Metal salt regulated composite phosphating layer modified iron-based alloy hydrogen evolution electrode and preparation method thereof

By constructing a leaf-shaped composite phosphating layer on an iron-based alloy hydrogen evolution electrode and using metal salts for regulation, the problem of low performance of the iron-based alloy hydrogen evolution electrode was solved, achieving high efficiency catalytic performance and low cost preparation under different current densities.

CN123153101APending Publication Date: 2026-11-24ZHONGSHAN POWER SUPPLY BUREAU OF GUANGDONG POWER GRID +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611463904.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing iron-based alloy hydrogen evolution electrodes have low performance and cannot meet the energy consumption requirements of industrial-grade high current density. Traditional phosphating technology has high equipment requirements, high energy consumption, and uneven film formation, making it difficult to simultaneously meet the multi-step requirements of rapid water dissociation, moderate hydrogen adsorption, and rapid hydrogen desorption.

Method used

A method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer is proposed. This method involves constructing a leaf-shaped composite phosphating layer at room temperature using a manganese-zinc based phosphating system, and then using different metal ions for secondary regulation to optimize the alkaline hydrogen evolution activity of the iron-based alloy cathode.

Benefits of technology

The catalytic performance of the iron-based alloy hydrogen evolution electrode was significantly improved at both low and high current densities, the preparation cost was reduced, the limitations of high-temperature phosphating or strong ultrasonic fields were avoided, and the electrochemical performance of the electrode was ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153101A_ABST
    Figure CN123153101A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of water electrolysis, and particularly relates to a metal salt regulated composite phosphating layer modified iron-based alloy hydrogen evolution electrode and a preparation method thereof. The application provides a preparation method of a metal salt regulated composite phosphating layer modified iron-based alloy hydrogen evolution electrode. On the basis of in-situ construction of a leaf-shaped composite phosphating layer for morphology modification in a manganese-zinc basic phosphating system, metal salt regulation is used to perform secondary regulation on the leaf-shaped phosphating layer by using different metal ions, so that the alkaline hydrogen evolution activity of the iron-based alloy cathode is further optimized on the basis of retaining the original porous structure of the phosphating layer and the advantages of substrate combination. At the same time, by using different metal salt regulation, an experimental basis is provided for screening a promotion metal which takes into account the initial performance and high current density performance, and a cheap and high catalytic activity hydrogen evolution electrode is expected to be obtained, so that the technical problem of low performance of the iron-based alloy hydrogen evolution electrode in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of water electrolysis technology, and in particular relates to an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer and its preparation method. Background Technology

[0002] With the acceleration of global energy transition, using "green electricity" generated from renewable energy for water electrolysis to produce hydrogen has become a key path to solve the problem of wind and solar power consumption and achieve deep decarbonization. Among the mainstream water electrolysis technologies, alkaline water electrolysis (ALK) is widely used due to its high technological maturity. Large-scale hydrogen production places stringent requirements on equipment economy and catalytic efficiency. The hydrogen evolution reaction (HER) occurs at the cathode of the alkaline electrolyzer, and the cathode overpotential directly determines the cell voltage and hydrogen production energy consumption. Currently, commercial cathodes mostly use nickel mesh, nickel foam, or nickel-based alloys, and the cost is significantly constrained by the price of nickel.

