A method for preparing an inverse perovskite transition metal nitride
By preparing anti-perovskite transition metal nitrides on a nickel foam substrate, the problems of high preparation cost and catalyst stability were solved, achieving low-cost, high-activity, and high-stability electrocatalytic effects, which promoted the development of metal-air batteries and alkaline water splitting technology.
Patent Information
- Application Number
- CN202611561697.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-24
AI Technical Summary
Existing preparation methods use expensive precursors, resulting in high costs and hindering large-scale commercial applications. Furthermore, Fe-NC catalysts exhibit rapid aging in proton exchange membrane fuel cells and zinc-air batteries, while Co-NC catalysts suffer from low Fenton reaction activity.
Using nickel foam as a substrate, the electrode is treated with a mixed solution of Co(NO₃)₂·6H₂O, Fe(NO₃)₃·9H₂O and urea, and then heated in an NH₃ atmosphere to form an anti-perovskite transition metal nitride, thus constructing a self-supporting nitride electrode.
This improved the electrocatalytic performance of transition metal nitrides, achieving low cost, high activity, and high stability, and promoted the development of metal-air batteries and alkaline water splitting technology.
Smart Images

Figure CN123153091A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water electrolysis technology, and more specifically to a method for preparing anti-perovskite transition metal nitrides. Background Technology
[0002] Some preparation methods use expensive precursors, such as metal-organic frameworks (MOFs), which are costly and unsuitable for large-scale commercial applications. Fe is abundant in nature, and iron-nitrogen-carbon (Fe-NC) materials have been shown to exhibit excellent oxygen activation capabilities in alkaline electrolytes. However, Fe-NC catalysts often exhibit rapid aging in practical operation, especially in proton exchange membrane fuel cells and zinc-air batteries, because the Fenton reaction activity of Co-NC catalysts is lower than that of Fe-NC materials. Doping Co at the Fe4N active site is expected to further enhance the structural stability of metal nitrides and solve the problems of Fe dissolution and aggregation in Fe-NC materials. It has been reported that the targeted introduction of pyridine nitrogen helps achieve reversibility and 4-electron transfer, with ammonia reduction to generate pyridine nitrogen, Fe / Ni-Nx, pyrrole nitrogen, graphitic nitrogen, and some nitrogen oxides, realizing bifunctional reversibility in zinc-air batteries. However, developing a simple and practical method for preparing metal nitride catalysts remains an unsolved problem. Summary of the Invention
[0003] To address the shortcomings of existing technologies, this invention provides a method for preparing anti-perovskite transition metal nitrides, the technical solution of which is as follows: A method for preparing anti-perovskite transition metal nitrides includes the following steps: S1, Pretreatment of nickel foam; S2. Dissolve Co(NO3)2·6H2O, Fe(NO3)3·9H2O and urea in deionized water to form a mixed solution. After stirring evenly, add nickel foam, heat to react, cool to room temperature, wash and dry to obtain nickel foam loaded with the sample precursor. S3. In an NH3 atmosphere, heat nickel foam loaded with the sample precursor and maintain the temperature to obtain an anti-perovskite transition metal nitride.
[0004] Preferably, the pretreatment of the nickel foam in step S1 is specifically performed as follows: the nickel foam is placed in acetone, 3 MHCl and anhydrous ethanol respectively and ultrasonically cleaned for 20-25 minutes in an ultrasonic cleaner, then washed three times with deionized water and dried in a vacuum drying oven at 70-72°C for 0.5 hours before being taken out.
[0005] Preferably, the molar ratio of Co(NO3)2·6H2O, Fe(NO3)3·9H2O and urea in step S2 is 1:3:14.
[0006] Preferably, the heating reaction in step S2 is carried out in an electrically heated drying oven at 120-125°C for 10 h.
[0007] Preferably, the washing in step S2 specifically involves washing the sample-loaded nickel foam 3-4 times with anhydrous ethanol and deionized water, and drying at a temperature of 60-62°C.
[0008] Preferably, the heating in step S3 is specifically heating to 420°C at a heating rate of 10°C / min and holding at that temperature for 4-4.2 hours.
