A self-supporting nickel-based oxygen evolution anode and a preparation method thereof
By sandblasting and chemically treating the nickel mesh, more active sites are exposed, which solves the problem of insufficient catalytic activity and structural stability of nickel mesh in the existing technology, and achieves efficient and stable hydrogen production performance through water electrolysis.
Patent Information
- Application Number
- CN202611546055.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-24
AI Technical Summary
Existing OER catalysts are structurally unstable at high current densities, and the introduction of binders leads to electron transport obstruction and active site coverage, making it difficult to meet the requirements for efficient water electrolysis to produce hydrogen.
By sandblasting and chemical treatment of the nickel mesh, including immersion in an acidic mixed solution and a metal salt solution, followed by annealing under an argon atmosphere, more active sites are exposed, thereby improving catalytic activity and structural stability.
It achieves excellent catalytic activity and good durability at high current density, with a current density of 4000 A/m² at a voltage of only 1.59 V. Its performance decreases slightly after 150 h of aging operation, making it suitable for industrial water electrolysis to produce hydrogen.
Smart Images

Figure CN123153085A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic electrode technology for hydrogen production through water electrolysis, specifically to a self-supporting nickel-based oxygen evolution anode and its preparation method. Background Technology
[0002] Electrolysis of water to produce hydrogen is currently a key technological pathway for building a future renewable energy system, and the resulting "green hydrogen" is considered an important energy carrier for achieving deep decarbonization goals. The water electrolysis process involves two half-reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. The OER, involving a four-electron-proton coupling transfer process, exhibits extremely slow reaction kinetics and is the bottleneck determining the overall water electrolysis efficiency, typically requiring a high overpotential to drive the reaction. While noble metal-based catalysts (such as Pt, Ir, Ru, and their oxides) exhibit excellent OER catalytic activity, their high cost and extremely low abundance in the Earth's crust severely limit their practical application in large-scale electrolyzer devices. Therefore, academia and industry have widely shifted their research focus to transition metal-based catalysts (such as Ni, Co, Fe, Mn, and Cu). These materials, with their advantages of low cost, abundant resources, variable valence states, and tunable electronic structures, are considered ideal candidate systems to replace noble metal catalysts.
[0003] Currently, most OER catalysts are synthesized in powder form and then coated onto the surface of current collectors such as glassy carbon electrodes, carbon cloth, or nickel foam using polymer binders such as Nafion and PTFE to form the working electrode. However, the introduction of binders inevitably brings two drawbacks: firstly, the insulating binder layer hinders direct electron transport between the catalyst and the current collector, increasing the interfacial contact resistance; secondly, the binder covers some of the catalyst's active sites, leading to a decrease in the utilization efficiency per unit mass of catalyst and sacrificing intrinsic catalytic activity. More importantly, at high current densities (>250 mA·cm⁻¹), -2 Under industrial-grade water electrolysis conditions, the oxygen evolution reaction on the electrode surface is intense. The rapid nucleation, growth, and detachment of bubbles exert strong mechanical erosion and stripping effects on the catalyst layer, seriously threatening the structural integrity and long-term operational stability of the electrode. Therefore, developing catalytic electrode materials with both high intrinsic activity and excellent structural stability to meet the practical needs of high current density water electrolysis has become a core issue that urgently needs to be addressed in current research.
[0004] In terms of commercial substrates, nickel mesh, nickel felt, and nickel foam are relatively mature products. Among them, pure nickel mesh is widely used as an anode substrate material due to its relatively low price, adjustable width, ability to meet the size requirements of large alkaline water electrolyzers, and wide range of mesh count and thickness options. However, the OER catalytic activity of unactivated bare nickel mesh is extremely limited, far from meeting the requirements of high-efficiency electrolysis for anode overpotential and durability. Therefore, its catalytic performance needs to be improved through reasonable surface engineering and structural design. Summary of the Invention
[0005] This invention provides a self-supporting nickel-based oxygen evolution anode and its preparation method, aiming to overcome at least some of the defects existing in the prior art and to achieve the large-scale preparation of a highly active and highly stable self-supporting oxygen evolution electrode.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a self-supporting nickel-based oxygen-evolving anode and its preparation method, comprising the following steps:
[0007] (1) The nickel mesh is sandblasted and then cut into small pieces to serve as electrode substrates;
[0008] (2) Immerse the nickel mesh treated in step (1) in an acidic mixed solution, wherein the acidic mixed solution contains two or three of sulfuric acid, nitric acid, hydrochloric acid and acetic acid;
[0009] (3) The nickel mesh treated in step (2) is ultrasonically cleaned in water and then dried;
[0010] (4) Immerse the dried nickel mesh in a metal salt mixture solution containing three of the following: nickel salt, iron salt, cobalt salt, sodium hypochlorite, and sodium permanganate; then remove the nickel mesh, rinse it with water, and dry it.
[0011] (5) Anneal the nickel mesh after step (4) in an argon atmosphere at a temperature of 250-550℃ for 2-10h.
