A heterojunction catalyst MnS / Ni3S2 / NF, its preparation method, and its application in the electrocatalytic oxidation of furfural.
By in-situ growing Ni₃S₂ nanosheets and MnS nanoparticles on a nickel foam substrate to form a heterojunction catalyst MnS/Ni₃S₂/NF, the problem of insufficient active sites in single-component catalysts was solved, and the activity and stability of furfural oxidation were improved.
Patent Information
- Application Number
- CN202611484293.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing single-component catalysts have insufficient active sites in the electrocatalytic conversion of furfural, resulting in low efficiency. There is an urgent need to develop heterojunction catalysts that combine high activity and high stability.
A one-step hydrothermal method was used to grow Ni₃S₂ nanosheets and MnS nanoparticles in situ on a nickel foam substrate to form a heterojunction catalyst MnS/Ni₃S₂/NF, with urea used to regulate the morphology and provide an alkaline environment.
It significantly improved the oxidation activity and stability of furfural, reduced the overpotential, and enhanced the electron transfer rate and the abundance of active sites.
Smart Images

Figure CN123153104A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrocatalyst technology, specifically relating to a heterojunction catalyst MnS / Ni3S2 / NF, its preparation method, and its application in the electrocatalytic oxidation of furfural. Background Technology
[0002] Grain by-product resources are relatively abundant. Among them, furfural and 5-hydroxymethylfurfural compounds from pyrolysis volatiles are listed as the top ten biomass platform molecules, which can be used to derive a series of high-value-added chemicals, such as furoic acid, furfuryl alcohol, 2,5-furandicarboxylic acid, and 2,5-dicarboxyfuran. Their derivatives are widely used in polymer materials, fine chemicals, pharmaceuticals, and agriculture, showing broad application prospects. Traditional catalytic conversion processes usually rely on harsh conditions such as high temperature and high pressure, while electrocatalysis technology can operate efficiently at ambient temperature and pressure, demonstrating significant application potential. Notably, furfural can undergo selective oxidation (FOR) at the anode of the electrolytic cell, and can also undergo hydrogenation or couple with hydrogen evolution reaction at the cathode, thereby improving energy utilization efficiency and synergistically generating high-value-added products, which has important research significance and application value.
[0003] Achieving efficient electrocatalytic conversion of furfural urgently requires the development of catalytic materials that combine high activity and high stability. Previous studies have shown that catalysts based on nickel foam exhibit good structural stability. Nickel (Ni) and manganese (Mn), as typical transition metal elements, have been extensively explored in the field of electrocatalysis. However, single-component catalysts often suffer from insufficient active sites, while constructing heterojunction catalysts can fully leverage the synergistic advantages of each component, significantly improving electrocatalytic performance. Therefore, there is an urgent need to design and develop novel heterojunction catalysts to achieve efficient electrocatalytic conversion of furfural. Summary of the Invention
[0004] To address the problem of insufficient active sites in existing single-active-component electrocatalytic furfural oxidation catalysts, the present invention aims to provide a heterojunction catalyst MnS / Ni3S2 / NF, its preparation method, and its application in electrocatalytic furfural oxidation.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A heterojunction catalyst MnS / Ni3S2 / NF is provided, wherein the catalyst is based on NF (nickel foam), and Ni3S2 (nickel disulfide) nanosheets and MnS (manganese sulfide) nanoparticle heterojunctions are grown in situ on the substrate.
[0006] A method for preparing the heterojunction catalyst MnS / Ni3S2 / NF, comprising the following steps: (1) After cutting the nickel foam, pickle and dry it for later use; (2) Mix the nickel salt, manganese salt, sulfur source, urea and water together to obtain a mixed solution; (3) Transfer the nickel foam obtained in step (1) and the mixed solution obtained in step (2) to the hydrothermal reaction device and immerse the nickel foam in the mixed solution. Seal the hydrothermal reaction device and perform hydrothermal reaction at 120~260℃ for 5~25h. (4) After the reaction in step (3) is completed, cool naturally to room temperature, remove the nickel foam, dry it, and the target catalyst is obtained; Among them, the nickel salt is calculated based on the nickel element provided, the manganese salt is calculated based on the manganese element provided, and the sulfur source is calculated based on the sulfur element provided: the raw material usage ratio is nickel salt: manganese salt: sulfur source: urea: water = (0.5~3.5) mmol: (0.5~3.5) mmol: (1~6) mmol: (6~18) mmol: (15~35) mL, and the total molar sum of nickel salt and manganese salt is 4 mmol; in step (3), the area of the foamed nickel is 1~5 cm². 2 / 4mmol (nickel salt + manganese salt).
