A CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis and its preparation method

By growing a Ni₃S₂-Co₉S₈ core in situ on the surface of nickel foam and electrodepositing a CoFe-LDH shell, a CoFe-LDH@Ni₃S₂-Co₉S₈/NF electrode was prepared. This solved the problem of slow reaction kinetics of water electrolysis catalysts in HER and OER, achieving high efficiency and stability while reducing costs.

CN123153084APending Publication Date: 2026-11-24JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611335808.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing water electrolysis catalysts exhibit slow reaction kinetics in the hydrogen evolution reaction (HER) and oxygen evolution reaction (OER), making it difficult to simultaneously meet the different optimization requirements for the adsorption energy of reaction intermediates. Furthermore, precious metal catalysts are expensive and scarce, resulting in low energy conversion efficiency in water electrolysis.

Method used

A bifunctional electrode, CoFe-LDH@Ni₃S₂-Co₉S₈/NF, was formed by in-situ growth of a composite sulfide core on a nickel foam surface and electrodeposition of a CoFe-LDH shell on it. The synergistic effect of the core and shell was utilized to improve catalytic activity and conductivity.

Benefits of technology

It achieves high-efficiency HER and OER performance, reduces charge transfer resistance, improves the stability and activity of catalytic reactions, simplifies the preparation process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153084A_ABST
    Figure CN123153084A_ABST
Patent Text Reader

Abstract

This invention discloses a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis and its preparation method, relating to the field of electrocatalytic materials technology. The preparation method of the bifunctional electrode is as follows: Nickel foam is pretreated on the surface, then the pretreated nickel foam is mixed with a mixed aqueous solution of nickel salt, cobalt salt, and urea and heated to obtain a precursor. The precursor is mixed with a sulfur source solution and then heated to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray. A three-electrode system is used, with the nickel foam-supported Ni3S2-Co9S8 nanoarray as the working electrode, a saturated calomel electrode as the reference electrode, and a platinum sheet as the counter electrode. Electrodeposition is performed in an electrolyte composed of cobalt salt and ferrous salt to obtain the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis. This invention achieves the preparation of an electrode material with both excellent conductivity and abundant active sites through the synergistic effect of the preparation process and raw materials. The operation process is simple, the raw materials are readily available, there is no pollution, and no expensive equipment is required, showing broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis and its preparation method, belonging to the field of electrocatalytic materials technology. Background Technology

[0002] In the field of industrial hydrogen production, electrocatalytic water splitting is considered a green chemistry-compliant technology due to its absence of harmful byproducts. However, the inherently slow reaction kinetics of the hydrogen evolution reaction (HER) and oxygen evolution reaction (OER) severely limit the overall energy conversion efficiency of water electrolysis. While noble metal Pt and Ru / Ir-based oxides are benchmark electrocatalysts for HER and OER, their high cost and resource scarcity greatly limit their large-scale industrial application. OER, in particular, involves a complex four-electron transfer process, and the strong oxidizing environment at the anolyte causes severe corrosion to the electrode materials, making it more challenging than HER. Therefore, developing water electrolysis catalysts based on non-noble metals that combine high catalytic activity with cost advantages has become an important research direction. Transition metal sulfides and layered double hydroxides have attracted widespread attention due to their unique electronic structures and catalytic properties; however, single-material systems still cannot simultaneously meet the different optimization requirements of HER and OER for the adsorption energy of reaction intermediates, necessitating the achievement of synergistic catalysis through rational composite structure design.