[0003] Iron (Fe)-based alloys are considered ideal alternatives to pure nickel oxygen evolution electrodes due to their low raw material costs, excellent mechanical properties, and the presence of transition metals on their surface. However, when used directly in water electrolysis, iron-based alloys are often limited by a lack of surface active sites and sluggish intrinsic hydrogen evolution kinetics, making it difficult to meet the energy consumption requirements of high current densities in industrial applications. Improving the electrocatalytic activity of iron-based alloys is expected to meet the economic and catalytic efficiency requirements of alkaline water electrolysis for hydrogen production. Surface modification is an effective way to improve the hydrogen evolution performance of iron-based alloys, addressing issues such as surface active sites and intrinsic hydrogen evolution kinetics. Transition metal phosphides (TMPs) are widely used in constructing hydrogen evolution catalyst layers because they possess moderate hydrogen adsorption free energy and good electronic conductivity, simultaneously improving hydrogen intermediate adsorption and charge transport processes. However, traditional phosphating... Phosphating techniques often rely on high temperatures and ultrasound, requiring sophisticated equipment and consuming large amounts of energy, which is not conducive to the low-cost fabrication of large-area electrodes. Furthermore, previous phosphating methods, relying solely on a single phosphating solution component, are prone to problems such as uneven film formation, a single active phase, localized excessive corrosion, or weak adhesion of the deposited layer when processing multi-element iron-based alloys. In recent years, multi-component phosphating solution modification has focused on constructing porous, rough surfaces on the iron-based alloy surface to increase specific surface area and the number of exposed active sites through morphological modification. While this method can improve electrode surface roughness and electrolyte contact area, at higher current densities, relying solely on phosphating layer morphology control often fails to simultaneously meet the requirements of rapid water dissociation, moderate hydrogen adsorption, and rapid hydrogen desorption, resulting in insufficient hydrogen evolution catalytic performance. Therefore, although iron-based alloy-based oxygen evolution electrodes exist, their catalytic performance still needs improvement. Summary of the Invention

[0004] In view of this, this application provides a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode and its preparation method, which is used to solve the technical problem of low performance of iron-based alloy hydrogen evolution electrodes in the prior art.

[0005] The first aspect of this application provides a method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode, comprising the following steps: Preparation steps of basic phosphating solution: Add phosphoric acid (H3PO4), potassium dihydrogen phosphate (KH2PO4), trans-cinnamic acid (C9H8O2), manganese chloride (MnCl2), and zinc nitrate (Zn(NO3)2) to water and stir until dissolved to obtain basic phosphating solution; Preparation steps for regulating phosphating solution: Add at least one metal salt selected from copper salt, erbium salt, indium salt, molybdenum salt, and bismuth salt to the base phosphating solution and stir until dissolved to obtain metal ion regulated phosphating solution; The steps for modifying the phosphating layer are as follows: The iron-based alloy is immersed in a metal ion-controlled phosphating solution and stirred at room temperature (20~35℃) to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer.

[0006] Preferably, in the preparation step of the basic phosphating solution, each 30 mL of the basic phosphating solution comprises: 3-9 mmol of phosphoric acid (H3PO4), 3-9 mmol of potassium dihydrogen phosphate (KH2PO4), 0.005-0.02 mmol of trans-cinnamic acid (C9H8O2), 1-5 mmol of manganese chloride (MnCl2), and 3-9 mmol of zinc nitrate (Zn(NO3)2).

[0007] Preferably, each 30 mL of the basic phosphating solution comprises: 6.3 mmol phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 0.01 mmol trans-cinnamic acid (C9H8O2), 3 mmol manganese chloride (MnCl2), and 6 mmol zinc nitrate (Zn(NO3)2).

[0008] Preferably, in the step of preparing the phosphating solution, the copper salt is selected from at least one of copper nitrate, copper chloride, copper sulfate, copper acetate, and their hydrates; The erbium salt is selected from at least one of erbium nitrate, erbium chloride, erbium sulfate, erbium acetate, and their hydrates; The indium salt is selected from at least one of indium nitrate, indium chloride, indium sulfate, indium acetate, and their hydrates; The molybdenum salt is selected from at least one of sodium molybdate, potassium molybdate, and ammonium molybdate. The bismuth salt is selected from at least one of bismuth nitrate, bismuth chloride, bismuth sulfate, bismuth acetate, and their hydrates.

[0009] Preferably, in the preparation step of the phosphating solution, 1-6 mmol of metal salt is added to every 30 mL of the base phosphating solution.

[0010] Preferably, in the step of modifying the phosphate layer, the iron-based alloy is a sheet-like iron-based alloy obtained by smelting, casting, and cutting elemental raw materials of Fe, Ni, Co, Cr, and Mo in mass percentages of 55-85%, Ni, 10-20%, Co, 5-15%, Cr, 2.5-3.5%, and Mo, 0.5-1.5%; and contains unavoidable carbon (C) with a content not exceeding 0.5%.