[0007] Preferably, the nickel salt is nickel nitrate, nickel sulfate, or nickel acetate.
[0008] Preferably, the manganese salt is manganese sulfate, manganese acetate, or manganese nitrate.
[0009] Preferably, the sulfur source is thiourea.
[0010] Application of the heterojunction catalyst MnS / Ni3S2 / NF in the electrocatalytic high-efficiency furfural oxidation.
[0011] In this invention, urea is used to regulate morphology and provide an alkaline environment.
[0012] Beneficial effects: This invention uses a one-step hydrothermal method to prepare the heterojunction catalyst MnS / Ni3S2 / NF. The process is simple, economical and practical, with high stability, and exhibits excellent electrocatalytic furfural oxygenation activity. Attached Figure Description
[0013] Figure 1 XRD patterns of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention, the Ni3S2 / NF catalyst prepared in Comparative Example 1, and the MnS / NF catalyst prepared in Comparative Example 2.
[0014] Figure 2 SEM image of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention.
[0015] Figure 3 TEM image of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention.
[0016] Figure 4 Diagram of the electrochemical testing apparatus and LSV linear sweep voltammetry curves of the catalysts in Example 4 and Comparative Examples 1-2.
[0017] Figure 5 Cyclic stability test diagram of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention. Detailed Implementation
[0018] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described below in conjunction with specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the described embodiments, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.
[0019] Example 1
[0020] A method for preparing an electrocatalyst MnS / Ni3S2 / NF, comprising the following steps: (1) Cut the nickel foam into pieces with an area of 3cm². 2 Afterwards, it is pickled and dried using conventional techniques for later use; (2) Add 0.5 mmol nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 3.5 mmol manganese sulfate monohydrate (MnSO4·H2O), 3 mmol thiourea and 9 mmol urea to 20 mL of deionized water and stir well to obtain a mixed solution. (3) Transfer the mixed solution from step (2) to the hydrothermal reactor, and at the same time place the nickel foam from step (1) into the hydrothermal reactor, tighten the reactor lid, and transfer the hydrothermal reactor to the oven; (4) Set the oven heating temperature to 170℃ and the heating time to 12h; (5) Cool the oven to room temperature, open the kettle, take out the foamed nickel, and dry the resulting solid, which is the target catalyst.
[0021] Example 2 The difference from Example 1 is that in step (2), the amount of nickel nitrate hexahydrate is changed to 1 mmol and the amount of manganese sulfate monohydrate is changed to 3 mmol; everything else is the same as in Example 1.
[0022] Example 3 The difference from Example 1 is that in step (2), the amount of nickel nitrate hexahydrate is changed to 2 mmol and the amount of manganese sulfate monohydrate is changed to 2 mmol; all other steps are the same as in Example 1.
[0023] Example 4 The difference from Example 1 is that in step (2), the amount of nickel nitrate hexahydrate is changed to 3 mmol and the amount of manganese sulfate monohydrate is changed to 1 mmol; all other steps are the same as in Example 1.
[0024] Example 5 The difference from Example 1 is that in step (2), the amount of nickel nitrate hexahydrate is changed to 3.5 mmol and the amount of manganese sulfate monohydrate is changed to 0.5 mmol; all other steps are the same as in Example 1.
[0025] Example 6 The difference from Example 1 is that in step (4), the oven temperature is changed to 240°C; everything else is the same as in Example 1.
[0026] Example 7 The difference from Example 1 is that in step (4), the heating time is set to 20h; everything else is the same as in Example 1.
[0027] Compare with Example 1 The difference from Example 4 is that in step (2), the amount of nickel nitrate hexahydrate is 4 mmol and the amount of manganese sulfate monohydrate is 0; everything else is the same as in Example 4.
[0028] The catalyst prepared in this comparative example is Ni3S2 / NF.