[0003] This invention uses Ni3S2-Co9S8 grown in situ on the surface of nickel foam (NF) as a composite sulfide core, and then constructs a CoFe-LDH shell on it through a short electrodeposition time. Through the synergistic effect of raw materials and preparation process, a bifunctional electrode material with excellent hydrogen evolution reaction and oxygen evolution reaction performance is prepared. Due to the synergistic effect of the core and shell structure, the electrode material prepared by this invention has both excellent conductivity and abundant active sites, and good stability. Summary of the Invention

[0004] To address the shortcomings of related technologies, this invention provides a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis and its preparation method. The prepared bifunctional electrode has excellent conductivity and abundant active sites, which can simultaneously improve the activity of hydrogen evolution and oxygen evolution reactions. This solves the problem that single material systems still cannot simultaneously meet the different optimization requirements of HER and OER for the adsorption energy of reaction intermediates.

[0005] One objective of this invention is to provide a method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis, specifically including the following steps: (1) The surface of the nickel foam is cleaned and then dried to obtain the pretreated nickel foam.

[0006] (2) Prepare a mixed aqueous solution of nickel salt, cobalt salt and urea, then add the pretreated foamed nickel to the mixed aqueous solution of nickel salt, cobalt salt and urea, heat the reaction, and then cool to obtain the reaction product. Wash and dry the reaction product to obtain the precursor (i.e. NiCo-pre / NF).

[0007] (3) The precursor was immersed in a sulfur source solution, then heated to react, and then cooled to obtain a crude product. The crude product was washed and dried to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray.

[0008] (4) A three-electrode system was adopted, with a nickel foam-loaded Ni3S2-Co9S8 nanoarray as the working electrode, a saturated calomel electrode as the reference electrode, and a platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt salt and ferrous salt to obtain a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis.

[0009] More preferably, the method of cleaning the surface of the nickel foam in step (1) is as follows: the nickel foam is ultrasonically cleaned in acetone for 10 min, then immersed in 1 mol / L hydrochloric acid solution for ultrasonic treatment for 20 min, and then ultrasonically cleaned in deionized water and anhydrous ethanol for 10 min respectively; the drying conditions are: drying at 60℃ for 12 h.

[0010] Preferably, in step (2), the nickel salt in the mixed aqueous solution of nickel salt, cobalt salt and urea is nickel chloride hexahydrate, and the cobalt salt is cobalt chloride hexahydrate; the concentration of nickel chloride hexahydrate in the mixed aqueous solution of nickel salt, cobalt salt and urea is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L, and the concentration of urea is 0.286 mol / L.

[0011] Preferably, the amount of foamed nickel pretreated in step (2) added to the mixed aqueous solution of nickel salt, cobalt salt and urea is 1~10 g / L.

[0012] More preferably, the amount of foamed nickel pretreated in step (2) added to the mixed aqueous solution of nickel salt, cobalt salt and urea is 6 g / L.

[0013] Preferably, the heating reaction conditions in step (2) are: reacting at 120°C for 6 hours.

[0014] More preferably, the cooling conditions in step (2) are: natural cooling; the rinsing conditions are: rinsing three times with anhydrous ethanol and deionized water in sequence; and the drying conditions are: drying at 60°C for 12 hours.

[0015] Preferably, the sulfur source solution in step (3) is a 0.05~0.1 mol / L Na2S aqueous solution.

[0016] More preferably, the sulfur source solution in step (3) is a 0.05 mol / L Na2S aqueous solution.

[0017] Preferably, the heating reaction conditions in step (3) are: reacting at 120°C for 10 hours.

[0018] More preferably, the cooling conditions in step (3) are: natural cooling; the washing conditions are: washing with deionized water 3 times; and the drying conditions are: drying at 60°C for 12 hours.

[0019] Preferably, in step (4), the cobalt salt is cobalt nitrate hexahydrate and the ferrous salt is ferrous sulfate heptahydrate; the concentrations of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte are both 0.15 mol / L.

[0020] Preferably, the deposition voltage of the electrodeposition in step (4) is -1.0V and the deposition time is 10~60s.

[0021] More preferably, the solvent for the electrolyte in step (4) is deionized water.

[0022] The second objective of this invention is to provide a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis.