[0011] Preferably, in the step of modifying the phosphate layer, the iron-based alloy is selected from iron-based alloys that are sequentially polished, cleaned, and dried.

[0012] Preferably, in the step of modifying the phosphating layer, the stirring speed during phosphating is 200~1000 rpm, and the phosphating time is 8~24h.

[0013] Preferably, in the step of modifying the phosphating layer, the post-treatment process after stirring phosphating includes: rinsing with deionized water and drying.

[0014] The second aspect of this application provides a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode, which is prepared by the preparation method described in the first aspect.

[0015] The third aspect of this application provides the application of the iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer as described in the second aspect in the field of hydrogen production by water electrolysis.

[0016] The fourth aspect of this application provides an alkaline electrolyzer, including end plates, bipolar plates, anodes, diaphragms, cathodes, alkaline electrolytes, and sealing components, which are assembled using existing conventional processes; among the components, the cathode is selected from the iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer as described in the second aspect, and the alkaline electrolyte is selected from a 0.5~1.5M KOH electrolyte.

[0017] Compared with the prior art, the method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode provided in this application has at least the following beneficial effects: 1. This application provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. Based on the morphological modification of the leaf-shaped composite phosphating layer constructed in situ using a manganese-zinc-based phosphating system, metal salt regulation is used to further regulate the leaf-shaped phosphating layer by using different metal ions. This further optimizes the alkaline hydrogen evolution activity of the iron-based alloy cathode while retaining the original porous structure and substrate bonding advantages of the phosphating layer. Moreover, the phosphating process is carried out by stirring at room temperature, avoiding the limitations of high-temperature phosphating or strong ultrasonic fields on the preparation of the hydrogen evolution electrode.

[0018] 2. The method for preparing a metal salt-regulated composite phosphating layer modified iron-based alloy hydrogen evolution electrode provided in this application can selectively regulate different stages of HER initiation, such as small current density and large current density, by using different metal salts. This provides experimental basis for screening promoting metals that take into account both initiation performance and high current density performance. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0020] Figure 1 XRD patterns of the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1 of this application before and after phosphating treatment with a basic phosphating solution. Figure 2 The images shown are scanning electron microscope (SEM) images and superimposed surface scanning mapping images of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 of this application before phosphating treatment with basic phosphating solution, wherein (a) is a scanning electron microscope image and (b) is a mapping image. Figure 3 The images shown are scanning electron microscope (SEM) images and superimposed surface scanning mapping images of the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 1 of this application before phosphating treatment in the basic phosphating solution. (a) is a scanning electron microscope image and (b) is a mapping image. Figure 4 The hydrogen evolution performance test results of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 of this application are shown in the figure before and after the basic phosphating solution phosphating treatment. Figure 5 The figure shows the test results of hydrogen evolution performance of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 of this application and the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer and regulated by metal salt provided in Example 1. Figure 6 The graph shows the test results of hydrogen evolution performance of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 and the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer and regulated by metal salt provided in Example 2. Figure 7 The graph shows the hydrogen evolution performance test results of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 and the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer and regulated by metal salt provided in Example 3. Figure 8The graph shows the test results of hydrogen evolution performance of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 and the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer and regulated by metal salt provided in Example 4. Figure 9 The graph shows the hydrogen evolution performance test results of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 and the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer and regulated by metal salt provided in Example 5. Detailed Implementation

[0021] This application provides a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode and its preparation method, which solves the technical problem of low performance of iron-based alloy hydrogen evolution electrodes in the prior art.

[0022] The technical solutions of this application will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0023] Example 1

[0024] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0025] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 3 mmol of bismuth nitrate (Bi(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0026] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0027] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Bi(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0028] Example 2

[0029] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0030] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 3 mmol of sodium molybdate (Na2MoO4) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0031] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0032] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Na2MoO4. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0033] Example 3

[0034] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0035] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 3 mmol of indium nitrate (In(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0036] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0037] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-In(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0038] Example 4

[0039] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0040] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 3 mmol of erbium nitrate (Er(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0041] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0042] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Er(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0043] Example 5

[0044] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0045] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 3 mmol of copper nitrate Cu(NO3)2 and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0046] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0047] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Cu(NO3)2. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0048] Example 1

[0049] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0050] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 1 mmol of bismuth nitrate (Bi(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0051] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0052] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Bi(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0053] Example 2

[0054] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0055] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 1 mmol of sodium molybdate (Na2MoO4) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-controlled phosphating solution.

