comparative Examples 1, 2, and 6. Figure 3 (b) It can be seen that the semicircular diameter of the electrochemical impedance spectrum of Example 1 is smaller than that of Comparative Examples 1, 2, and 6, indicating that its charge transfer resistance is lower. Figure 3 (c) It can be seen that the Tafel slope of Example 1 is 69.7 mV dec -1 Comparative Example 1 is 92.2 mVdec -1 Comparative Example 2 is 93.6 mV dec -1 The Tafel slope of Comparative Example 6 is 128.3 mV dec. -1The Tafel slope of Example 1 is significantly smaller than that of Comparative Examples 1, 2, and 6. These results indicate that the titanium felt self-supporting anode with an iridium-manganese active layer obtained in Example 1 possesses excellent oxygen evolution reaction activity and kinetic performance.
[0073] Figure 4 The self-supporting anodes obtained in Example 1, Comparative Example 2, and Comparative Example 6 were tested at 100 mA cm⁻¹. -2 Graphs showing the constant current stability test at current density. Figure 4 It can be seen that in Example 1 at 100 mA cm -2 Comparative Example 2 operated stably for over 450 hours with a relatively stable voltage; Comparative Example 6 experienced a rapid voltage increase to above 2.0 V after approximately 50 hours of operation, indicating electrode deactivation; Comparative Example 6 operated at 100 mA cm⁻¹ -2 The voltage rose to over 2.0 V after only about 3 hours of operation. These results demonstrate that the self-supporting anode obtained in Example 1 exhibits excellent stability under prolonged high-current operation.
[0074] Figure 5 The self-supporting anode obtained in Example 1 at 10 mA cm -2 Graphs showing the constant current stability test at current density. Figure 5 It can be seen that in Example 1 at 10 mA cm -2 The voltage remained essentially constant during nearly 1000 hours of stable operation; the above results indicate that the self-supporting anode obtained in Example 1 also exhibits excellent stability under long-term low-current operation.
[0075] II. Performance Testing of Membrane Electrode Modules Single-cell performance tests were conducted on the membrane electrode assemblies obtained in Examples 2, 3-5, and 7-9. Each membrane electrode assembly was installed in a proton exchange membrane water electrolyzer, with the titanium felt self-supporting anode containing an iridium-manganese active layer located on the anode side, and the Pt / C cathode catalyst layer and carbon paper located on the cathode side. The test temperature was 80°C, and deionized water was supplied to the anode side. Polarization curves were determined using the linear sweep voltammetry method, and the constant current stability test recorded the change in cell voltage over time at a constant current density.
[0076] Figure 6 The figures show the single-cell performance test results of the membrane electrode assemblies obtained in Examples 2, 3-5, and 7-9, where (a) is the polarization curve and (b) is the 500 mA cm⁻¹ curve. -2 Graphs showing the constant current stability test at current density. Figure 6 (a) It can be seen that at 1 A cm -2At the given current density, the slot voltage of Example 2 was 1.672 V, the slot voltage of Comparative Example 3 was 2.013 V, the slot voltage of Comparative Example 4 was 1.888 V, the slot voltage of Comparative Example 5 was 1.692 V, and the slot voltages of Comparative Examples 7-9 were 1.801 V, 1.692 V, and 1.712 V, respectively. The slot voltage of Example 2 was significantly lower than that of Comparative Examples 3, 4, and 7-9. Figure 6 (b) It can be seen that at 500 mA cm⁻¹ -2 In Example 2, the cell voltage remained stable for over 350 hours, consistently around 1.65 V. Comparative Examples 3 and 4 showed a rapid increase in cell voltage to over 2.0 V after approximately 50 hours of operation. Comparative Example 5, while operating stably in the electrolytic cell, exhibited a higher cell voltage than Example 2 after the same operating time. Comparative Example 7 failed to operate stably in the electrolytic cell, with its voltage rising to 2 V within hours. Comparative Examples 8 and 9, while operating stably in the electrolytic cell, also showed higher cell voltages than Example 2 after the same operating time. These results indicate that the membrane electrode assembly obtained in Example 2 exhibits lower electrolytic cell voltage and better long-term stability. The independent Nafion ionomer layer on the second surface of the proton exchange membrane effectively improves the proton conduction contact between the self-supporting anode and the proton exchange membrane, thereby reducing the electrolytic cell voltage.
[0077] Figure 7 The membrane electrode assembly obtained in Example 2 was measured at 1 A cm. -2 Graphs showing the constant current stability test at current density. Figure 7 It can be seen that in Example 2, at 1 A cm -2 The cell voltage remained relatively stable after more than 250 hours of stable operation. These results demonstrate that the membrane electrode assembly obtained in Example 2 also exhibits excellent stability under high current densities.