[0023] Mechanism of the invention: This invention uses Ni3S2-Co9S8 as a composite sulfide core, which is grown directly in situ on the surface of nickel foam. A thin LDH shell (CoFe-LDH) is then grown on the surface of the sulfide core via electrodeposition. The synergistic combination of raw materials and processes enables the preparation of bifunctional electrode materials within a short deposition time (10-60 s), exhibiting excellent hydrogen evolution reaction and oxygen evolution reaction performance. While maintaining the high conductivity and three-dimensional open structure of the sulfide framework, the growth thickness of the LDH shell and the interface coupling state are achieved. The electrode material preparation process of this invention requires no binder, and the electrode has a self-supporting integrated structure. Due to the synergistic effect of the core and shell structures, the electrode material prepared by this invention possesses both excellent conductivity and abundant active sites. The active material is firmly bonded to the conductive substrate, which improves the stability of the electrode material under high current.

[0024] The beneficial effects of this invention are: (1) The present invention uses Ni3S2-Co9S8 composite sulfide grown in situ on a nickel foam substrate as a conductive core to construct a three-dimensional ordered nanoneedle array framework, which provides a fast channel for electron transport, effectively reduces the charge transfer resistance in the HER and OER processes, and significantly reduces the overpotential of the catalytic reaction.

[0025] (2) The Mott-Schottky heterojunction formed at the interface of the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode prepared in this invention modulates the electronic structure of the interface through the built-in electric field, further optimizes the adsorption free energy of the reaction intermediate, and enhances the intrinsic catalytic activity.

[0026] (3) The present invention uses a two-step hydrothermal method combined with electrodeposition process to prepare electrodes. The operation process is simple, the raw material cost is low, and it has broad application prospects.

[0027] (4) The CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode prepared by the present invention has excellent hydrogen evolution reaction and oxygen evolution reaction performance. Attached Figure Description

[0028] Figure 1 The image shows a scanning electron microscope (SEM) image of the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode prepared in Example 1 of this invention.

[0029] Figure 2 The images shown are transmission electron microscopy (TEM) images and EDS elemental energy dispersive spectroscopy (EDS) images of the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode prepared in Example 1 of this invention. Figure 2 (a) is a TEM image. Figure 2 (b) is the elemental energy spectrum of EDS.

[0030] Figure 3 The XRD diffraction patterns are of the electrodes prepared in Example 1 and Comparative Example 1 of this invention.

[0031] Figure 4 The OER current density-voltage curves of the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrodes prepared in Examples 1-4 of this invention were obtained in an electrolyte of 1 mol / L KOH at a scan rate of 5 mV / s.

[0032] Figure 5 The HER current density-voltage curves of the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrodes prepared in Examples 1-4 of this invention were obtained in an electrolyte of 1 mol / L KOH at a scan rate of 5 mV / s.

[0033] Figure 6 The OER current density-voltage curves of the bifunctional electrodes prepared in Example 1 and Comparative Examples 1-3 of this invention were obtained in an electrolyte of 1 mol / L KOH at a scan rate of 5 mV / s.

[0034] Figure 7The HER current density-voltage curves of the bifunctional electrodes prepared in Example 1 and Comparative Examples 1-3 of this invention were obtained in an electrolyte of 1 mol / L KOH at a scan rate of 5 mV / s. Detailed Implementation

[0035] To better illustrate the purpose, technical solution, and advantages of this invention, the invention will be further described below with reference to specific embodiments. In the embodiments and comparative examples of this invention, unless otherwise specified, all chemical reagents used were commercially available analytical grade reagents.

[0036] Example 1 A method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min respectively, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0037] (2) Prepare a mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea. The concentration of nickel chloride hexahydrate in the mixed aqueous solution is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L and the concentration of urea is 0.286 mol / L. Then add the pretreated foamed nickel to the mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea (the amount of pretreated foamed nickel added to the mixed aqueous solution is 6 g / L). Heat the reaction at 120°C for 6 h and then cool it naturally to room temperature to obtain a solid reaction product. Wash the solid reaction product three times with anhydrous ethanol and deionized water in sequence, and dry it in a vacuum drying oven at 60°C for 12 h to obtain the precursor (i.e. NiCo-pre / NF).

