Cobalt and phosphorus doped molybdenum disulfide electrocatalyst, and preparation method and application thereof
By growing cobalt and phosphorus co-doped molybdenum disulfide in situ on carbon cloth, the 1T phase transformation of MoS₂ was achieved, which solved the problems of poor conductivity and insufficient active sites in the prior art, improved the catalytic activity of the catalyst and the stability of the electrode, and simplified the preparation process.
Patent Information
- Application Number
- CN202611205553.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-24
AI Technical Summary
Existing molybdenum disulfide-based electrocatalysts exhibit reduced activity in alkaline hydrogen evolution reactions due to poor conductivity and insufficient active sites in the 2H phase, complex preparation processes, and the need for binder coating. Existing doping modification methods suffer from limited improvement in 1T phase content and require multiple processing steps.
In-situ growth of cobalt and phosphorus co-doped molybdenum disulfide on carbon cloth via a one-step hydrothermal synthesis method forms a self-supporting electrode structure, achieving the 2H to 1T phase transition of MoS₂, simplifying the preparation process and improving charge transport efficiency.
It significantly increased the 1T phase content to 73.56%, exhibited excellent HER catalytic activity under alkaline conditions, simplified the electrode preparation process, avoided active site blockage, and reduced costs.
Smart Images

Figure CN123153100A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrocatalytic energy materials technology, specifically to cobalt and phosphorus-doped molybdenum disulfide electrocatalysts, their preparation methods, and applications. Background Technology
[0002] Hydrogen energy, as a clean energy carrier with high energy density and zero carbon emissions, is considered an important component of the future energy structure. Electrolysis of water to produce hydrogen is a key technological pathway for achieving large-scale green hydrogen production. Its core challenge lies in developing efficient, stable, and economical electrocatalysts to reduce the overpotential of the hydrogen evolution reaction (HER) and improve energy conversion efficiency. Currently, while platinum-based noble metal catalysts exhibit excellent performance, their scarcity and high cost severely restrict their large-scale commercial application. Therefore, the development of high-performance non-noble metal HER catalysts based on abundant Earth elements has become a research hotspot in the field of energy materials.
[0003] Transition metal-based materials, particularly two-dimensional layered transition metal chalcogenides (TMDs), have attracted considerable attention due to their abundant resources, tunable structure, and promising catalytic potential. Among them, molybdenum disulfide (MoS2), with its unique two-dimensional layered structure, suitable hydrogen adsorption free energy, and good chemical stability, is considered one of the most promising non-noble metal HER catalysts. Studies have shown that the catalytic activity of MoS2 mainly originates from its edge unsaturated coordinating atoms (such as Mo and S atoms), which can effectively promote proton adsorption and reduction; however, its large-area basal surface atoms are in a saturated coordination state, resulting in extremely low catalytic activity, which severely limits its overall catalytic efficiency.
[0004] Despite the theoretical advantages of MoS2 in the field of HER (Heterochromatographic reaction), its practical application still faces several key bottlenecks. First, the thermodynamically stable 2H phase of MoS2 exhibits poor electrical conductivity, limiting charge transfer efficiency during catalysis. Second, its active sites are confined to peripheral regions, are limited in number, and the adsorption energy for reaction intermediates is difficult to precisely control, resulting in slow water molecule dissociation kinetics in alkaline media, further restricting breakthroughs in catalytic performance. To address these challenges, researchers have developed various modification strategies, including morphology engineering, defect engineering, heteroatom doping, and heterostructure construction. Among these, heteroatom doping has been proven to effectively regulate the electronic structure of MoS2 and optimize the adsorption / desorption behavior of active sites. Studies have shown that by introducing transition metals or non-metallic elements, the local electron density of MoS2 can be adjusted, and even a transition from the 2H phase to the 1T / 1T' phase can be induced, thereby significantly improving the intrinsic conductivity and catalytic activity of the material.
[0005] However, existing doping modification studies still have the following shortcomings: On the one hand, the 1T phase content of most doped systems (such as N,P-MoS2) is still limited, and phase transformation requires multiple heat treatments or additional carbon layer coating, which is complex and energy-intensive; on the other hand, traditional powdered catalysts require the addition of polymer binders during electrode preparation, which not only increases the preparation steps, but also easily blocks active sites, reduces interfacial charge transport efficiency, and affects the long-term stability of the catalyst layer.