[0012] In a preferred embodiment of the present invention, in step (1), the nickel mesh is cut into square pieces of 5cm×5cm.
[0013] In a preferred embodiment of the present invention, in step (2), the concentration of the mixed solution containing two or three of sulfuric acid, nitric acid, hydrochloric acid and acetic acid is 0.01-1M; the nickel mesh is immersed in the above solution for 5-20 minutes.
[0014] In a preferred embodiment of the present invention, in step (4), the concentration of the mixed solution containing nickel salt, iron salt, cobalt salt, sodium hypochlorite and sodium permanganate is 0.01-0.1M; the nickel mesh is immersed in the above solution for 0.6-16h.
[0015] In a preferred embodiment of the present invention, in step (5), the annealing temperature is 250-550°C and the annealing time is 2-10h.
[0016] The beneficial effects of this invention are:
[0017] A chemical treatment method can be used to increase the catalytic activity of nickel mesh and expose more active sites. This chemical treatment method is simple, low-cost, and easily scalable. The resulting nickel mesh, used as an anode electrocatalyst for alkaline water electrolysis, exhibits excellent activity and good durability at high current densities. It can achieve a current density of 4000 A / m² at only 1.59 V, and after 150 hours of continuous aging operation at 4000 A / m², its performance shows minimal degradation, demonstrating promising application prospects in industrial water electrolysis for hydrogen production. Attached Figure Description
[0018] Figure 1 This is a 5500x electron microscope image of the nickel mesh surface after sandblasting in this invention;
[0019] Figure 2 This is a 5500x electron microscope image of the nickel mesh surface after chemical treatment in this invention;
[0020] Figure 3 This is a 5500x imaging electron microscope image of the nickel mesh surface after chemical treatment and annealing in this invention;
[0021] Figure 4 This is a performance diagram of the chemically treated electrode in the experimental examples of this invention application;
[0022] Figure 5 The graphs show the electrode performance at different times during chemical treatment in Experimental Example 3 of this application.
[0023] Figure 6 This is a durability test diagram for embodiment 150h@4000A / m² of the present invention. Detailed Implementation
[0024] In the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," "front end," "rear end," "head," "tail," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the invention. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0025] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0026] Example 1: A self-supporting nickel-based oxygen evolution anode and its preparation method are as follows:
[0027] (1) Nickel mesh pretreatment: The 40-mesh plain weave nickel mesh is sandblasted and then cut to form 5cm×5cm nickel mesh pieces, which are used as electrode substrates;
[0028] (2) Transfer the nickel mesh treated in step (1) to a mixed aqueous solution containing 0.01M sulfuric acid and 1M acetic acid and soak for 15 minutes;
[0029] (3) The nickel mesh treated in step (2) is ultrasonically cleaned in water for 20 minutes, and then dried in a vacuum drying oven at 60°C for 5 hours;
[0030] (4) After drying in step (3), the nickel mesh is transferred to a mixed solution containing 0.02M ferric sulfate, 0.01M cobalt nitrate and 0.1M sodium hypochlorite and soaked at room temperature of 25°C for 16 hours; then the nickel mesh is taken out and rinsed with water 3-5 times, and finally dried in a vacuum drying oven at 60°C overnight.
[0031] Example 2: A self-supporting nickel-based oxygen evolution anode and its preparation method are as follows:
[0032] (1) Nickel mesh pretreatment: The 40-mesh plain weave nickel mesh is sandblasted and then cut to form 5cm×5cm nickel mesh pieces, which are used as electrode substrates;
[0033] (2) Transfer the nickel mesh treated in step (1) to a mixed aqueous solution containing 0.01M sulfuric acid and 1M acetic acid and soak for 15 minutes;
[0034] (3) The nickel mesh treated in step (2) is ultrasonically cleaned in water for 20 minutes, and then dried in a vacuum drying oven at 60°C for 5 hours;
[0035] (4) After drying in step (3), the nickel mesh is transferred to a mixed solution containing 0.02M ferric sulfate, 0.01M cobalt nitrate and 0.1M sodium hypochlorite and soaked at room temperature of 25°C for 16 hours; then the nickel mesh is taken out and rinsed with water 3-5 times, and finally dried in a vacuum drying oven at 60°C overnight.
[0036] (5) The nickel mesh processed in step (4) is transferred to a heat treatment furnace and annealed at 400°C for 2 hours under an argon atmosphere.