[0038] (3) The precursor was immersed in a 0.05 mol / L Na2S aqueous solution, then heated at 120℃ for 10 h, and then cooled naturally to obtain a solid crude product. The solid crude product was washed three times with deionized water and then vacuum dried at 60℃ for 12 h in a vacuum drying oven to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray.

[0039] (4) A three-electrode system was adopted, with the Ni3S2-Co9S8 nanoarray supported on nickel foam as the working electrode, the saturated calomel electrode as the reference electrode, and the platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate (the concentration of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte was 0.15 mol / L, and the electrolyte solvent was deionized water). The deposition voltage was -1.0 V and the deposition time was 20 s, thus obtaining a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis.

[0040] The electrodes obtained in this embodiment were characterized by SEM, TEM, and XRD; such as Figure 1 As shown, SEM results reveal that the product exhibits a rod-like structure encapsulated in nanosheets; TEM results are as follows. Figure 2 As shown in (a), the rod-like structure encapsulated in nanosheets is further confirmed. Figure 2 (b) confirms that Fe, Ni, Co, and S elements are uniformly distributed in the sample; XRD results are as follows. Figure 3 As shown, the electrode prepared in this embodiment exhibits obvious phase characteristic diffraction peaks; as Figure 4 As shown, the electrode obtained in this embodiment achieves 100 mA·cm⁻¹ as an oxygen evolution catalyst. -2 The required overpotential for the current density is 285mV; such as Figure 5 As shown, the electrode obtained in this embodiment achieves a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2 The overpotential required for the current density is 102mV.

[0041] Example 2 A method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min respectively, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0042] (2) Prepare a mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea. The concentration of nickel chloride hexahydrate in the mixed aqueous solution is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L and the concentration of urea is 0.286 mol / L. Then add the pretreated foamed nickel to the mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea (the amount of pretreated foamed nickel added to the mixed aqueous solution is 6 g / L). Heat the reaction at 120°C for 6 h and then cool it naturally to room temperature to obtain a solid reaction product. Wash the solid reaction product three times with anhydrous ethanol and deionized water in sequence, and dry it in a vacuum drying oven at 60°C for 12 h to obtain the precursor (i.e. NiCo-pre / NF).

[0043] (3) The precursor was immersed in a 0.05 mol / L Na2S aqueous solution, then heated at 120℃ for 10 h, and then cooled naturally to obtain a solid crude product. The solid crude product was washed three times with deionized water and then vacuum dried at 60℃ for 12 h in a vacuum drying oven to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray.

[0044] (4) A three-electrode system was adopted, with the nickel foam-supported Ni3S2-Co9S8 nanoarray as the working electrode, the saturated calomel electrode as the reference electrode, and the platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate (the concentration of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte was 0.15 mol / L, and the electrolyte solvent was deionized water). The deposition voltage was -1.0 V and the deposition time was 10 s, resulting in a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis (CoFe-LDH@Ni3S2-Co9S8 / NF-10s).

[0045] The electrode obtained in this embodiment was characterized by XRD and SEM, and its phase and morphology were basically consistent with those of Example 1; Figure 4 As shown, the electrode obtained in this embodiment achieves 100 mA·cm⁻¹ as an oxygen evolution catalyst. -2 The required overpotential for the current density is 290mV; such as Figure 5 As shown, the electrode obtained in this embodiment achieves a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2 The required overpotential for the current density is 113mV.