[0056] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0057] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Na2MoO4. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0058] Example 3

[0059] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0060] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 1 mmol of indium nitrate (In(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0061] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0062] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-In(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0063] Example 4

[0064] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0065] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 1 mmol of erbium nitrate (Er(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0066] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0067] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Er(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0068] Example 5

[0069] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0070] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 1 mmol of copper nitrate Cu(NO3)2 and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0071] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0072] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Cu(NO3)2. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0073] Example 1

[0074] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0075] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 6 mmol of bismuth nitrate (Bi(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0076] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0077] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Bi(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0078] Example 2

[0079] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0080] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 6 mmol of sodium molybdate (Na2MoO4) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-controlled phosphating solution.

[0081] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0082] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Na2MoO4. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0083] Example 3

[0084] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0085] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 6 mmol of indium nitrate (In(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain a metal ion-regulated phosphating solution.

[0086] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0087] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-In(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0088] Example 4

[0089] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0090] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 6 mmol of erbium nitrate (Er(NO3)3) and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0091] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0092] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Er(NO3)3. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0093] Example 5

[0094] This embodiment provides a method for preparing an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer. The preparation method includes a basic phosphating solution preparation step, a regulated phosphating solution preparation step, and a phosphating layer modification step.

[0095] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for preparing the phosphating solution include: Weigh 6 mmol of copper nitrate Cu(NO3)2 and add it to 30 mL of basic phosphating solution. Stir until dissolved to obtain metal ion-regulated phosphating solution.

[0096] The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0097] The pretreated iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphating was performed at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the stirring speed and time were controlled to avoid incomplete phosphating layer due to too slow speed or too short stirring time, while too fast speed or too long stirring time may lead to over-etching or damage to the phosphating layer structure. After the phosphating treatment, the electrode was removed, repeatedly rinsed with deionized water, and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P-Cu(NO3)2. In this embodiment, a large amount of deionized water was used to repeatedly rinse the electrode surface to thoroughly remove residual phosphating solution and reaction byproducts. Thorough cleaning and drying can avoid active layer contamination and ensure the final electrochemical performance of the electrode.

[0098] Comparative Example 1

[0099] This comparative example provides a method for preparing a composite phosphating layer modified iron-based alloy hydrogen evolution electrode. The preparation method includes the steps of preparing a basic phosphating solution and modifying the phosphating layer.

[0100] The preparation steps for the basic phosphating solution include: Weigh 18 mL of 0.35 mol / L phosphoric acid (H3PO4), 6 mmol potassium dihydrogen phosphate (KH2PO4), 3 mmol manganese chloride (MnCl2), 6 mmol zinc nitrate (Zn(NO3)2) and 0.1 mmol trans-cinnamic acid (C9H8O2), add them to deionized water and stir until dissolved to obtain 30 mL of basic phosphating solution; The steps for modifying the phosphating layer include: The raw materials of Fe, Ni, Co, Cr, and Mo, weighed according to the mass percentages of Fe: 71%, Ni: 15%, Co: 10%, Cr: 3%, and Mo: 1%, are subjected to conventional metal smelting and ingot casting processes and cut into sheet form to form an iron-based alloy; the carbon (C) content in the iron-based alloy, which is inevitably introduced by the raw materials and smelting process, shall not exceed 0.5%; The iron-based alloy substrate surface is successively polished using metallographic sandpaper ranging from 200 to 800 grit. The polished substrate is then ultrasonically cleaned in anhydrous ethanol and deionized water, and finally dried. This pretreatment process can obtain a uniform surface state and thoroughly remove oil and impurities, providing a relatively ideal initial surface for the subsequent formation of a uniform phosphating layer.

[0101] The pretreated iron-based alloy was immersed in a basic phosphating solution and phosphated at room temperature (20~35℃) with magnetic stirring at 500 rpm for 16 hours. In this embodiment, the phosphate treatment can control the morphology of the iron-based alloy substrate, thereby forming a leaf-shaped phosphate layer on the surface of the iron-based alloy. After the phosphating treatment, the electrode was removed, rinsed repeatedly with deionized water and dried to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer, denoted as P.