[0009] Beneficial effects This scheme focuses on a relatively systematic study of transition metal nitride electrocatalytic materials. By constructing self-supporting nitride electrodes, the performance of HER was improved. This research not only enriches the design ideas of transition metal nitrides in the field of multifunctional electrocatalysis, but also provides experimental basis and theoretical reference for the development of low-cost, high-activity, and high-stability non-precious metal electrocatalytic materials. It has certain scientific significance and application value for promoting the development of metal-air batteries and alkaline water splitting technology. Attached Figure Description
[0010] Figure 1 SEM images (a) and (b) of CoNFe3@NC and Fe4N@NC, TEM image (c), HRTEM image (d and e), corresponding SAED pattern (f), and element mapping of CoNFe3@NC. Figure 2 TEM image of CoNFe3@NC after MHNO3 etching; Figure 3 (a) XRD pattern; (b) XRD images of CoNFe3@NC and Fe4N@NC after nitric acid etching; (c) N2 adsorption-desorption isotherm; (d) PSD curve; (e) Raman spectrum; (f) FT-IR spectrum. Figure 4 (a) XPS spectra. (b) XPS c 1s region of CoNFe3@NC and Fe4N@NC, (c) and (d) XPS n1s spectra of CoNFe3@NC and Fe4N@NC; Figure 5 In the figures (a) and (b), Fe4N@NC, Pt / C, and CoNFe3@NC were obtained in 0.1 M KOH at a scan rate of 10 mV / s. -1(c) LSV curve at 1600 rpm, (d) LSV curve of CoNFe3@NC after nitric acid etching, (e) Tafel image of the catalyst, and (j) half-wave potential and dynamic current density of the catalyst at 0.85 V. k (f) In a 0.1 M KOH solution saturated with nitrogen and oxygen, the scan rate is 50 mV s. -1 The CV curves of Fe4N@NC and CoNFe3@NC recorded at the time; Figure 6 (a), (b), and (c) in the figure represent the electrochemical double-layer capacitance (C) of Fe4N@NC and CoNFe3@NC. dl (d) Electrochemical impedance spectroscopy (EIS) of the catalyst recorded at 0.85 V; (e) H2O2 production and number of transferred electrons; (f) Line graphs of CoNFe3@NC and Pt / C after adding 3 mL of methanol at 0.75 V for 300 s. Figure 7 (a) shows the it curves of CoNFe3@NC and Pt / C at 0.8 V; (b) and (c) show the oxygen reduction LSV curves before and after 5000 cycles; (d) and (e) show the oxygen reduction LSV curves of CoNFe3@NC and Pt / C after 5000 cycles (100 mV s) in 0.1 M KOH. −1 CV curves before and after; Figure 8 (a) ORRLSV curves of CoNFe3@NC at 400-2500 rpm under 0.1 mol / L HClO4 conditions, (b) LSV curves of CoNFe3@NC and Pt / C, (c) and (d) LSV curves of CoNFe3@NC and Pt / C before and after 5000 cycles in 0.1 M HClO4; Figure 9 (c) Schematic diagram of the water-bearing ZAB assembled in this work; (d) Polarization and power density curves; (e) At 10 mA cm⁻¹ −2 The specific capacitance is (f) the open-circuit voltage of CoNFe3@NC water-based ZAB using a multimeter; Figure 10 (a) Photograph of an LED powered by a CoNFe3@NC water-based zinc-air battery, (b) Charge-discharge cycle stability of the CoNFe3@NC water-based zinc-air battery (5 mA cm⁻¹). −2 Each cycle consists of 5 minutes of charging and 5 minutes of discharging. Figure 11 (a) Co4N@NC in 0.1 M KOH at a scan rate of 10 mV s -1(a) LSV curves at 400-2500 rpm, (b) Tafel image of the catalyst, (c) scan rate at 50 mV / s in 0.1 M KOH saturated solution of nitrogen and oxygen. -1 (d) CV curve of Co4N@NC recorded at 0.85 V; Electrochemical impedance spectroscopy (EIS) of Co4N@NC recorded at 0.85 V; Figure 12 CoNFe3@NC obtained by air annealing was subjected to a scan at 0.1 M KOH and a scan rate of 10 mV / s. -1 (a) LSV curves at 400-2500 rpm; (b) Tafel image of the catalyst; (c) scan rate of 50 mV / s in 0.1 M KOH saturated solution of nitrogen and oxygen. -1 CV curves of CoNFe3@NC obtained by air annealing. (d) Cyclic voltammetry curves of the catalyst. (e) Electrochemical double-layer capacitance (C0) of CoNFe3@NC obtained by air annealing. dl (f) Electrochemical impedance spectroscopy (EIS) of the catalyst recorded at 0.85 V; Figure 13 SEM images of (a) Fe4N / NF, (b and c) NiFe-MOF@Fe4N / NF, (d) CoNFe3 / NF, and (e and f) NiFe-MOF@CoNFe3 / NF. Figure 14 XRD patterns of NiFe-MOF@Fe4N / NF, Fe4N / NF, NiFe-MOF@CoNFe3 / NF and CoNFe3 / NF on nickel foam, respectively; Figure 15 The results of HER electrocatalysis tests on Fe4N / NF, NiFe-MOF@Fe4N / NF, CoNFe3 / NF, and NiFe-MOF@CoNFe3 / NF in 1 M KOH solution are shown. (a) LSV polarization curve, (b) Tafel slope plot, and (c) results at 10 mA cm⁻¹ -2 Overpotential at 100 mA cm⁻¹, (d) ESI plot, (e) Fe₄N / NF at 100 mA cm⁻¹ -2 Vt plot of continuous operation for 90 hours at current density; Figure 16 In the table, (a), (b), (c), and (d) represent samples of CoNFe3 / NF, Fe4N / NF, NiFe-MOF@CoNFe3 / NF, and NiFe-MOF@Fe4N / NF used to calculate HER C at different scan rates. dl CV curve of the value, (e)Cdl picture. Detailed Implementation
[0011] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0012] Unless otherwise specified, all reagents used in the following schemes are commercially available products.
[0013] Example: A method for preparing anti-perovskite transition metal nitrides (CoNFe3 / NF): S1. Cut out the 3×3cm... 2 The foamed nickel was placed in acetone, 3M HCl and anhydrous ethanol respectively and ultrasonicated in an ultrasonic cleaner for 20 minutes. Then it was washed three times with deionized water and dried in a vacuum drying oven at 70°C for 0.5 hours before being taken out. S2. Dissolve 1 mmol of Co(NO3)2·6H2O, 3 mmol of Fe(NO3)3·9H2O, and 14 mmol of urea in 60 ml of deionized water and stir until homogeneous. Then transfer the mixed solution and the cut nickel foam to a 100 ml reaction vessel lined with polytetrafluoroethylene and react in a 120 °C electric heating drying oven for 10 h. After the reaction time is complete, allow it to cool to room temperature before removing it. Then wash the sample-loaded nickel foam three to four times with anhydrous ethanol and deionized water, and then dry it in a vacuum oven at 60 °C for 0.5 h to obtain nickel foam loaded with the sample precursor. S3. Next, place the dried nickel foam loaded with the sample precursor on a ceramic boat (four pieces at a time) and put it into a tube furnace. Then, continuously circulate ammonia gas into the tube furnace for 0.5 hours. After the tube furnace is filled with ammonia gas, heat it to 420°C at a heating rate of 10°C / min and maintain it for 4 hours under continuous ammonia gas circulation. After the tube furnace cools naturally, the black CoNFe3 / NF sample can be obtained.