[0046] Example 3 A method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min respectively, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0047] (2) Prepare a mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea. The concentration of nickel chloride hexahydrate in the mixed aqueous solution is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L and the concentration of urea is 0.286 mol / L. Then add the pretreated foamed nickel to the mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea (the amount of pretreated foamed nickel added to the mixed aqueous solution is 6 g / L). Heat the reaction at 120°C for 6 h and then cool it naturally to room temperature to obtain a solid reaction product. Wash the solid reaction product three times with anhydrous ethanol and deionized water in sequence, and dry it in a vacuum drying oven at 60°C for 12 h to obtain the precursor (i.e. NiCo-pre / NF).

[0048] (3) The precursor was immersed in a 0.05 mol / L Na2S aqueous solution, then heated at 120℃ for 10 h, and then cooled naturally to obtain a solid crude product. The solid crude product was washed three times with deionized water and then vacuum dried at 60℃ for 12 h in a vacuum drying oven to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray.

[0049] (4) A three-electrode system was adopted, with the nickel foam-supported Ni3S2-Co9S8 nanoarray as the working electrode, the saturated calomel electrode as the reference electrode, and the platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate (the concentration of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte was 0.15 mol / L, and the electrolyte solvent was deionized water). The deposition voltage was -1.0 V and the deposition time was 30 s, resulting in a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis (CoFe-LDH@Ni3S2-Co9S8 / NF-30s).

[0050] The electrode obtained in this embodiment was characterized by XRD and SEM, and its phase and morphology were basically consistent with those of Example 1; Figure 4 As shown, the electrode obtained in this embodiment achieves 100 mA·cm⁻¹ as an oxygen evolution catalyst. -2 The required overpotential for the current density is 295mV; such as Figure 5 As shown, the electrode obtained in this embodiment achieves a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2The required overpotential for the current density is 118mV.

[0051] Example 4 A method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min respectively, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0052] (2) Prepare a mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea. The concentration of nickel chloride hexahydrate in the mixed aqueous solution is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L and the concentration of urea is 0.286 mol / L. Then add the pretreated foamed nickel to the mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea (the amount of pretreated foamed nickel added to the mixed aqueous solution is 6 g / L). Heat the reaction at 120°C for 6 h and then cool it naturally to room temperature to obtain a solid reaction product. Wash the solid reaction product three times with anhydrous ethanol and deionized water in sequence, and dry it in a vacuum drying oven at 60°C for 12 h to obtain the precursor (i.e. NiCo-pre / NF).

[0053] (3) The precursor was immersed in a 0.05 mol / L Na2S aqueous solution, then heated at 120℃ for 10 h, and then cooled naturally to obtain a solid crude product. The solid crude product was washed three times with deionized water and then vacuum dried at 60℃ for 12 h in a vacuum drying oven to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray.

[0054] (4) A three-electrode system was adopted, with the nickel foam-supported Ni3S2-Co9S8 nanoarray as the working electrode, the saturated calomel electrode as the reference electrode, and the platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate (the concentration of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte was 0.15 mol / L, and the electrolyte solvent was deionized water). The deposition voltage was -1.0 V and the deposition time was 60 s, resulting in a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis (CoFe-LDH@Ni3S2-Co9S8 / NF-60s).

[0055] The electrode obtained in this embodiment was characterized by XRD and SEM, and its phase and morphology were basically consistent with those of Example 1; Figure 4As shown, the electrode obtained in this embodiment achieves 100 mA·cm⁻¹ as an oxygen evolution catalyst. -2 The required overpotential for the current density is 296mV; such as Figure 5 As shown, the electrode obtained in this embodiment achieves a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2 The required overpotential for the current density is 121mV.

[0056] Comparative Example 1 A method for preparing a Ni3S2-Co9S8 / NF electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min respectively, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0057] (2) Prepare a mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea. The concentration of nickel chloride hexahydrate in the mixed aqueous solution is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L and the concentration of urea is 0.286 mol / L. Then add the pretreated foamed nickel to the mixed aqueous solution of nickel chloride hexahydrate, cobalt chloride hexahydrate and urea (the amount of pretreated foamed nickel added to the mixed aqueous solution is 6 g / L). Heat the reaction at 120°C for 6 h and then cool it naturally to room temperature to obtain a solid reaction product. Wash the solid reaction product three times with anhydrous ethanol and deionized water in sequence, and dry it in a vacuum drying oven at 60°C for 12 h to obtain the precursor (i.e. NiCo-pre / NF).

