NiZnFe-Ni-C / C self-supporting cathode electrode material and preparation method thereof

By growing Ni, Zn, and Fe catalytic components in situ on a nickel transition layer C/C substrate, the problems of insufficient adhesion of coated electrodes and high cost of precious metals were solved. This achieved a strong bond between the catalytic layer and the substrate, reduced dependence on precious metals, improved electrocatalytic activity, and simplified the preparation process.

CN123153102APending Publication Date: 2026-11-24XIAN CHAOMA SCI TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611466871.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing coated electrodes suffer from insufficient adhesion, high cost of precious metals, and difficulty in uniformly loading multi-component non-precious metal catalytic components.

Method used

A self-supporting cathode electrode material, NiZnFe-Ni-C/C, is used. By growing Ni, Zn, and Fe catalytic components in situ on the nickel transition layer C/C substrate, binders are avoided. Urea is used to control the morphology of the catalytic layer and the dispersion of alcohol solvent, simplifying the preparation process and forming an integrated structure.

Benefits of technology

It achieves a strong bond between the catalyst layer and the substrate, reduces dependence on precious metals, enhances electrocatalytic activity, simplifies the preparation process and reduces costs, and is suitable for hydrogen production by water electrolysis in alkaline solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153102A_ABST
    Figure CN123153102A_ABST
Patent Text Reader

Abstract

This invention discloses a NiZnFe-Ni-C / C self-supporting cathode electrode material and its preparation method. The preparation method includes the following steps: dissolving nickel salt, zinc salt, iron salt, and urea in an alcohol solvent to obtain a mixed solution; pretreating a porous carbon / carbon composite matrix with a nickel transition layer on its surface by degreasing and deoxide removal; completely immersing the matrix in the mixed solution; and conducting a hydrothermal reaction at 150–200°C for 5–20 hours in a sealed reactor to form a catalytic layer of Ni, Zn, and Fe components in situ on the surface of the Ni-C / C matrix; after the reaction, cleaning and drying are performed to obtain the self-supporting NiZnFe-Ni-C / C cathode electrode. This method is simple, operates under mild conditions, requires no binder, and the resulting electrode exhibits good hydrogen evolution activity in alkaline electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional materials and electrocatalysis technology, specifically relating to a NiZnFe-Ni-C / C self-supporting cathode electrode material and its preparation method. Background Technology

[0002] Hydrogen energy, as a clean energy source, has advantages such as high energy density, clean and renewable nature, green environmental protection, and flexible storage and transportation. It is regarded as an ideal clean alternative energy source and can reduce carbon emissions.

[0003] In the electrocatalytic water splitting hydrogen production system, the introduction of a catalyst can change the electron transfer path and reaction energy barrier in the electrocatalytic hydrogen evolution process, effectively reducing the reaction overpotential and improving the energy efficiency of water electrolysis for hydrogen production.

[0004] Precious metal catalysts such as Pt and Ru have shown excellent performance in the field of water electrolysis for hydrogen production, but their high price limits the large-scale application of water electrolysis for hydrogen production technology. Therefore, there is an urgent need to develop efficient non-precious metal catalysts.

[0005] Transition metals (such as Fe, Co, Ni, Mo, and W) possess unique d-electron structures, facilitating electron transfer and transport during reactions and enabling the formation of diverse coordination modes. These metals exhibit high intrinsic catalyst activity and are therefore widely used as highly efficient non-noble metal catalysts for hydrogen production via water electrolysis. Furthermore, nanostructured catalysts formed by heteroatom doping, supported on highly conductive and high specific surface area substrates, further enhance catalyst performance.

[0006] Against this backdrop, various potential supporting materials, such as porous carbon / graphene, carbon cloth, and metal foam, have been widely used to support catalysts with nanostructures of different dimensions. The synergistic effects between materials, self-supporting structures, and multi-metal composites significantly increase the number of active sites and the electron / charge transfer rate, thereby promoting the hydrogen evolution reaction (HER) kinetics. Furthermore, the design of nanocomposite materials can prevent the aggregation of active sites and ensure the stability of the catalyst throughout the reaction process. Therefore, synthesizing catalysts with multi-metal nanostructures supported on conductive substrates to form novel HER electrode materials and enhancing catalyst activity is one of the effective strategies for achieving highly efficient catalysis.