[0014] Comparative Example 1: A method for preparing an anti-perovskite transition metal nitride (Fe4N / NF): This comparative example follows the preparation method of Example 1, except that 1 mmol of Co(NO3)2·6H2O and 3 mmol of Fe(NO3)3·9H2O in the raw materials are replaced with 4 mmol of Fe(NO3)3·9H2O, and all other steps are the same.
[0015] Comparative Example 2: A method for preparing anti-perovskite transition metal nitrides (NiFe-MOF@CoNFe3 / NF): 0.192 g of FeCl2·4H2O and 0.16 g of terephthalic acid were dissolved in a mixed solution prepared by 28 mL of DMF, 2 mL of water, and 2 mL of anhydrous ethanol, and stirred at 500 rpm for 1 h at room temperature. The mixed solution and the CoNFe3 / NF sample prepared in the first step were then transferred to a 50 mL reaction vessel and reacted in an electrically heated drying oven at 125 °C for 10 h. After the reaction, the reaction vessel was allowed to cool to room temperature, washed two to three times with ultrapure water and anhydrous ethanol, and finally dried under vacuum to obtain NiFe-MOF@CoNFe3 / NF.
[0016] Comparative Example 3: A method for preparing an anti-perovskite transition metal nitride (NiFe-MOF@Fe4N / NF): The preparation of NiFe-MOF@Fe4N / NF was the same as that of NiFe-MOF@CoNFe3 / NF, using Fe4N / NF as the precursor. Finally, it was cut into 1×3cm pieces. 2 Nickel foam is available for use.
[0017] Detection: 1. CoNFe3@NC was prepared and its ORR performance was tested. Fe4N@NC was also prepared for comparison. Sample preparation: 0.1212 g Fe(NO3)3·9H2O and 2 g soluble starch were added to 45 mL of ultrapure water and heated at 80 °C until completely gelatinized. Then, 1.19 g Zn(NO3)2·6H2O and 4 g dicyandiamide were added to the above solution to form a pale yellow hydrogel. Finally, 0.0291 g Co(NO3)2·6H2O was added and stirred until homogeneous. After cooling to room temperature, the solution was frozen in a freezer for 4 h. The resulting gel-like solid was then freeze-dried at -45 °C for 36 h to prepare an aerogel. Finally, the aerogel was heated in an NH3 atmosphere to 425 °C at a rate of 1 °C / min, then to 600 °C at a rate of 2 °C / min, and finally to 850 °C at a rate of 3 °C / min, and held at these temperatures for 6 h. The resulting sample was recorded as CoNFe3@NC.
[0018] The preparation method of Fe4N@NC is roughly the same as that of CoNFe3@NC, but the amount of Fe(NO3)3·9H2O added is 0.1616g, Co(NO3)2·6H2O cobalt nitrate hexahydrate is not added, and the final temperature is increased to 900℃ and maintained for 4h.
[0019] Following the preparation of the CoNFe3@NC / Fe4N@NC samples, a coating treatment was required: 2 mg (CoNFe3@NC / Fe4N@NC) was dispersed in a mixture of 60 μL ultrapure water, 60 μL ethanol solution, and 6 μL Nafion solution. The mass loading of the prepared transition metal nitride was controlled at 0.8086 mg / cm² in both acidic and alkaline media. 2 Two mg of Pt / C transition metal nitride was dispersed in 100 mL of ultrapure water, 50 mL of ethanol solution, and 10 mL of Nafion solution, with the mass loading controlled at 0.6299 mg / cm³. 2 .
[0020] Preparation of a liquid zinc-air battery: The liquid zinc-air battery used homogeneous nickel foam as the air cathode, 6 M KOH and 0.2 M (CH3COO)2Zn as the electrolyte, and a polished Zn plate as the anode. 2.5 mg of transition metal nitride, 1 mg of acetylene black, and 4 mg of activated carbon were added to a mixed solution containing 30 μL Nafion and 200 μL isopropanol. Subsequently, a homogeneous transition metal nitride ink was drop-coated onto the surface of the nickel foam as the air cathode. The prepared transition metal nitride and 60 wt% Pt / C commercially available transition metal nitride had a mass loading of 2.5 mg cm⁻¹. -2 The polarization curves and performance of the batteries were collected in an air environment using the Xinwei battery testing system. The batteries were tested at 5 mA cm⁻¹. -2 Repeat this cycle every 10 minutes.
[0021] 2. ORR performance test: Experimental instruments and equipment: The microstructure was characterized using scanning electron microscopy (SEM, Quanta 200FEG) and transmission electron microscopy (TEM, JEM-F200(HRP)). The crystal structure was characterized using X-ray diffraction (XRD, Rigaku SmartLab SE powder diffractometer). Raman spectra were collected using a Horiba LabRAM HR Evolution. Nitrogen adsorption / desorption isotherms were analyzed on a Micromeritics ASAP 2460. X-ray photoelectron spectroscopy (XPS) measurements were performed using an Experiment\X-Ray003 400µm-FGON.
[0022] For electrochemical tests, all potentials were converted to reversible hydrogen electrode (RHE) potentials. Except for the hydrogen production rate test, which was conducted using a CHI-760E electrochemical workstation, all other electrochemical tests were performed using a CHI-660E electrochemical workstation. The working electrodes were a rotating disk electrode (RDE) and a rotating ring-disc glassy carbon electrode (RRDE). Hg / HgO (alkaline medium) or saturated calomel electrode (acidic medium) and a graphite rod electrode were used as the reference and counter electrodes, respectively.