[0102] Experimental Example 1

[0103] This experimental example analyzes the surface structure, composition and morphology of the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1 and the iron-based alloy (Pristine) provided in Comparative Example 1 that was not immersed in the base phosphating solution for phosphating treatment. The analysis was performed using X-ray diffraction (XRD) and scanning electron microscopy combined with energy dispersive spectroscopy (SEM-EDS). The composite phosphating layer modified iron-based alloy hydrogen evolution electrode provided in Comparative Example 1 was analyzed before and after phosphating treatment in the basic phosphating solution. The analytical results are as follows: Figure 1-3 And as shown in Table 1.

[0104] from Figure 1The X-ray diffraction (XRD) characterization pattern shown indicates that the iron-based alloy immersed in the base phosphating solution for phosphating mainly exhibits α-Fe matrix characteristic peaks. After phosphating with the base phosphating solution, the hydrogen evolution electrode of the iron-based alloy modified with the composite phosphating layer still retains α-Fe matrix peaks, indicating that the phosphating layer is only constructed on the surface and does not destroy the main structure of the iron-based alloy. At the same time, new diffraction peaks related to hydrated zinc phosphate appear in the treated sample, which can be attributed to zinc phosphate tetrahydrate (Zn3(PO4)2·4H2O). This result indicates that zinc salt induces the formation of a crystalline Hopstone-type phosphating layer in the room temperature phosphate system. Since this layer originates from the micro-area reaction on the substrate surface and the co-deposition of solution ions, the coexistence of matrix peaks and phosphate peaks in the XRD is consistent with the characteristics of thin-layer surface chemical transformation products.

[0105] from Figure 2 Figure (a) shows an electron micrograph of an iron-based alloy that was not immersed in the base phosphating solution for phosphating. The surface is relatively smooth, with visible mechanical polishing marks and a lack of obvious micro / nano structures. Figure 3 As shown in Figure (a), after phosphating with the basic phosphating solution, a continuous, rough layer appears on the electrode surface, locally exhibiting a leaf-like, interlocking morphology. The formation of these plate-like crystals increases the actual contact area of ​​the electrode surface and provides more interfacial channels for electrolyte wetting and gas desorption; while Figure 2 , Figure 3 As shown in Figure (b) and Table 1, the mapping analysis results indicate that compared to the untreated sample, the levels of O, P, Zn, and Mn on the P electrode surface significantly increased, with P increasing from 0 to 14.78 at.%, Zn from 0 to 13.21 at.%, and Mn from 0 to 4.15 at.%. Simultaneously, the surface signals of substrate elements such as Fe, Co, and Cr were relatively weakened, indicating that a phosphating layer had been formed on the iron-based alloy surface. This result is corroborated by the presence of hydrated zinc phosphate crystalline phases in XRD, further demonstrating that manganese components participated in the formation of the surface layer.

[0106] Table 1: Surface distribution of various elements on the surface of iron-based alloys before and after phosphating in the base phosphating solution.

[0107] Experiment Example 2

[0108] This experiment tests the performance of the iron-based alloy hydrogen evolution electrode modified with metal salt-controlled composite phosphating layer provided in Examples 1-5, the iron-based alloy hydrogen evolution electrode modified with composite phosphating layer provided in Comparative Example 1, and the iron-based alloy (Pristine) provided in Comparative Example 1 that was not immersed in the base phosphating solution for phosphating treatment.

[0109] The performance testing process included: using a standard three-electrode system from an electrochemical workstation, in a 1M KOH electrolyte, the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Examples 1-5 and the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1 were used as working electrodes. The potential of the iron-based alloy hydrogen evolution electrode at different current densities was tested, and the performance test results are shown in Table 2 and... Figures 4-9 As shown.