[0007] In the prior art, CN114182280B discloses a MEC hydrogen evolution cathode made by forming a suspension of Ni-SAPO-34 composite material and drop-coating it onto carbon paper. Its catalyst layer relies on coating and bonding, limiting the bonding between the catalyst and the substrate and its long-term stability. CN119050378B discloses a non-precious metal membrane electrode with variable contact angle formed by changing the ionomer content, belonging to the membrane electrode structure of fuel cells, requiring the setting of a proton exchange membrane and multiple catalyst layers. None of the above solutions disclose the closed-loop hydrothermal in-situ growth of the Ni, Zn, and Fe ternary components on a nickel transition layer C / C substrate used in this invention, nor do they provide the combination of precursor concentration, urea control, and hydrothermal window.

[0008] Therefore, existing technologies still require a method for preparing a self-supporting cathode electrode that requires no binder, has a simple process, a strong bond between the catalyst layer and the conductive substrate, and exhibits good alkaline hydrogen evolution performance. Summary of the Invention

[0009] The technical problem this invention aims to solve is to provide a NiZnFe-Ni-C / C self-supporting cathode electrode material and its preparation method, thereby addressing the issues of insufficient adhesion of existing coated electrodes, high cost of precious metals, and difficulty in uniformly loading multi-component non-precious metal catalytic components. This method is simple to operate, has a controllable structure, mild conditions, a short preparation cycle, and low cost. Testing has shown that it exhibits excellent electrocatalytic activity in water electrolysis for hydrogen production in alkaline solution.

[0010] To solve the above-mentioned technical problems, according to a first aspect of the present invention, a method for preparing a NiZnFe-Ni-C / C self-supporting cathode electrode material is proposed, comprising the following steps: S1, nickel salt, zinc salt, iron salt and urea are added to an alcohol solvent and stirred at room temperature to obtain a mixed solution; S2, the porous C / C composite matrix with a nickel transition layer on the surface is subjected to ultrasonic pretreatment with acetone and hydrochloric acid, then completely immersed in the mixed solution, and hydrothermally reacted in a closed reactor at 150-200℃ for 5-20h, so that Ni, Zn and Fe catalytic components grow in situ on the surface of the Ni-C / C matrix. S3. After cooling, the sample was removed, and then washed and dried alternately with deionized water and ethanol to obtain a NiZnFe-Ni-C / C self-supporting cathode electrode.

[0011] Preferably, the molar concentrations of nickel salt, zinc salt, and iron salt metal ions are 0.01–0.05 mol / L, 0.01–0.05 mol / L, and 0.005–0.05 mol / L, respectively, and the molar concentration of urea is 0.02–0.10 mol / L; the alcohol solvent is methanol, anhydrous ethanol, or isopropanol; and the magnetic stirring time is 20–50 min.

[0012] Preferably, the nickel salt in step S1 is selected from one or more of nickel chloride hexahydrate, nickel nitrate hexahydrate, and nickel acetate tetrahydrate; the zinc salt is selected from one or more of zinc nitrate hexahydrate, zinc acetate dihydrate, and zinc chloride hexahydrate; and the iron salt is selected from one or more of ferric chloride hexahydrate, ferric nitrate nonahydrate, and ferric sulfate.

[0013] Preferably, the alcohol solvent in step S1 is selected from methanol, anhydrous ethanol or isopropanol; the stirring is magnetic stirring at room temperature for 20 to 50 minutes.

[0014] Preferably, in step S2, the ultrasonic treatment time with acetone is 3-10 min, and the ultrasonic treatment time with hydrochloric acid is 3-10 min, in order to remove oil and oxides from the surface of the Ni-C / C substrate.

[0015] Preferably, the hydrothermal reaction temperature in step S2 is 165–175°C, and the reaction time is 10–14 h.

[0016] Preferably, in step S3, deionized water and ethanol are used alternately for washing 2 to 4 times, followed by natural drying at room temperature for 15 to 30 hours.

[0017] Preferably, the Ni-C / C matrix is ​​prepared by the following method: oxidizing the porous C / C composite material at 450°C for 10–20 min, then oxidizing it in a 15–25% nitric acid solution for 20–40 min, ultrasonically cleaning it with deionized water, and drying it; spraying a 0.20–0.40 mol / L nickel chloride hexahydrate solution onto the treated porous C / C composite material, freeze-drying it, and then reducing it at 500–600°C for 1–3 h in a hydrogen atmosphere to form a nickel transition layer.

[0018] According to a second aspect of the present invention, a NiZnFe-Ni-C / C material for a cathode electrode used in alkaline water hydrogen production is provided, which is prepared by the above-described preparation method. The material is an integrated structure of NiZnFe multi-component catalytic components and Ni-C / C self-supporting conductive matrix.

[0019] Preferably, in an alkaline electrolyte at room temperature, at 5000 A / m 2 At the given current density, the hydrogen evolution overpotential of the cathode electrode is no higher than 436 mV.