[0023] Zinc-air batteries were tested using a Xinwei battery tester.
[0024] Electrochemical performance tests were conducted using a CHI660E workstation (hydrogen production rate was measured using a CHI-760E workstation) in a three-electrode system at ambient temperature and pressure. The deposited film was placed on a rotating disk electrode apparatus and used as the working electrode. The counter electrode and reference electrode were a carbon rod and Hg / HgO, respectively, with 0.1 M KOH solution as the electrolyte. All potentials obtained in the experiment were calculated according to the formula: E(vs.RHE) = E Hg / HgO +0.098 +0.059 pH is converted into a potential relative to the reversible hydrogen electrode (RHE). Before the formal ORR test, nitrogen gas is bubbled into the electrolyte for 0.5 h to activate the transition metal nitride, which is beneficial for subsequent tests. For LSV testing, oxygen needs to be bubbled into the electrolyte for 0.5 h beforehand to purge other gases; this bubbling needs to be continuous during the test. For other tests, nitrogen gas needs to be bubbled into the electrolyte solution for 0.5 h.
[0025] Linear voltammetric scanning (LSV) tests will be performed under the above conditions. Detailed parameters are as follows: a scan rate of 10 mV / s within the range of 0.2 to 1.2 V (vs. RHE) with 90% internal resistance compensation (iR). CV tests will be performed within the range of 0.2–1.2 V (vs. RHE) at a scan rate of 10 mV / s, under both oxygen and nitrogen atmospheres. The Cdl scan rate range is 5–30 mV / s, with a gradient of 5 mV. Electrochemical impedance spectroscopy (EIS) tests will be performed at open-circuit voltage, with a low frequency of 0.1 Hz and a high frequency of 100,000 Hz, and an amplitude of 5 mV. The electrochemical active area (ESCA) will be calculated using the double-layer capacitance (Cdl) using the following formula: ESCA = Cdl / Cs. Where Cs represents a constant, with a value of 38 μF cm⁻¹ in 0.1 M KOH. -2 .
[0026] The stability of transition metal nitrides was evaluated using two methods. First, the transition metal nitrides were subjected to 5000 CV cycles under both acidic and alkaline conditions. The LSV curves before and after the cycles were compared, and the difference between the two curves was observed. A smaller difference indicates better stability of the transition metal nitride. Second, the stability of the transition metal nitrides was evaluated by observing the change in current over time at a certain voltage (0.85 V). In addition, the stability of the transition metal nitrides was also demonstrated by fabricating zinc-air batteries from the samples. Good durability of the zinc-air batteries indicates that the transition metal nitrides can be used for extended periods.
[0027] The morphology of transition metal nitrides was analyzed by SEM and TEM. Figure 1 In images a and 1b, we can see that both Fe4N@NC and CoNFe3@NC surfaces form pores. The difference lies in the more uniform pore distribution on the CoNFe3@NC surface, and the significantly richer pore size compared to the Fe4N@NC surface, indicating that Co plays a crucial role. We hypothesize that CoNFe3@NC has a higher pore surface area, providing more active sites for transition metal nitrides. Through TEM and HRTEM, we observed some nanosites (…). Figure 1 c, 1d, 1e), identified by SAED as CoNFe3 site ( Figure 1 f). Element distribution ( Figure 1 g) indicates that Co, Fe, N, and C are uniformly distributed on the three-dimensional porous carbon framework.
[0028] No CoNFe3 particles were found in the TEM image after acid etching, confirming that the transition metal nitrides had been removed. Finally, ORR testing of the sample showed a significant decrease in the activity of CoNFe3@NC after etching, indicating that CoNFe3 particles play a crucial role in the activity of transition metal nitrides.
[0029] Figure 3 a shows the XRD patterns of CoNFe3@NC and Fe4N@NC. The broad peaks at 25° and 43° are attributed to the typical planes of carbon, respectively. By comparing with the PDF card (PDF#83-0875), we generated CoNFe3@NC and Fe4N@NC, where the (111) and (200) crystal planes are particularly prominent, which is consistent with the results of SAED and HRTEM. Comparison with the XRD patterns after acid etching further highlights that the catalytic effect is due to the formation of transition metal nitride samples. Nitrogen adsorption-desorption isotherms of CoNFe3@NC and Fe4N@NC ( Figure 3c) shows a similar fourth-order curve, indicating the presence of mesopores and micropores. The surface area of CoNFe3@NC (718.57 m²) 2 The surface area ( / g) of Fe4N@NC is much larger than that of Fe4N@NC (489.384 m²). 2 / g). Pore size distribution curve as shown Figure 3 As shown in d, the total pore volumes of CoNFe3@NC and Fe4N@NC are 0.8557 and 0.5464 cm³ / g, respectively, and the main peaks of CoNFe3@NC and Fe4N@NC are below 4 nm. These results indicate that the introduction of Zn can effectively increase the specific surface area and form a layered porous structure. Furthermore, from TEM images (… Figure 1 c) It can be seen that CoNFe3@NC contains a large number of macropores. Therefore, the high surface area and micropore-mesopore-macropore structure of CoNFe3@NC can effectively accelerate the mass / electron transfer during ORR and promote the exposure of active sites in CoNFe3@NC. The Raman spectra of Fe4N@NC and CoNFe3@NC are at 1326 cm⁻¹. -1 and 1583 cm -1 There are two peaks on the left and right ( Figure 3 e). These are respectively assigned to the D band and the G band. We know that Raman spectroscopy can characterize the degree of graphitization of carbon materials. The results show that Fe4N@NC and CoNFe3@NC have I... D / I G The values of 1.29 and 1.15, respectively, further indicate a high degree of graphitization in CoNFe3@NC. To obtain the chemical structure of the transition metal nitride, FT-IR spectra were also measured. Figure 3 f shows that the transition metal nitride formed a CN bond (1351 cm⁻¹). -1 C=N bond (1627 cm) -1 ) and -NH / NH bonds (3438 cm -1 This indicates that N was successfully doped into the carbon matrix, forming CoNFe3@NC and Fe4N@NC.