[0006] Based on this, we developed a doped MoS2-based electrocatalyst with a simple process and integrated structure, which can achieve a self-supporting electrode structure while increasing the 1T phase content. This is of great significance for promoting the practical application of alkaline water electrolysis hydrogen production technology. Summary of the Invention
[0007] The present invention aims to overcome the problems of poor conductivity of the 2H phase, insufficient active sites, and complex preparation process of existing molybdenum disulfide-based electrocatalysts in alkaline hydrogen evolution reaction, which leads to reduced activity. Existing doping modification methods still have the problems of limited improvement of 1T phase content, need for multiple steps, and unsatisfactory electrode structure.
[0008] To achieve the above objectives, a first aspect of the present invention provides a method for preparing a cobalt and phosphorus-doped molybdenum disulfide electrocatalyst, comprising the following steps: Cobalt and phosphorus co-doped molybdenum disulfide was grown in situ on carbon cloth in a precursor solution by a one-step hydrothermal synthesis method to obtain a cobalt and phosphorus doped molybdenum disulfide electrocatalyst. The precursor solution is a solution obtained by dissolving a molybdenum source, a sulfur source, a cobalt source, and a phosphorus source in a solvent.
[0009] A second aspect of the present invention provides a cobalt and phosphorus-doped molybdenum disulfide electrocatalyst prepared by the method described in the first aspect.
[0010] The third aspect of this invention provides the application of the cobalt and phosphorus-doped molybdenum disulfide electrocatalyst described in the second aspect in the alkaline water electrolysis hydrogen evolution reaction.
[0011] Compared with the prior art, the present invention has at least the following beneficial effects: 1. This invention successfully induced the 2H to 1T phase transition in MoS2 through Co and P co-doping. Raman spectroscopy confirmed the presence of the characteristic vibrational peak of the 1T phase, and XPS quantitative analysis showed that the 1T phase accounted for as high as 73.56% of the total molybdenum disulfide phase in the cobalt and phosphorus-doped molybdenum disulfide electrocatalyst (Co,P-MoS2 / CC) provided by this invention, which is about 30% higher than that of undoped MoS2 / CC. The high 1T phase content endows the material with excellent intrinsic conductivity and effectively promotes the charge transport efficiency during the catalytic process.
[0012] 2. The Co,P-MoS2 / CC self-supporting electrode prepared in this invention exhibits excellent HER catalytic activity under alkaline conditions of 1.0 M KOH. At 10 mA cm⁻¹ -2 At a current density of only 54.3 mV, the overpotential was demonstrated to be only 54.3 mV, proving that the synergistic effect of Co and P co-doping significantly enhances catalytic activity.
[0013] 3. This invention employs a one-step hydrothermal method to grow Co,P-MoS2 in situ on carbon cloth, forming a self-supporting electrode structure. This structure eliminates the need for polymer binders or additional coating steps, avoiding the problems of active site blockage and reduced interfacial charge transport efficiency encountered in traditional powder catalyst electrode preparation. It can be directly used as a working electrode, simplifying the electrode preparation process.
[0014] 4. This invention achieves co-doping of Co and P and in-situ growth of MoS2 on carbon cloth simultaneously through a one-step hydrothermal synthesis method. The reaction conditions are mild, the operation is simple, the cycle is short, the cost is low, and it is easy to scale up production and promote industrialization, thus having good prospects for commercial application. Attached Figure Description
[0015] Figure 1 These are scanning electron microscope images of the electrocatalysts prepared in the preferred embodiments and comparative examples of the present invention; Figure 2 These are Raman spectra comparisons of the electrocatalysts prepared in the preferred embodiments and comparative examples of the present invention; Figure 3 This is a comparison of linear sweep voltammetry curves of the electrocatalysts prepared in the preferred embodiment and comparative example of the present invention. Detailed Implementation
[0016] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0017] As previously stated, the first aspect of this invention provides a method for preparing cobalt and phosphorus-doped molybdenum disulfide electrocatalysts, comprising the following steps: Cobalt and phosphorus co-doped molybdenum disulfide was grown in situ on carbon cloth in a precursor solution by a one-step hydrothermal synthesis method to obtain a cobalt and phosphorus doped molybdenum disulfide electrocatalyst. The precursor solution is a solution obtained by dissolving a molybdenum source, a sulfur source, a cobalt source, and a phosphorus source in a solvent.