[0020] This invention has the following advantages: it employs a ternary non-precious metal synergistic catalytic component of Ni, Zn, and Fe, reducing dependence on precious metals; it uses a Ni-C / C self-supporting matrix and hydrothermal in-situ growth, avoiding additional binders and improving electron transport and catalyst layer bonding; it regulates the morphology and coverage uniformity of the catalyst layer through urea slow-release precipitation and alcohol solvent dispersion; the process requires only a conventional reactor and a forced-air drying oven, with moderate reaction temperature and cycle time, suitable for scale-up preparation; and it operates at 5000 A / m 2The hydrogen evolution overpotential can reach 436mV at current density (without compensation). Attached Figure Description

[0021] Figure 1 This is a scanning electron microscope image of the NiZnFe-Ni-C / C electrode material prepared in Example 2 of the present invention; Figure 2 The polarization curve of the NiZnFe-Ni-C / C electrode material prepared in Example 2 of this invention under alkaline conditions; Figure 3 The polarization curve of the Ni-C / C matrix prepared in Comparative Example 1 of this invention under alkaline conditions is shown. Detailed Implementation

[0022] The present invention will be further described below with reference to the embodiments. It should be noted that the following embodiments are used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention; equivalent substitutions for salts, alcohol solvents, cleaning methods and reaction parameters without departing from the concept of the present invention are all within the scope of the present invention.

[0023] Preparation steps: Step S1: Preparation of the mixed solution: Weigh nickel salt, zinc salt, iron salt, and urea sequentially into a glass container, add alcohol solvent, and stir with a magnetic stirrer at room temperature for 20–50 min until homogeneous, forming a mixed solution containing Ni, Zn, Fe precursors and urea. The slow decomposition of urea during the hydrothermal process regulates the local precipitation rate, which is beneficial for the uniform nucleation of the multi-component catalytic components.

[0024] Step S2, Pretreatment and Hydrothermal In-situ Growth: The Ni-C / C substrate is sequentially placed in acetone and hydrochloric acid and sonicated for 3-10 min to remove surface oil and oxides; the pretreated substrate is then completely immersed in the mixed solution from Step S1, the reactor is sealed, and the reaction is carried out at 150-200℃ for 5-20 h. The Ni-C / C substrate is a substrate for a porous C / C composite material with a nickel transition layer modified on its surface. The nickel transition layer provides a conductive framework and nucleation interface, and Ni, Zn, and Fe components grow in situ on its surface to form an integrated catalytic layer.

[0025] Step S3, Cleaning and Drying: After the reaction is complete and cooled to room temperature, take out the sample and wash it 2 to 4 times with deionized water and ethanol alternately to remove residual salts and organic matter. Then, let it air dry at room temperature for 15 to 30 hours to obtain the NiZnFe-Ni-C / C cathode electrode.

[0026] Preparation of Ni-C / C matrix: The porous C / C composite material was oxidized at 450℃ for 10–20 min, then oxidized in a 15–25% nitric acid solution for 20–40 min, ultrasonically cleaned with deionized water, and dried at 120℃ for 20–30 h. A 0.20–0.40 mol / L nickel chloride hexahydrate solution was uniformly sprayed onto the treated porous C / C composite material, first freeze-dried at -60℃ for approximately 24 h, and then reduced at 500–600℃ for 1–3 h under a hydrogen atmosphere to form a Ni-C / C matrix with a nickel transition layer on the surface.

[0027] Comparative Example 1 This comparative example presents a method for preparing a Ni-C / C matrix, which includes the following steps: Step S1, matrix roughening treatment: The porous carbon / carbon composite material is pre-oxidized at 450℃ for 15 min, then acid-washed in 20wt.% nitric acid solution for 30 min, then ultrasonically cleaned with deionized water, and then dried in an oven at 120℃ for 24 h to obtain the roughened porous carbon / carbon (C / C) composite material.

[0028] Step S2, Ni transition layer preparation: A 0.30 mol / L NiCl2·6H2O solution was uniformly sprayed onto the roughened porous carbon / carbon composite material obtained in step S1. Then, it was first transferred to a freeze dryer and freeze-dried at -60℃ for 24 h. Then, it was transferred to a reduction furnace and reacted at 550℃ for 2 h under H2 atmosphere to obtain the Ni-C / C matrix.