[0030] To obtain information on the chemical composition, X-ray photoelectron spectroscopy (XPS) measurements were performed on the sample. N, C, O, Fe, and Co elements were detected in CoNFe3@NC. Figure 4 a). Meanwhile, the 1s region of Fe4N@NC and CoNFe3@NC can be fitted with three peaks, corresponding to the C, CN, and CO bonds, respectively. Figure 4 b). The N1s spectrum can be divided into four peaks, corresponding to pyridine N, pyridine N, graphitic N, and partially oxidized N, respectively. Figure 4 c). The content of each of the N types is as follows: Figure 4 As shown in d, CoNFe3@NC has a high content of pyridine N and graphitic N, which, as expected, greatly promotes its ORR activity.
[0031] From the LSV curve ( Figure 5 From a and b), the half-wave potential of CoNFe3@NC is 0.925 V, which is much higher than that of Fe4N@NC (0.845 V), Pt / C (0.866 V), and the recently published Pt-free transition metal nitrides, indicating that CoNFe3@NC has higher ORR performance. Furthermore, the Tafel slope of CoNFe3@NC (60.79 mV dec) is also higher. -1 The value is less than Fe4N@NC (74.01 mV dec). -1 ) and Pt / C (81.44 mV dec -1 This indicates that the ORR kinetics of CoNFe3@NC are better ( Figure 5 d). To further understand the relationship between the structure and activity of transition metal nitrides, we also etched the transition metal nitrides. The transition metal nitrides were placed in 3 M HNO3 and allowed to stand at 80°C for 24 h. Subsequently, XRD analysis of the etched samples revealed that only two diffraction peaks of carbon appeared in the pattern, while no diffraction peaks were observed in other samples. No CoNFe3 particles were found in the TEM images, confirming the previous results that the transition metal nitrides had been removed. Finally, ORR testing of the samples showed a significant decrease in the activity of CoNFe3@NC after etching, indicating that CoNFe3 particles play a crucial role in the activity of transition metal nitrides. Figure 5 Comparison shows that in the presence of transition metal nitrides, superior oxygen reduction performance is observed. However, after acid etching, the transition metal nitrides are washed away, resulting in a significant decrease in oxygen reduction performance, which corresponds perfectly to the appearance observed by TEM and XRD. Figure 5 From e, we can know that the dynamic current density of CoNFe3@NC (j k The value reached 349.216 mA cm⁻¹ -2 It is Fe4N@NC (27.526 mA cm⁻¹) -2 It is 1.8 times that of Pt / C (40.315 mA cm⁻¹) -2 The ORR activity of transition metal nitrides was investigated by CV and LSV tests in 0.1 mol / L KOH solution. Fe4N@NC and CoNFe3@NC showed obvious oxygen reduction peaks in oxygen-saturated solution, while no obvious oxygen reduction peak was observed in nitrogen-saturated solution. Figure 5f). This indicates that Fe4N@NC and CoNFe3@NC possess ORR electrocatalytic activity. Furthermore, the ORR peak potential of CoNFe3@NC (0.863 V) is more accurately corrected than that of Fe4N@NC (0.851 V), suggesting that CoNFe3@NC exhibits superior ORR performance.
[0032] A larger electrochemical double-layer capacitance (Cdl) indicates a larger electrochemical surface area. (From...) Figure 6 From a, 6b, and 6c, we know that the calculated Cdl of CoNFe3@NC is 44.78 mF cm. -2 It is much higher than the 21.51 mF cm⁻¹ of Fe₄N@NC. -2 This further confirms that CoNFe3@NC exhibits excellent mass transport during the ORR process due to its highly porous structure. Electrochemical impedance spectroscopy (EIS) of transition metal nitrides is shown below. Figure 6 As shown in d, the charge transfer resistance (Rct) values of CoNFe3@NC and Fe4N@NC are not significantly different, comparable to those of Pt / C, indicating that the micropore-mesopore-macropore structure can effectively reduce Rct, thereby accelerating the kinetic process on CoNFe3@NC. When the voltage is in the range of 0.536-1.0 V, the yield (0.871-3.467%) and electron transfer number (3.931-3.983) of CoNFe3@NC are superior to those of Pt / C (hydrogen peroxide yield: 3.479-3.936%, n=3.3930-3.936). Figure 6 e). Finally, when 3 ml of 3M methanol was injected into the solution, the Pt / C current suddenly decreased, while the CoNFe3@NC current did not change significantly. Figure 6 f), thus it can be demonstrated that CoNFe3@NC exhibits greater stability and resistance to methanol.