[0018] Preferably, the method of the present invention further includes pretreating the carbon cloth before performing the one-step hydrothermal synthesis method, including: placing the carbon cloth in acetone, ethanol and water for ultrasonic treatment for 15 min each to remove organic impurities on the surface, and then immersing it in a 65 wt% nitric acid solution for 30 min to obtain the pretreated carbon cloth, which is then applied to the one-step hydrothermal synthesis method.
[0019] In a preferred embodiment, the molybdenum source is ammonium molybdate tetrahydrate, the sulfur source is thiourea, the cobalt source is a cobalt salt, and the phosphorus source is hypophosphite.
[0020] Preferably, the cobalt salt is selected from one or more of cobalt chloride, cobalt nitrate, and cobalt acetate.
[0021] Preferably, the hypophosphite is sodium hypophosphite.
[0022] In a preferred embodiment, the molar ratio of cobalt to phosphorus in the precursor solution is 1:0.5-2.
[0023] Preferably, the molar ratio of molybdenum to sulfur in the precursor solution is 1:4.5-6.5.
[0024] More preferably, the method for preparing the precursor solution includes: dissolving a molybdenum source and a sulfur source in deionized water at a speed of 500-800 rpm, stirring for 10-30 min, then adding a cobalt source and a phosphorus source in sequence, and continuing to stir for 10-30 min.
[0025] According to a preferred embodiment, the conditions for the one-step hydrothermal synthesis method are at least: a temperature of 160-200°C and a time of 18-30 hours.
[0026] In a preferred embodiment, after the one-step hydrothermal synthesis is completed, the reaction product is further further comprising: repeatedly rinsing the reaction product with deionized water and anhydrous ethanol in sequence, and then drying it in a vacuum drying oven.
[0027] According to a preferred embodiment, the drying temperature is 50-80°C and the drying time is 8-16 hours.
[0028] As previously described, a second aspect of the present invention provides a cobalt and phosphorus-doped molybdenum disulfide electrocatalyst prepared by the method described in the first aspect.
[0029] According to a preferred embodiment, the molybdenum disulfide in the catalyst is a mixed phase of 1T phase and 2H phase, and the ratio of 1T phase to the total molybdenum disulfide phase content in the catalyst is not less than 70%.
[0030] More preferably, in this catalyst, the ratio of the 1T phase to the total molybdenum disulfide phase is 73-75%.
[0031] It should be noted that, in this invention, the ratio of the 1T phase to the total molybdenum disulfide phase content is calculated based on the peak area fitting results of Mo3d or S2p peaks in the XPS spectrum, with the total molybdenum disulfide phase content being 100%.
[0032] Preferably, the Raman spectrum of the cobalt and phosphorus-doped molybdenum disulfide has a value at least at 145.3 ± 2 cm⁻¹. -1 192.6±2 cm -1 and 232.5±2 cm -1 It has a characteristic vibration peak of the 1T phase.
[0033] As previously stated, the third aspect of the present invention provides the application of the cobalt and phosphorus-doped molybdenum disulfide electrocatalyst described in the second aspect in the alkaline water electrolysis hydrogen evolution reaction.
[0034] The present invention will be described in detail below through examples. Unless otherwise specified, the raw materials used are all commercially available products.
[0035] Unless otherwise specified, "room temperature" or "normal temperature" in this invention refers to a temperature of 20-25°C.
[0036] Carbon cloth: HCP330N, resistance measurement value is 0.35*10 -2 Ohm, thickness: 0.4±0.02mm, purchased from Shanghai Hesen Electric Co., Ltd.; Molybdenum source: ammonium molybdate tetrahydrate, purchased from Shanghai Titan Technology Co., Ltd. Sulfur source: Thiourea, purchased from Shanghai Titan Technology Co., Ltd.