[0029] Example 1 Weigh 0.15 g of nickel chloride hexahydrate, 0.14 g of zinc acetate dihydrate, 0.08 g of ferric chloride hexahydrate, and 0.07 g of urea, add 60 mL of methanol, and stir magnetically at room temperature for 30 min. Transfer the mixture to a reaction vessel, add the pretreated Ni-C / C matrix and completely immerse it, seal, and hydrothermally react at 170 °C for 12 h. After cooling to room temperature, remove the vessel, wash it three times alternately with deionized water and ethanol, and dry it at room temperature for 25 h to obtain the NiZnFe-Ni-C / C cathode electrode.

[0030] Example 2 Weigh 0.36 g of nickel chloride hexahydrate, 0.33 g of zinc acetate dihydrate, 0.10 g of ferric chloride hexahydrate, and 0.18 g of urea, add 60 mL of methanol, and stir magnetically at room temperature for 30 min. Prepare a NiZnFe-Ni-C / C cathode electrode according to the pretreatment, hydrothermal, cleaning, and drying steps described in Example 1. Scanning electron microscopy showed that the electrode surface exhibited a nanosheet-like porous morphology. Three-electrode polarization testing was performed in an alkaline electrolyte at 5000 A / m. 2 The hydrogen evolution overpotential at the current density is 436mV (without compensation).

[0031] SEM image of the NiZnFe-Ni-C / C electrode material prepared in Example 2 is shown below. Figure 1 As shown, from Figure 1 It can be seen that the surface of the NiZnFe-Ni-C / C sample is entirely composed of nanosheets. The polarization curve of the NiZnFe-Ni-C / C electrode material prepared in Example 2 under alkaline conditions is shown below. Figure 2 As shown, from Figure 2 It can be seen that NiZnFe-Ni-C / C at 5000 A / m 2 At the given current density, the hydrogen evolution overpotential at room temperature is 436 mV.

[0032] Example 3 Weigh 0.70 g of nickel chloride hexahydrate, 0.65 g of zinc acetate dihydrate, 0.16 g of ferric chloride hexahydrate, and 0.36 g of urea, add 60 mL of methanol, and stir for 30 min. React hydrothermally at 170 °C for 12 h, wash three times, and dry at room temperature for 25 h to obtain a NiZnFe-Ni-C / C cathode electrode. This example is used to verify the effect of increasing the precursor feed amount on the catalyst layer coverage and electrode current response.

[0033] Example 4 Using the same precursor feed and solvent system as in Example 2, the hydrothermal temperature was adjusted to 150°C and the reaction time to 15 h. The mixture was washed three times and dried at room temperature for 30 h. This example was used to verify the effectiveness of catalyst layer formation at a lower hydrothermal temperature and a longer reaction time.

[0034] Comparison of proportions and effects The comparative example used a Ni-C / C matrix without NiZnFe hydrothermal in-situ growth. The porous C / C composite material was first oxidized at 450℃ for 15 min, then oxidized in 20 wt.% nitric acid for 30 min, followed by cleaning and drying to achieve surface roughening. A 0.30 mol / L nickel chloride hexahydrate solution was sprayed onto the composite, followed by freeze-drying for 24 h, and then reduction at 550℃ for 2 h under a hydrogen atmosphere to obtain the Ni-C / C matrix. Figure 2 , Figure 3 As shown, at 5000A / m 2 Under current density and room temperature conditions, the hydrogen evolution overpotential of the Ni-C / C matrix was 518 mV (without compensation), which was higher than 436 mV in Example 2, indicating that the hydrothermal in-situ composite of the NiZnFe multi-component catalytic component and the Ni-C / C self-supporting matrix can significantly improve the hydrogen evolution activity of the electrode.

[0035] Examples 1-4 demonstrate that, within the range of precursor concentration, alcohol solvent, hydrothermal temperature, and reaction time specified in the claims, a continuous NiZnFe catalytic layer can be formed on the Ni-C / C substrate. The nanosheet-like structure formed at 170℃ for 12 hours combines catalytic layer coverage with mass transfer channels, achieving an electrochemically active area of ​​10.76 mF / cm². 2 It exhibits superior overall hydrogen evolution performance. The main reason is that in the hydrothermal system, the ion migration and precursor hydrolysis nucleation rate are significantly enhanced at an appropriate high temperature, which can quickly form nanocatalyst materials with moderate crystallinity and good dispersibility. At the same time, it constructs an interconnected and open pore structure, reducing the embedding of active sites caused by particle agglomeration. The appropriate high temperature environment facilitates the generation of lattice defects and target active phases that are beneficial to catalysis, and removes surface adsorbed impurities. The short holding time can effectively inhibit excessive grain growth, ultimately obtaining a higher electrochemical active area.