[0033] In addition, Figure 7 As shown in (a), the Pt / C ratio drops rapidly during the It test, with a retention rate of 81.5% after 10,000 seconds. There is an upward phase in the middle, presumably due to oxygen fluctuations during the test. In contrast, CoNFe3@NC exhibits a retention rate as high as 97.6%, far exceeding that of commercially available transition metal nitrides. Furthermore, the ORR durability of CoNFe3@NC was analyzed using CV and LSV. Figure 7In the study, the half-wave potential of CoNFe3@NC shifted backward by only 38 mV after 5000 cycles over a long voltage range, exhibiting higher ORR cycling stability compared to Pt / C. Simultaneously, after 5000 cycles, the oxygen reduction peak potential of CoNFe3@NC retreated by 40 mV under the same conditions, while Pt / C retreated by 82 mV. Furthermore, in 0.1 M perchloric acid, the ORR activity of CoNFe3@NC showed a half-wave potential of 0.694 V (…). Figure 8 The half-wave potentials were almost identical before and after 5000 cycles, while the half-wave potential of Pt / C decreased significantly compared to CoNFe3@NC. ΔE 1 / 2 =41 mV). The results show that CoNFe3@NC exhibits excellent ORR durability in both acidic and alkaline media, which is superior to most platinum-free transition metal nitrides.
[0034] Table 1. Comparison of the performance of this study with recently reported platinum-free transition metal nitrides in alkaline and acidic media. Table 2. Comparison of ORR durability in alkaline and acidic media between this work and recently reported Pt-free transition metal nitrides. The DE value of CoNFe3@NC transition metal nitrides is 0.658 V, which is superior to Pt / C and RuO2 (0.762 V), indicating that CoNFe3@NC transition metal nitrides have stronger bifunctional activity. To explore the application of CoNFe3@NC as a cathode, we assembled a zinc-air battery (ZAB), as follows: Figure 9 As shown in (c), the zinc-air battery based on CoNFe3@NC achieves a peak power density of up to 124.9 mW / cm². -2 Higher than Pt / C (103.5 mW cm⁻¹) -2 ) and many reported transition metal nitrides ( Figure 9 d). At the same time, in Figure 9 In e, the specific capacity of ZABs with CoNFe3@NC as the air cathode is 1475 mA hg. -1 Superior to Pt / C ZAB (1394 mA hg) -1 ZABs based on CoNFe3@NC show open-circuit voltages up to 1.569 V (). Figure 9 f). As expected, one ZAB can drive a standard display and keep it running normally for 6.3 hours without power interruption. Figure 10a). More importantly, long-term charge-discharge cycle stability is a technical hurdle for novel air batteries without platinum transition metal nitrides. The ZAB based on CoNFe3@NC exhibits almost negligible charge-discharge voltage difference after 1419 hours of operation, indicating extremely high charge-discharge cycle stability. Figure 10 b). It has significant advantages over other platinum-free transition metal nitrides.
[0035] Table 3. Performance overview of water-solid two-phase zinc-air batteries based on platinum-free transition metal nitride anodes. Table 4. Summary of the durability of aqueous zinc-air batteries based on platinum-free anode transition metal nitrides Comparison with Co4N catalyst: The preparation process of Co4N@NC is the same as that of CoNFe3@NC, but ferric nitrate nonahydrate was not added. The ORR activity of the transition metal nitrides was studied by performing CV and LSV tests in 0.1 mol / L KOH solution. CoNFe3@NC transition metal nitrides showed a very obvious oxygen reduction peak in oxygen-saturated KOH solution, while Co4N@NC did not. Neither showed a significant peak in nitrogen-saturated solution. Figure 11 c). This indicates that Co4N@NC and CoNFe3@NC possess ORR electrocatalytic activity. Furthermore, the ORR peak potential of CoNFe3@NC (0.863 V) is more positive than that of Co4N@NC (0.812 V), indicating that CoNFe3@NC has higher ORR performance. From the LSV curves ( Figure 11 a) The half-wave potential of CoNFe3@NC is 0.925 V, which is much more positive than that of Co4N@NC (0.821 V), indicating that CoNFe3@NC has higher ORR performance. Furthermore, the Tafel slope of CoNFe3@NC (60.79 mV dec) is... -1 The value is less than Co4N@NC (131.73 mV dec). -1 () Figure 11 b) indicates that CoNFe3@NC exhibits better ORR kinetics. Electrochemical impedance spectroscopy (EIS) of transition metal nitrides is shown in Figure [image / data]. Figure 11 As shown in Figure d, it can be read from the figure that the charge transfer resistance (Rct) of CoNFe3@NC is less than that of Co4N@NC, indicating that CoNFe3@NC has better ORR performance.
[0036] Comparison with CoNFe3@NC catalysts annealed in air: The fabrication process involved placing the aerogel in an air atmosphere, with all other steps identical to those for CoNFe3@NC. The ORR activity of the transition metal nitrides was investigated using CV and LSV tests in 0.1 mol / L KOH solution. In oxygen-saturated KOH solution, CoNFe3@NC exhibited a significant oxygen reduction peak regardless of whether annealed under air or nitrogen. In contrast, no significant peak was observed in nitrogen-saturated solution. Figure 12 c). This indicates that CoNFe3@NC possesses ORR electrocatalytic activity. Furthermore, the ORR peak potential of the CoNFe3@NC transition metal nitride annealed in ammonia (0.863 V) is comparable to that of the transition metal nitride annealed in air (0.867 V).
[0037] The LSV curves show that the half-wave potential of the CoNFe3@NC transition metal nitride annealed in ammonia is 0.925 V, which is significantly higher than that of the transition metal nitride annealed in air (0.885 V). Figure 12 a) This indicates that CoNFe3@NC exhibits higher ORR performance through ammonia annealing. Furthermore, the Tafel slope of CoNFe3@NC annealed in ammonia is 60.79 mV dec. −1 This is significantly less than the 96.67 mV dec obtained by annealing in air. −1 ( Figure 12 b). A larger electrochemical double-layer capacitance (Cdl) indicates a larger electrochemical surface area. As shown in the figure, the calculated Cdl of CoNFe3@NC under ammonia conditions is 44.78 mF cm⁻¹. -2 It is much higher than the 30.72 mF cm⁻¹ in atmospheric environment. -2 ( Figure 12 (d,e) further confirms that CoNFe3@NC has better quality transfer in the ORR process due to the participation of ammonia.