[0110] From Table 2 and Figure 4 It can be seen that, compared with the iron-based alloy that was not immersed in the base phosphating solution for phosphating treatment, the iron-based alloy hydrogen evolution electrode modified with the composite phosphating layer provided in Comparative Example 1 has a larger absolute value of cathode current at the same potential, and compared with the original untreated sample: the low current density at HER start-up is -10 mA cm⁻¹. -2 The potential dropped by approximately 102 mV at -100 mA cm⁻¹. -2 and -300mA cm -2 The potentials also decreased by approximately 187 mV and 260 mV, respectively. This means that at the same current density, the potential required for Comparative Example 1 is closer to 0 V, and the overpotential is lower. This indicates that the HER performance of the electrode after phosphating is significantly improved. This shows that the leaf-shaped phosphating layer obtained by growing phosphating under room temperature stirring conditions in Comparative Example 1 of this application has a high efficiency of hydrogen evolution reaction activity, especially in the medium and high current density range.

[0111] From Table 2 and Figure 5 As can be seen, compared with the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1, the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 1 exhibits lower HER start-up current density of -10 mA cm⁻¹. -2 At -72mV, the potential decreased, indicating that the introduction of bismuth salt on top of the basic phosphating layer significantly improved the hydrogen evolution initiation performance in the low current density region of the electrode. However, at -100mA cm⁻¹, the potential decreased further. -2 and -300mA cm -2 At lower current densities, the potential did not show a further decrease; therefore, the introduction of bismuth nitrate mainly promotes the hydrogen evolution in the low current density region and the reaction initiation process, while its regulatory effect is relatively limited at higher current densities.

[0112] From Table 2 and Figure 6 As can be seen, compared with the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1, the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 2 exhibits lower HER start-up current density of -10 mA cm⁻¹. -2 At -100mA cm⁻¹, the potential decreased by approximately 90mV, while at -100mA cm⁻¹... -2The potential also dropped by about 57mV, but at -300mA cm -2 The potential did not decrease further, indicating that the addition of molybdate not only facilitates hydrogen evolution initiation but also has a significant promoting effect in the medium current density region.

[0113] From Table 2 and Figure 7 As can be seen, compared with the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1, the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 3 exhibits lower HER start-up current density of -10 mA cm⁻¹. -2 At -100 mA cm⁻¹, the potential decreased by approximately 107 mV, while at -100 mA cm⁻¹... -2 The potential also decreased by about 89mV, and at -300mA cm⁻¹ -2 The potential decreased slightly by 20mV, indicating that the introduction of indium nitrate not only significantly reduced the cathode potential required to reach the target hydrogen evolution current at low current densities, but also maintained a promoting effect over a wide range of current densities.

[0114] From Table 2 and Figure 8 As can be seen, compared with the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1, the iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer provided in Example 4 exhibits lower HER start-up current density of -10 mA cm⁻¹. -2 At -100mA cm⁻¹, the potential decreased by approximately 84mV, while at -100mA cm⁻¹... -2 The potential also dropped by about 25mV, but at -300mA cm -2 The potential did not decrease further, indicating that the addition of erbium nitrate not only facilitates the initiation of hydrogen evolution, but also has a significant promoting effect in the medium current density region. However, the promoting effect of erbium nitrate tends to weaken in the higher current density range.

[0115] From Table 2 and Figure 9 As can be seen, compared with the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1, the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 5 exhibits lower HER start-up current density of -10 mA cm⁻¹. -2 The potential dropped by approximately 145 mV, and at -100 mA cm⁻¹ -2 and -300mA cm -2 At -300 mA cm⁻¹, the potential also showed a significant decrease, at -300 mA cm⁻¹ -2 Within the current density range, the required potentials are close to 0 V, and the overpotentials are even lower, indicating that the addition of copper salt can significantly reduce the cathode polarization required for the hydrogen evolution reaction at low current densities. This allows the iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer provided in Example 5 to achieve the desired effect at -300 mA cm⁻¹.-2 Significant improvements in HER performance were achieved across the entire current density range.