[0078] Figure 8 The images show the single-cell electrochemical impedance spectroscopy and relaxation time distribution of the membrane electrode assemblies obtained in Examples 2, 5, 8, and 9, where (a) is the electrochemical impedance spectroscopy and (b) is the relaxation time distribution of Examples 2 and 5. Figure 8(a) It can be seen that the electrochemical impedance spectroscopy (EIS) of Example 2 has the smallest semicircular diameter, indicating that its charge transfer impedance is the lowest. Comparative Examples 8 and 9, which respectively use Nafion impregnation to fill the pores of titanium felt and Nafion coating on the anode surface, both have larger semicircular diameters than Example 2, indicating that placing Nafion on the self-supporting anode side leads to increased charge transfer impedance. Comparative Example 5, which does not have an independent Nafion ionomer layer, also has a larger semicircular diameter than Example 2, indicating that the lack of an independent Nafion layer hinders interfacial proton transport. To further illustrate the optimization effect of Example 2 on proton transport, the relaxation time distribution of the EIS data of Example 2 and Comparative Example 5 was fitted, and the results are as follows: Figure 8 As shown in (b). Studies in this field have shown that in the high-frequency region (τ≈10... -4 s) is usually attributed to the anodic proton transport process. From Figure 8 (b) It can be seen that in Example 2, τ≈10 -4 The peak area at point s is smaller than that in Comparative Example 5, indicating that the independent Nafion ionomer layer in Example 2 effectively reduced the anodic proton transport impedance and optimized proton conduction within the membrane electrode assembly.
[0079] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, and is not intended to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention do not depart from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a titanium felt self-supporting anode containing an iridium-manganese active layer, characterized in that, Includes the following steps: (i) The titanium felt is washed in an oxalic acid solution to obtain titanium felt treated with oxalic acid; (ii) Dissolve the iridium salt and manganese salt in a mixed solvent of ethanol and deionized water to obtain an iridium-manganese precursor solution; (iii) The iridium-manganese precursor solution is coated onto the surface of the titanium felt treated with oxalic acid, dried and then calcined. After calcination and cooling, the titanium felt is washed with deionized water and dried to obtain the titanium felt self-supporting anode with the iridium-manganese active layer.
2. The preparation method according to claim 1, characterized in that, In step (ii), the iridium salt is one or more of iridium trichloride, iridium tetrachloride, ammonium chloroiridate, iridium acetate, and iridium nitrate; the manganese salt is one or more of manganese acetate, manganese chloride, manganese sulfate, and manganese nitrate.
3. The preparation method according to claim 1, characterized in that, In step (ii), the mass ratio of the iridium salt to the manganese salt is 1:0.5~2; the volume ratio of the ethanol to the deionized water is 1:0.5~2.
4. The preparation method according to claim 1, characterized in that, In step (iii), the coating is performed multiple times, with each coating followed by drying under an infrared drying lamp for 2-3 minutes before the next coating is applied; in step (iii), the iridium loading in the iridium-manganese active layer is 0.2-0.8 mg / cm³. 2 In step (iii), the calcination is carried out in an air atmosphere, the calcination temperature is 300~400℃, the heating rate is 4~6℃ / min, and the holding time is 1~3 h.
5. A titanium felt self-supporting anode containing an iridium-manganese active layer, characterized in that, It is prepared by the method for preparing the titanium felt self-supporting anode containing an iridium-manganese active layer as described in any one of claims 1-4.
6. A membrane electrode assembly, characterized in that, The anode comprises, in sequence, carbon paper, a Pt / C cathode catalyst layer, a proton exchange membrane, a Nafion ionomer layer, and a titanium felt self-supporting anode containing an iridium-manganese active layer; the Pt / C cathode catalyst layer is disposed on the first surface of the proton exchange membrane, and the Nafion ionomer layer is disposed on the second surface of the proton exchange membrane; the carbon paper is in contact with the Pt / C cathode catalyst layer, and the titanium felt self-supporting anode is in contact with the Nafion ionomer layer; the Nafion ionomer layer is an independent layer without catalyst.
7. The membrane electrode assembly according to claim 6, characterized in that, The Nafion ionomer layer is formed by coating the second surface of the proton exchange membrane with a diluted Nafion solution.
8. The membrane electrode assembly according to claim 6, characterized in that, The carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer, and titanium felt self-supporting anode are hot-pressed together into an integral structure.
9. A method for preparing a membrane electrode assembly according to any one of claims 6-8, characterized in that, Includes the following steps: (1) Pt / C catalyst is prepared into a slurry and coated onto the first surface of the proton exchange membrane to form a Pt / C cathode catalyst layer; a diluted Nafion solution is coated onto the second surface of the proton exchange membrane to form an independent Nafion ionomer layer without catalyst; (2) The carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer and titanium felt self-supporting anode containing iridium and manganese active layer are stacked in the order of carbon paper, Pt / C cathode catalyst layer, proton exchange membrane, Nafion ionomer layer and titanium felt self-supporting anode containing iridium and manganese active layer, so that the carbon paper is in contact with the Pt / C cathode catalyst layer and the titanium felt self-supporting anode containing iridium and manganese active layer is in contact with the Nafion ionomer layer. (3) The laminate obtained in step (2) is hot-pressed to obtain the membrane electrode assembly.
10. The preparation method according to claim 9, characterized in that, In step (1), the diluted Nafion solution is obtained by diluting the Nafion stock solution with a mixed solvent of water and isopropanol, and the concentration of the diluted Nafion solution is 0.5~2wt%; in step (1), the thickness of the Nafion ionomer layer is 1~5 μm; in step (3), the hot pressing temperature is 120~140℃.
Citation Information
Patent Citations
Titanium fiber felt anode diffusion layer for PEM water electrolysis tank as well as preparation method and application thereof
CN112647086A
Proton exchange membrane fuel cell with directly added ionomer and preparation method of proton exchange membrane fuel cell
CN120033254A
PEM electrolyzed water self-supporting anode electrode and preparation method and application thereof
CN120818840A