[0038] Electrochemical impedance spectroscopy (EIS) of transition metal nitrides, such as Figure 12 As shown in f, the charge transfer resistance (Rct) values of CoNFe3@NC do not differ significantly under different gas environments, but the data still indicate that the participation of ammonia further reduces Rct during oxygen reduction, thereby accelerating the kinetic process on CoNFe3@NC.
[0039] In summary, the ORR performance of CoNFe3@NC was further improved by the participation of ammonia.
[0040] 2. HRE performance test: The microstructure was characterized using scanning electron microscopy (SEM, Quanta 200FEG). The crystal structure was characterized using X-ray diffraction (XRD, Rigaku SmartLab SE powder diffractometer).
[0041] For electrochemical testing, all potentials were converted to reversible hydrogen electrode (RHE) potentials. All tests were performed using a CHI660E electrochemical station. The working electrode was a self-made nickel foam. Hg / HgO (alkaline medium) and graphite rod electrodes were used as the reference and counter electrodes, respectively.
[0042] First, pre-treat the nickel foam: cut the 3×3 cm pieces... 2 The nickel foam was placed in acetone, 3 M HCl and anhydrous ethanol and ultrasonicated for 20 min in an ultrasonic cleaner. After being cleaned three times with deionized water, it was dried in a vacuum drying oven at 70°C for 0.5 h before being taken out.
[0043] Preparation of standard Pt / C and RuO2 electrodes: 10 mg of standard Pt / C (RuO2) sample powder was added to a mixed solution containing 600 μL of isopropanol and 60 μL of Nafion solution. The mixed solution was then ultrasonically treated for 40 min in an ultrasonic cleaner, resulting in a uniform black ink-like solution. The ultrasonically treated solution was then dropwise added to blank nickel foam, maintaining a drop density of 4 mg / cm³. -2 about.
[0044] All electrochemical performance tests in the experiment were conducted using a three-electrode system on a CHI660E workstation at ambient temperature and pressure. A 1cm × 3cm piece of nickel foam, precisely cut, was immersed in the electrolyte, with its size controlled to 1cm × 1cm, and used as the working electrode. The counter electrode and reference electrode were a carbon rod and a Hg / HgO electrode, respectively, with 1M KOH as the electrolyte. All potentials obtained in the experiment were converted to potentials relative to the reversible hydrogen electrode using the formula: E(vs.RHE) = E + 0.098 + 0.059 × pH.
[0045] Before performing the HER test, nitrogen gas was bubbled into the electrolyte solution for 0.5 h to purge any other air bubbles. Then, the solution was tested at 100 mV s⁻¹. -1 The scanning rates were cyclic voltammetric scans performed within the HER test range of LSV, with 100 scan cycles per cycle, to activate the catalyst on the nickel foam surface.
[0046] Before the linear voltammetric scan (LSV) test, oxygen was bubbled into the solution for 0.5 h to eliminate gas interference. The parameters were: 10 mV / s. -1The scan rate for HER is in the range of 0.1 to -0.4 V (vs. RHE).
[0047] The electrochemical impedance spectroscopy (HER) test voltage is -270 mV, the amplitude is 5 mV, and the frequency range is from 100 Hz to 50000 Hz.
[0048] Electrochemical active area (ESCA) uses double-layer capacitance (C dl ) Perform the calculation, C dl Using different scan rates (5 to 30 mV s) within the non-Radidatic interval -1 ) to perform calculations.
[0049] The stability test of the catalyst is based on the catalyst operating at a certain current density (100 mA cm⁻¹). -2 The stability of a catalyst is evaluated by observing the magnitude of its potential change over time.
[0050] To further investigate the microstructural characteristics of the synthesized catalyst sample, Figure 13 Scanning electron microscopy (SEM) images of four samples are presented. Observation revealed that Fe4N / NF and CoNFe3 / NF adhered to the nickel foam in cluster form, exhibiting a flower-like structure composed of smaller-radius clusters. Figure 13 (a) and (d) are distinctly different from the nanosheet structures of NiFe-MOF@Fe4N / NF and NiFe-MOF@CoNFe3 / NF. Although the structures differ significantly, they are uniformly distributed. Furthermore, these morphological differences will have different effects on the water electrolysis process.
[0051] The XRD patterns of NiFe-MOF@Fe4N / NF, Fe4N / NF, NiFe-MOF@CoNFe3 / NF and CoNFe3 / NF are as follows: Figure 14 As shown, the XRD pattern exhibits only a distribution similar to that of nickel foam, due to the overlap between the generated catalyst and the nickel foam. Furthermore, since 2dsinθ=nλ, we know that as the atomic radius of the crystal increases, the corresponding diffraction peaks will shift to the left. Since the atomic radius of Co is smaller than that of Fe, the pattern of Fe4N / NF should shift to the left compared to CoNFe3 / NF, which corresponds exactly to the generated pattern. Similarly, the MOF structures of NiFe-MOF@Fe4N / NF and NiFe-MOF@CoNFe3 / NF are simply products of FeCl2·4H2O and terephthalic acid at 120℃, and are amorphous; therefore, no new diffraction peaks should appear, consistent with the obtained XRD patterns.