[0036] The preparation method described in this invention can also be used for Ni-C / C substrates of different areas and shapes. The catalyst loading can be adjusted by modifying the volume of the mixed solution, the substrate size, and the precursor concentration; the morphology and pore structure of the catalyst layer can be adjusted by changing the hydrothermal time and urea concentration. These modifications do not affect the technical concept of this invention: the in-situ growth of a self-supporting alkaline hydrogen evolution cathode on the surface of a Ni-C / C substrate using NiZnFe multi-component components.

[0037] Matters not covered in this invention are common knowledge to those skilled in the art. All equivalent substitutions, simple modifications, or improvements made within the spirit and principles of this invention should be included within the scope of protection of the claims of this invention.

Claims

1. A method for preparing a NiZnFe-Ni-C / C cathode electrode material for alkaline water hydrogen production, characterized in that, Includes the following steps: S1. Nickel salt, zinc salt, iron salt, and urea are sequentially added to an alcohol solvent and stirred at room temperature to form a homogeneous mixed solution; S2. The Ni-C / C matrix, which has been ultrasonically pretreated with acetone and hydrochloric acid respectively, is completely immersed in the mixed solution and subjected to a hydrothermal reaction at 150-200°C for 5-20 hours in a sealed reactor to allow the catalytic components containing nickel, zinc, and iron to grow in situ on the surface of the Ni-C / C matrix; S3. After the reaction is completed and cooled to room temperature, the matrix is ​​removed, and it is cleaned alternately with deionized water and ethanol and dried to obtain a NiZnFe-Ni-C / C cathode electrode; wherein, the Ni-C / C matrix is ​​a self-supporting conductive matrix with a nickel transition layer on the surface of a porous C / C composite material.

2. The preparation method according to claim 1, characterized in that, In step S1, the molar concentrations of metal ions in the nickel salt, zinc salt, and iron salt are 0.01–0.05 mol / L, 0.01–0.05 mol / L, and 0.005–0.05 mol / L, respectively, and the molar concentration of urea is 0.02–0.10 mol / L.

3. The preparation method according to claim 1, characterized in that, The nickel salt in step S1 is selected from one or more of nickel chloride hexahydrate, nickel nitrate hexahydrate, and nickel acetate tetrahydrate; the zinc salt is selected from one or more of zinc nitrate hexahydrate, zinc acetate dihydrate, and zinc chloride hexahydrate; and the iron salt is selected from one or more of ferric chloride hexahydrate, ferric nitrate nonahydrate, and ferric sulfate.

4. The preparation method according to claim 1, characterized in that, The alcohol solvent in step S1 is selected from methanol, anhydrous ethanol or isopropanol; the stirring is magnetic stirring at room temperature for 20 to 50 minutes.

5. The preparation method according to claim 1, characterized in that, In step S2, the ultrasonic treatment with acetone lasts for 3 to 10 minutes, and the ultrasonic treatment with hydrochloric acid lasts for 3 to 10 minutes, in order to remove oil and oxides from the surface of the Ni-C / C substrate.

6. The preparation method according to claim 1, characterized in that, In step S2, the hydrothermal reaction temperature is 150–200℃, and the reaction time is 5–20 h.

7. The preparation method according to claim 1, characterized in that, In step S3, wash with deionized water and ethanol alternately 2 to 4 times, and then air dry at room temperature for 15 to 30 hours.

8. The preparation method according to claim 1, characterized in that, The Ni-C / C matrix is ​​prepared by the following method: the porous C / C composite material is oxidized at 450°C for 10-20 min, then oxidized in a nitric acid solution with a mass fraction of 15-25% for 20-40 min, ultrasonically cleaned with deionized water, and dried; a 0.20-0.40 mol / L nickel chloride hexahydrate solution is sprayed onto the treated porous C / C composite material, freeze-dried, and then reduced at 500-600°C for 1-3 h in a hydrogen atmosphere to form a nickel transition layer.

9. A NiZnFe-Ni-C / C material for a cathode electrode used in alkaline water hydrogen production, characterized in that, The material is prepared by the preparation method according to any one of claims 1 to 8, and the material is an integrated structure of NiZnFe multi-component catalytic components and Ni-C / C self-supporting conductive matrix.

10. The NiZnFe-Ni-C / C cathode electrode material for alkaline water hydrogen production according to claim 9, characterized in that, In an alkaline electrolyte at room temperature, 5000 A / m 2 At the given current density, the hydrogen evolution overpotential of the cathode electrode is no higher than 436 mV.

Citation Information

Patent Citations

  • Variable contact angle non-noble metal-based film electrode and preparation method and application thereof

    CN119050378B