[0037] Cobalt source: Co(NO3)2·6H2O, purchased from Shanghai Titan Technology Co., Ltd.; Phosphorus source: NaH2PO2·H2O, purchased from Shanghai Titan Technology Co., Ltd.
[0038] Pretreatment of carbon fiber cloth: Cut the carbon fiber cloth into 2×3 cm pieces. 2 The sheet-like material was placed in acetone, ethanol, and water for 15 min each to remove organic impurities from the surface. Then it was immersed in 65 wt% nitric acid solution for 30 min, washed with deionized water, and dried to obtain the pretreated carbon cloth.
[0039] Precursor solution: Preparation of precursor solution I: At a speed of 500 rpm, 0.742 g of molybdenum source and 1.370 g of sulfur source were dissolved in deionized water and stirred for 30 min. Then, 0.029 g of cobalt source and 0.021 g of phosphorus source were added in sequence, and stirring was continued for 30 min.
[0040] Preparation of precursor solution II: 0.742 g of molybdenum source and 1.370 g of sulfur source were dissolved in deionized water at 600 rpm and stirred for 30 min.
[0041] Preparation of precursor solution III: At a speed of 700 rpm, 0.742 g of molybdenum source and 1.370 g of sulfur source were dissolved in deionized water and stirred for 15 min. Then, 0.021 g of phosphorus source was added and stirred for another 15 min.
[0042] Preparation of precursor solution IV: At a speed of 800 rpm, 0.742 g of molybdenum source and 1.370 g of sulfur source were dissolved in deionized water and stirred for 10 min. Then, 0.029 g of cobalt source was added and stirred for another 10 min.
[0043] Example 1
[0044] This embodiment illustrates that the method for preparing cobalt and phosphorus-doped molybdenum disulfide electrocatalysts provided by the present invention is carried out according to the following steps: In a 50 mL polytetrafluoroethylene-lined reactor, pretreated carbon was placed in a precursor solution and hydrothermally synthesized in situ at 180 °C for 24 h using a one-step hydrothermal method to grow cobalt and phosphorus co-doped molybdenum disulfide on the carbon cloth. The reaction product was repeatedly washed with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 60 °C for 12 h to obtain a cobalt and phosphorus doped molybdenum disulfide electrocatalyst, named P1. P1 was analyzed by scanning electron microscopy (SEM). Figure 1 The right image in the figure shows the SEM image of P1. It can be seen from the figure that the microstructure of P1 is a fine and tiny nanosheet with a high specific surface area, which can expose more active sites.
[0045] Comparative Example 1 The procedure was carried out using a method similar to that in Example 1, except that the precursor solution used was Precursor Solution II; The undoped MoS2 / CC electrocatalyst was finally obtained and named DP1.
[0046] DP1 was analyzed by scanning electron microscopy (SEM). Figure 1 The left image shows a SEM image of DP1, which shows that the microstructure of DP1 consists of dense nanospheres that are arranged in a neat and orderly manner.
[0047] Comparative Example 2 The procedure was carried out using a method similar to that in Example 1, except that the precursor solution used was Precursor Solution III; The final P-MoS2 / CC electrocatalyst was obtained and named DP2.
[0048] Comparative Example 3 The procedure was carried out using a method similar to that in Example 1, except that the precursor solution used was Precursor Solution IV; The final Co-MoS2 / CC electrocatalyst was obtained and named DP3.
[0049] Test Example 1 This application example demonstrates Raman spectroscopy testing of the electrocatalysts prepared in the above examples. Figure 2 The Raman spectra of P1 and DP1 are shown in the comparison diagram. It can be seen from the figure that for DP1, the spectrum is located at 383.2 cm⁻¹. -1 and 408.1cm -1 The peak at this point corresponds to both in-plane and out-of-plane vibrational modes of the 2H phase. In P1, a peak at 145.3 cm⁻¹ is also observed. -1 192.6 cm -1 232.5 cm -1 279.4 cm -1 333.3cm -1 A new characteristic peak was observed, which corresponds to the characteristic phonon vibration mode of 1T phase MoS2.