[0052] The electrochemical catalytic activity of the prepared metal nitrides grown on nickel foam and their MOF structures was tested in 1 M KOH solution. The LSV polarization curves of HER are shown below. Figure 15 As shown in (a), at 10 mA cm -2 At different current densities, the overpotentials exhibited by Fe4N / NF, NiFe-MOF@Fe4N / NF, CoNFe3 / NF, NiFe-MOF@CoNFe3 / NF, nickel foam NF, and Pt / C were 162, 209, 173, 230, 215, and 22 mV, respectively. It can be seen that at 10 mA cm⁻¹... -2 At the given current density, Fe4N / NF and CoNFe3 / NF exhibited very similar overpotentials, while NiFe-MOF@Fe4N / NF and NiFe-MOF@CoNFe3 / NF showed very large overpotentials, approaching the catalytic performance of nickel foam alone. This indicates that the MOF structure did not significantly improve the HER performance of the original metal nitride catalysts; in fact, the NiFe-MOF encapsulation led to a significant decrease in the HER electrocatalytic performance of transition metal nitrides, and overall, none of them achieved the performance of commercially available catalysts. Figure 15 As shown in (b), the Tafel slopes of the synthesized catalysts are illustrated. The Tafel slope plot clearly shows a significant deceleration in the HER electrochemical kinetics of all catalysts. The Tafel slope value for Fe4N / NF is 134.45 mV dec. -1 The value is much smaller than that of NiFe-MOF@Fe4N / NF (184.85 mV dec). -1 ), CoNFe3 / NF (183.47 mV dec -1 ), NiFe-MOF@CoNFe3 / NF (187.66mV dec -1 The slope value of Pt / C. The Tafel slope of Pt / C is 23 mV dec. -1 This confirms that the catalytic reaction rate of Pt / C is much higher than that of the synthesized catalyst, and corresponds one-to-one with the LSV images. For example... Figure 15 As shown in (d), the electrochemical impedance spectroscopy (EIS) performance of the samples was tested at an overpotential of -240 mV. It can be seen that the semi-circular radii of the resistance exhibited by the four catalysts—Fe4N / NF, NiFe-MOF@Fe4N / NF, CoNFe3 / NF, and NiFe-MOF@CoNFe3 / NF—are similar, all ranging from 1 to 2 ohms, indicating that the catalysts have relatively low interfacial transfer resistance (Rct). Furthermore, based on the HER test results above, it can be seen that Fe4N / NF exhibits the best HER catalytic performance. Therefore, for the Fe4N / NF catalyst sample, at a current density of 100 mA cm⁻¹...-2 The stability of the sample was then tested and passed. Figure 15 (e) We can observe that after 90 hours of durability testing, the voltage value of Fe4N / NF still shows a retention rate of 99.9%, which also proves that metal nitrides have great development potential.
[0053] To further investigate the catalytic performance of transition metal nitrides (HER), the catalytic performance of various samples was also tested in the range of 5–30 mV / s. -1 Cyclic voltammetry at scan rate ( Figure 16 ), and fit its C dl value( Figure 16 e), because C dl The size of C can also reflect the size of the catalyst's electrochemical active surface area (ESCA), therefore we can also determine the size of C from the C value. dl The size of the ESCA (Excision Cycle Scale) of the electrocatalyst can be used to infer the possible factors affecting its performance. Figure 16 It can be seen that Fe4N / NF has the largest C dl Value (85.42 mF cm) -2 The value was significantly higher than that of the other three catalysts (58.25 mF cm⁻¹). -2 43.67 mF cm -2 36.45 mF cm -2 Therefore, this can also explain why FeNNi3 / NF exhibits good HER catalytic activity; it may be due to its larger electrochemical active area, resulting in more electrochemical active sites. Similarly, MOF treatment leads to a decrease in the electrochemical active area of the catalyst sample, corresponding to the two smallest C sites. dl The decrease in this value has a particularly significant impact on the catalyst's HER catalytic activity. In summary, NiFe-MOF treatment has an adverse effect on the catalytic performance of transition metal nitrides in the HER process. This effect may stem from the reduction in electrochemical active area during the encapsulation process, thereby affecting the electron transfer rate and the number of electrochemical active sites.
[0054] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing anti-perovskite transition metal nitrides, characterized in that, The preparation method includes the following steps: S1, Pretreatment of nickel foam; S2. Dissolve Co(NO3)2·6H2O, Fe(NO3)3·9H2O and urea in deionized water to form a mixed solution. After stirring evenly, add nickel foam, heat to react, cool to room temperature, wash and dry to obtain nickel foam loaded with the sample precursor. S3. In an NH3 atmosphere, heat nickel foam loaded with the sample precursor and maintain the temperature to obtain an anti-perovskite transition metal nitride.
2. The preparation method according to claim 1, characterized in that, The specific operation of the pretreatment of nickel foam in step S1 is as follows: place the nickel foam in acetone, 3 M HCl and anhydrous ethanol respectively and sonicate it in an ultrasonic cleaner for 20-25 minutes. Then, wash it three times with deionized water and dry it in a vacuum drying oven at 70-72℃ for 0.5 hours before taking it out.
3. The preparation method according to claim 1, characterized in that, The molar ratio of Co(NO3)2·6H2O, Fe(NO3)3·9H2O and urea in step S2 is 1:3:
14.
4. The preparation method according to claim 1, characterized in that, The heating reaction described in step S2 is carried out in an electrically heated drying oven at 120-125°C for 10 h.
5. The preparation method according to claim 1, characterized in that, The washing process described in step S2 specifically involves washing the sample-loaded nickel foam 3-4 times with anhydrous ethanol and deionized water, and drying at a temperature of 60-62°C.
6. The preparation method according to claim 1, characterized in that, The heating described in step S3 is specifically heating to 420°C at a heating rate of 10°C / min and holding at that temperature for 4-4.2 hours.