[0058] (3) The precursor was immersed in a 0.05 mol / L Na2S aqueous solution, then heated at 120℃ for 10 h, and then cooled naturally to obtain a solid crude product. The solid crude product was washed three times with deionized water and then vacuum dried at 60℃ for 12 h in a vacuum drying oven to obtain a Ni3S2-Co9S8 / NF electrode for water electrolysis.

[0059] The electrode obtained in this comparative example was characterized by XRD and SEM. The XRD results showed obvious diffraction peaks characteristic of the Ni3S2 and Co9S8 phases. (See [link to relevant documentation]). Figure 3 SEM results showed that the electrode had a rod-like structure; such as Figure 6 As shown, the electrode obtained in this comparative example achieved an oxygen evolution catalyst strength of 100 mA·cm⁻¹. -2 The required overpotential for the current density is 305mV; such as Figure 7 As shown, the electrode obtained in this comparative example achieved a hydrogen evolution catalyst strength of 10 mA·cm⁻¹.-2 The required overpotential for the current density is 150mV.

[0060] Comparative Example 2 A method for preparing a CoFe-LDH / NF electrode for water electrolysis specifically includes the following steps: (1) The foam nickel with a size of about 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10min to remove surface oil stains, and then immersed in 1mol / L hydrochloric acid solution for ultrasonic treatment for 20min to remove surface oxide layer. After taking it out, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10min in sequence, and then dried at 60℃ for 12h to obtain pretreated foam nickel.

[0061] (2) A three-electrode system was adopted, with nickel foam as the working electrode, saturated calomel electrode as the reference electrode, and platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate (the concentration of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte was 0.15 mol / L, and the electrolyte solvent was deionized water). The deposition voltage was -1.0 V and the deposition time was 20 s, thus obtaining a CoFe-LDH / NF electrode for water electrolysis.

[0062] The product obtained in this comparative example was characterized by XRD and SEM. XRD results showed obvious CoFe-LDH phase characteristic diffraction peaks, while SEM results showed that the product exhibited a nanosheet structure. Figure 6 As shown, the electrode obtained in this comparative example achieved an oxygen evolution catalyst strength of 100 mA·cm⁻¹. -2 The required overpotential for the current density is 299mV; such as Figure 7 As shown, the electrode obtained in this comparative example achieved a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2 The required overpotential for the current density is 248mV.

[0063] Comparative Example 3 A method for preparing an NF electrode for water electrolysis specifically includes the following steps: Nickel foam with dimensions of approximately 2cm×3cm×2mm was ultrasonically cleaned in acetone for 10 minutes to remove surface oil, then immersed in 1mol / L hydrochloric acid solution and ultrasonically treated for 20 minutes to remove the surface oxide layer. After removal, it was ultrasonically cleaned in deionized water and anhydrous ethanol for 10 minutes in sequence, and then dried at 60℃ for 12 hours to obtain the NF electrode.

[0064] The electrode obtained in this comparative example was characterized by XRD and SEM. The XRD results showed obvious NF phase characteristic diffraction peaks, and the SEM revealed a typical three-dimensional network structure. Figure 6 As shown, the electrode obtained in this comparative example achieved an oxygen evolution catalyst strength of 100 mA·cm⁻¹.-2 The required overpotential for the current density is 452mV; such as Figure 7 As shown, the electrode obtained in this comparative example achieved a hydrogen evolution catalyst strength of 10 mA·cm⁻¹. -2 The required overpotential for the current density is 251mV.