[0116] The above experiments show that the iron-based alloy hydrogen evolution electrode modified with a composite phosphating layer provided in Comparative Example 1 uses an iron-based alloy as a substrate. A leaf-shaped composite phosphating layer is constructed in situ using a manganese-zinc based phosphating system under stirring at room temperature. Morphological modification on the iron-based alloy surface increases the specific surface area and the number of exposed active sites. While this method can improve the electrode surface roughness and electrolyte contact area, further control of the chemical composition and local electronic structure of the phosphating layer is still needed. In contrast, the iron-based alloy hydrogen evolution electrodes modified with metal salts and modified with composite phosphating layers provided in Examples 1-5 utilize copper salts, erbium salts, indium salts, and molybdenum salts. The iron-based alloy cathode utilizes metal salts such as bismuth salts to modulate the foliated phosphating layer, thereby further optimizing its alkaline hydrogen evolution activity while retaining the original porous structure and substrate bonding advantages of the phosphating layer. Simultaneously, it achieves uniform in-situ growth of the phosphating layer under milder conditions, avoiding the limitations imposed by high-temperature phosphating or strong ultrasonic fields on the equipment and large-area electrodes. Furthermore, the iron-based alloy hydrogen evolution electrodes modified with composite phosphating layers regulated by metal salts provided in Examples 1-5 exhibit different catalytic performances when using different metal salts, showing varying current densities at low and high current densities during HER initiation.

[0117] The selective regulatory effect at different stages provides experimental basis for further screening of promoting metals that balance initiation performance and high current density performance.

[0118] Table 2: Potential of iron-based alloy hydrogen evolution electrode at different current densities

[0119] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode, characterized in that, Includes the following steps: Phosphoric acid, potassium dihydrogen phosphate, trans-cinnamic acid, manganese chloride, and zinc nitrate are added to water and stirred until dissolved to obtain a basic phosphating solution. At least one metal salt selected from copper salt, erbium salt, indium salt, molybdenum salt, and bismuth salt is added to the basic phosphating solution and stirred until dissolved to obtain a metal ion-controlled phosphating solution; The iron-based alloy was immersed in a metal ion-controlled phosphating solution and phosphated at room temperature (20~35℃) with stirring to obtain an iron-based alloy hydrogen evolution electrode modified with a metal salt-controlled composite phosphating layer.

2. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, Each 30 mL of the basic phosphating solution comprises: 3-9 mmol phosphoric acid, 3-9 mmol potassium dihydrogen phosphate, 0.005-0.02 mmol trans-cinnamic acid, 1-5 mmol manganese chloride, and 3-9 mmol zinc nitrate.

3. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, The copper salt is selected from at least one of copper nitrate, copper chloride, copper sulfate, copper acetate, and their hydrates; The erbium salt is selected from at least one of erbium nitrate, erbium chloride, erbium sulfate, erbium acetate, and their hydrates; The indium salt is selected from at least one of indium nitrate, indium chloride, indium sulfate, indium acetate, and their hydrates; The molybdenum salt is selected from at least one of sodium molybdate, potassium molybdate, and ammonium molybdate. The bismuth salt is selected from at least one of bismuth nitrate, bismuth chloride, bismuth sulfate, bismuth acetate, and their hydrates.

4. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, 1-6 mmol of metal salt is added to every 30 mL of the basic phosphating solution.

5. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, The iron-based alloy is a sheet-like iron-based alloy obtained by melting, casting, and cutting elemental raw materials of Fe, Ni, Co, Cr, and Mo in the mass percentages of Fe: 55~85%, Ni: 10~20%, Co: 5~15%, Cr: 2.5~3.5%, and Mo: 0.5~1.5%.

6. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, The iron-based alloy is selected from iron-based alloys that have been successively polished, cleaned, and dried.

7. The method for preparing a metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode according to claim 1, characterized in that, The stirring speed for phosphating is 200~1000 rpm, and the phosphating time is 8~24h.

8. A metal salt-controlled composite phosphating layer modified iron-based alloy hydrogen evolution electrode, characterized in that, It is prepared by the preparation method according to any one of claims 1-7.

9. The application of the iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer as described in claim 8 in the field of hydrogen production by water electrolysis.

10. An alkaline electrolytic cell, characterized in that, The cathode is selected from the iron-based alloy hydrogen evolution electrode modified with a metal salt-regulated composite phosphating layer as described in claim 8, and the alkaline electrolyte is selected from 0.5~1.5 MkOH electrolyte.