[0050] Test Example 2 The relative contents of the 1T and 2H phases of MoS2 in the electrocatalysts prepared in the above examples were quantitatively determined by X-ray photoelectron spectroscopy (XPS) peak fitting. The total amount of molybdenum disulfide phase was taken as 100%. Al Kα rays (1486.6 eV) were used as the excitation source, and all binding energies were corrected with the C 1s peak (284.8 eV). The results are shown in Table 1.
[0051] Table 1
[0052] Test Example 3 The electrocatalytic activity of the electrocatalysts prepared in the above examples for the hydrogen evolution reaction (HER) in 1.0 M KOH solution was determined by linear sweep voltammetry (LSV). Figure 3 The linear sweep voltammetry curves of the electrocatalysts prepared in the above examples are shown for comparison. The figure shows that the HER activity of P1 is significantly enhanced at 10 mA cm⁻¹. -2The overpotential at current density is only 54.3 mV, which is better than DP2 (72.8 mV), DP3 (82.7 mV) and DP1 (139.5 mV). This is because the sulfur atoms at the edge of MoS2 have a moderate adsorption energy for hydrogen, which is conducive to the adsorption and desorption of hydrogen.
[0053] The above experimental results demonstrate that in the co-doped molybdenum disulfide electrocatalyst prepared in situ on carbon cloth via a one-step hydrothermal method, the co-doping of Co and P successfully induced the transformation of MoS2 from the 2H phase to the 1T phase, with the 1T phase content significantly increasing from 56.43% to 73.56%. This catalyst requires only 54.3 mV overpotential to reach 10 mAcm in alkaline HER. -2 The current density is significantly better than that of single-doped and undoped samples. At the same time, the self-supporting electrode structure grown in situ with carbon cloth eliminates the need for binder coating and avoids the problem of active site blockage, showing excellent catalytic activity and good application prospects.
[0054] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for preparing cobalt and phosphorus-doped molybdenum disulfide electrocatalysts, characterized in that, Includes the following steps: Cobalt and phosphorus co-doped molybdenum disulfide was grown in situ on carbon cloth in a precursor solution by a one-step hydrothermal synthesis method to obtain a cobalt and phosphorus doped molybdenum disulfide electrocatalyst. The precursor solution is a solution obtained by dissolving a molybdenum source, a sulfur source, a cobalt source, and a phosphorus source in a solvent.
2. The preparation method according to claim 1, characterized in that, The molybdenum source is ammonium molybdate tetrahydrate, the sulfur source is thiourea, the cobalt source is cobalt salt, and the phosphorus source is hypophosphite.
3. The preparation method according to claim 1 or 2, characterized in that, In the precursor solution, the molar ratio of cobalt to phosphorus is 1:0.5-2.
4. The preparation method according to claim 1 or 2, characterized in that, The conditions for the one-step hydrothermal synthesis method must at least meet the following requirements: temperature 160-200℃ and time 18-30h.
5. The preparation method according to claim 1 or 2, characterized in that, After the one-step hydrothermal synthesis method is completed, the process further includes: repeatedly rinsing the reaction product with deionized water and anhydrous ethanol in sequence, and then drying it in a vacuum drying oven.
6. The preparation method according to claim 5, characterized in that, The drying temperature is 50-80℃, and the drying time is 8-16 hours.
7. A cobalt and phosphorus-doped molybdenum disulfide electrocatalyst prepared by the preparation method according to any one of claims 1-6.
8. The cobalt and phosphorus-doped molybdenum disulfide electrocatalyst according to claim 7, characterized in that, In this catalyst, molybdenum disulfide is a mixed phase of 1T phase and 2H phase, and the ratio of 1T phase to total molybdenum disulfide phase content is not less than 70%.
9. The cobalt and phosphorus-doped molybdenum disulfide electrocatalyst according to claim 8, characterized in that, In the Raman spectrum of the cobalt and phosphorus-doped molybdenum disulfide, at least at 145.3 ± 2 cm⁻¹ -1 192.6±2 cm -1 and 232.5±2 cm -1 It has a characteristic vibration peak of the 1T phase.
10. The application of the cobalt and phosphorus-doped molybdenum disulfide electrocatalyst according to any one of claims 7-9 in the alkaline water electrolysis hydrogen evolution reaction.