[0065] This invention utilizes a synergistic approach in preparing raw materials and processes, employing Ni3S2-Co9S8 as a composite sulfide core. This composite sulfide core is grown directly in situ on the surface of nickel foam. Subsequently, a thin LDH shell is grown on the surface of the sulfide core via electrodeposition, constructing a three-dimensional ordered nanoneedle array framework. This provides a rapid channel for electron transport, effectively reducing charge transfer resistance in the HER and OER processes and significantly decreasing the overpotential of the catalytic reaction. The resulting electrode material exhibits excellent oxygen evolution and hydrogen evolution performance. In contrast, the electrode material prepared in Comparative Example 1 lacks the CoFe-LDH shell, retaining only the composite sulfide core, resulting in lower activity. Insufficient sites prevent simultaneous optimization of the adsorption energies for H and OH, resulting in suboptimal HER and OER kinetics. Comparative Example 2 directly electrodeposited CoFe-LDH on NF without pre-growing a Ni3S2-Co9S8 conductive framework, lacking a highly conductive core. The LDH shell could not play a synergistic role, charge transfer was limited, and the overall electrode conductivity and intrinsic HER activity were severely insufficient. Comparative Example 3 prepared unloaded nickel foam. Although nickel foam has some conductivity, its surface has only a small amount of natural oxide layer, very few active sites, and extremely mismatched adsorption energies for H and OH, thus possessing almost no practical electrocatalytic activity.

[0066] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or improvement of the technology in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis, characterized in that, Specifically, the following steps are included: (1) The nickel foam is surface cleaned and then dried to obtain pretreated nickel foam; (2) Prepare a mixed aqueous solution of nickel salt, cobalt salt and urea, then add the pretreated foamed nickel to the mixed aqueous solution of nickel salt, cobalt salt and urea, heat the reaction, and then cool to obtain the reaction product. Wash and dry the reaction product to obtain the precursor. (3) The precursor was immersed in a sulfur source solution, then heated to react, and then cooled to obtain a crude product. The crude product was washed and dried to obtain a nickel foam-supported Ni3S2-Co9S8 nanoarray. (4) A three-electrode system was adopted, with a nickel foam-loaded Ni3S2-Co9S8 nanoarray as the working electrode, a saturated calomel electrode as the reference electrode, and a platinum sheet as the counter electrode. Electrodeposition was carried out in an electrolyte composed of cobalt salt and ferrous salt to obtain a CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis.

2. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, In step (2), the mixed aqueous solution of nickel salt, cobalt salt and urea contains nickel chloride hexahydrate as nickel salt and cobalt chloride hexahydrate as cobalt chloride hexahydrate. The concentration of nickel chloride hexahydrate in the mixed aqueous solution of nickel salt, cobalt salt and urea is 0.05 mol / L, the concentration of cobalt chloride hexahydrate is 0.1 mol / L, and the concentration of urea is 0.286 mol / L.

3. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, The amount of foamed nickel pretreated in step (2) added to the mixed aqueous solution of nickel salt, cobalt salt and urea is 1~10 g / L.

4. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, The heating reaction conditions in step (2) are: reacting at 120℃ for 6 hours.

5. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, The sulfur source solution in step (3) is a Na2S aqueous solution with a concentration of 0.05~0.1 mol / L.

6. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, The heating reaction conditions in step (3) are: reacting at 120℃ for 10 hours.

7. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, In step (4), the cobalt salt is cobalt nitrate hexahydrate and the ferrous salt is ferrous sulfate heptahydrate; the concentrations of cobalt nitrate hexahydrate and ferrous sulfate heptahydrate in the electrolyte are both 0.15 mol / L.

8. The method for preparing the CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis according to claim 1, characterized in that, The deposition voltage for electrodeposition in step (4) is -1.0V, and the deposition time is 10~60s.

9. A CoFe-LDH@Ni3S2-Co9S8 / NF bifunctional electrode for water electrolysis prepared by the method according to any one of claims 1 to 8.