[0037] Example 3: A self-supporting nickel-based oxygen evolution anode and its preparation method are as follows:
[0038] (1) Nickel mesh pretreatment: The 40-mesh plain weave nickel mesh is sandblasted and then cut to form 5cm×5cm nickel mesh pieces, which are used as electrode substrates;
[0039] (2) Transfer the nickel mesh treated in step (1) to a mixed aqueous solution containing 0.01M sulfuric acid and 1M acetic acid and soak for 15 minutes;
[0040] (3) The nickel mesh treated in step (2) is ultrasonically cleaned in water for 20 minutes, and then dried in a vacuum drying oven at 60°C for 5 hours;
[0041] (4) After drying in step (3), the nickel mesh pieces are transferred to a mixed solution containing 0.02M ferric sulfate, 0.01M cobalt nitrate and 0.1M sodium hypochlorite and soaked at room temperature of 25℃ for 2h, 5h and 8h respectively; then the nickel mesh is taken out and rinsed with water 3-5 times, and finally dried in a vacuum drying oven at 60℃ overnight.
[0042] like Figure 1 As shown, the surface of the nickel mesh becomes roughened after sandblasting, significantly increasing its specific surface area. From... Figure 2 As shown, the surface of the chemically treated nickel mesh is encapsulated by micro- and nano-structures, which expose more active sites. From Figure 3 As shown, the surface of the nickel mesh after chemical treatment and annealing retains the same morphology as the nickel mesh after chemical treatment.
[0043] like Figure 4 The LSV polarization curves of the chemically treated electrode are shown in the figure. The LSV curves primarily characterize the polarization of the catalyst. For the anode catalyst, the lower the degree of polarization, the smaller the overpotential at the same current density, resulting in less energy loss and better water electrolysis performance. Compared to the initially untreated nickel mesh, in Example 1, the anodic oxygen evolution performance of the nickel mesh electrode in an alkaline environment was effectively improved after chemical treatment. In Example 2, the anodic oxygen evolution performance of the nickel mesh electrode in an alkaline environment was further improved after chemical treatment and annealing.
[0044] And from Figure 5 As can be seen from the above, the anode performance of the nickel mesh electrode was greatly improved in Example 3 after the chemical treatment time was extended.
[0045] exist Figure 6In durability tests, chemically treated nickel mesh exhibited lower voltage and better durability compared to untreated nickel mesh. Furthermore, the voltage of chemically treated-annealed nickel mesh decreased further compared to chemically treated nickel mesh; this is related to… Figure 4 The polarization results also correspond.
[0046] The beneficial effects of this invention are: by treating nickel mesh with a chemical method, the catalytic activity of the nickel mesh can be increased, exposing more active sites. The corresponding chemical treatment method is simple to operate, low in cost, and easy to scale up. When the resulting nickel mesh is used as an anode electrocatalyst for alkaline water electrolysis, it exhibits excellent activity and good durability at high current densities. It can achieve a current density of 4000 A / m² at a voltage of only 1.59 V, and after 150 hours of continuous aging operation at a current density of 4000 A / m², its performance shows only slight degradation, demonstrating promising application prospects in industrial water electrolysis for hydrogen production.
[0047] It is understood that the above embodiments are merely exemplary implementations used to illustrate the principles of the present invention, and the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a self-supporting nickel-based oxygen evolution anode, characterized in that, Includes the following steps: (1) The nickel mesh is sandblasted and then cut into small pieces to serve as electrode substrates; (2) Immerse the nickel mesh treated in step (1) in an acidic mixed solution containing two or three of sulfuric acid, nitric acid, hydrochloric acid and acetic acid; (3) The nickel mesh treated in step (2) is ultrasonically cleaned in water and then dried; (4) Immerse the dried nickel mesh in a metal salt mixture solution containing three of the following: nickel salt, iron salt, cobalt salt, sodium hypochlorite, and sodium permanganate; then remove the nickel mesh, rinse it with water, and dry it. (5) Anneal the nickel mesh after step (4) in an argon atmosphere at a temperature of 250-550℃ for 2-10h.
2. The method for preparing a self-supporting nickel-based oxygen-evolving anode according to claim 1, characterized in that, In step (1), the nickel mesh is cut into square pieces of 5cm×5cm.
3. The method for preparing a self-supporting nickel-based oxygen-evolving anode according to claim 1, characterized in that, In step (2), the concentration of the acidic mixed solution is 0.01-1M; the soaking time is 5-20min.
4. The method for preparing a self-supporting nickel-based oxygen-evolving anode according to claim 1, characterized in that, In step (4), the concentration of the metal salt mixed solution is 0.01-0.1M; the soaking time is 0.6-16h.
5. The method for preparing a self-supporting nickel-based oxygen-evolving anode according to claim 1, characterized in that, In step (3), the ultrasonic cleaning time is 20 min and the drying is vacuum drying at 60℃ for 5 h; in step (4), the drying is vacuum drying at 60℃ overnight.
6. The method for preparing a self-supporting nickel-based oxygen-evolving anode according to claim 1, characterized in that, In step (5), the annealing temperature is 400℃ and the annealing time is 2h.
7. A self-supporting nickel-based oxygen-evolving anode, characterized in that, It is prepared by the preparation method according to any one of claims 1-6.
8. The self-supporting nickel-based oxygen evolution anode according to claim 7, characterized in that, The oxygen-evolving anode is used as the anode in an alkaline water electrolysis device.