[0029] Compare with Example 2 The difference from Example 4 is that in step (2), the amount of nickel nitrate hexahydrate is 0 mmol and the amount of manganese sulfate monohydrate is 4 mmol; all other aspects are the same as in Example 4.
[0030] The catalyst prepared in this comparative example is MnS / NF.
[0031] Compare with Example 3 The difference from Example 4 is that in step (2), the amount of nickel nitrate hexahydrate is 3 mmol, and manganese sulfate monohydrate is replaced with cobalt sulfate heptahydrate (CoSO4·7H2O), with the amount still being 1 mmol; everything else is the same as in Example 4.
[0032] The catalyst prepared in this comparative example is CoS2 / Ni3S2 / NF.
[0033] Compare with Example 4 The difference from Example 4 is that in step (2), the amount of nickel nitrate hexahydrate is 3 mmol, and manganese sulfate monohydrate is replaced with chromium sulfate pentahydrate (Cr2(SO4)3·15H2O) with an amount of 0.5 mmol; all other aspects are the same as in Example 4.
[0034] The catalyst prepared in this comparative example is CrS2 / Ni3S2 / NF.
[0035] Compare with Example 5 The difference from Example 4 is that in step (2), 9 mmol of urea is replaced with 9 mmol of ammonium chloride; everything else is the same as in Example 4.
[0036] The catalyst prepared in this comparative example is MnS / Ni3S2 / NF-NH4Cl.
[0037] Catalyst characterization Figure 1 The images show the XRD patterns of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention, the Ni3S2 / NF catalyst prepared in Comparative Example 1, and the MnS / NF catalyst prepared in Comparative Example 2. Figure 1 As can be seen from the comparison with the standard card, the product prepared in Example 4 of this invention is MnS / Ni3S2 / NF, the product prepared in Comparative Example 1 is Ni3S2 / NF, and the product prepared in Comparative Example 2 is MnS / NF. At the same time, the peak of Ni3S2 can be clearly observed in the MnS / Ni3S2 / NF catalyst, but no obvious peak of MnS is observed, indicating that the content of MnS generated is low.
[0038] Figure 2 SEM images of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention at different magnifications. Figure 2 The porous structure of the nickel foam is clearly visible, and Ni3S2 nanosheets and MnS nanoparticles are also loaded on the nickel foam.
[0039] Figure 3 This is a TEM image of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention. Figure 3 It can be seen that the heterogeneous interface between MnS and Ni3S2 can be clearly observed.
[0040] Catalyst evaluation The electrochemical tests described in items (i) and (ii) below were performed using an RST electrochemical workstation. An H-type electrolytic cell was used, consisting of two cells, A and B, separated by an ion-exchange membrane. Cell A contained the working electrode and reference electrode, while cell B contained the counter electrode. The prepared catalyst was prepared according to a nickel foam area of 1 cm². 2 The electrode is cut to size, with the reference electrode being a silver / silver chloride electrode and the counter electrode being a stone rod.
[0041] (a) The catalysts prepared in Examples 1-7 and Comparative Examples 1-5 after trimming were used as working electrodes respectively. 20 mL of 1M KOH electrolyte was added to two electrolytic cells A and B, and 1 mmol of furfural (FF) was added to electrolytic cell A. The test voltage was 1-2V. Figure 4The diagram shows the electrochemical testing setup and the LSV linear sweep voltammetry curves for the catalysts of Example 2 and Comparative Examples 1-2, with a scan rate of 20 mV / s. The current density was 100 mA / cm². -2 The corresponding overpotential test results for furfural oxidation are shown in Table 1. Table 1 shows that compared with pure Ni3S2 / NF and MnS / NF catalysts, the overpotential for furfural oxidation of the MnS / Ni3S2 / NF catalysts prepared in Examples 1-7 of this invention is significantly lower. This indicates that after the formation of Ni3S2 / NF and MnS / NF heterojunctions, the catalysts of this invention significantly improve the furfural oxidation activity due to the increased active surface area and accelerated electron transfer. The overpotentials of CoS2 / Ni3S2 / NF in Control Example 3 and CrS2 / Ni3S2 / NF in Control Example 4 are relatively high, mainly because under furfural oxidation conditions, the valence state of Mn can be... 2+ / Mn 3+ / Mn 4+ The rapid conversion between these states provides abundant redox active sites, while the oxidation state range of Co and Cr is relatively narrow. In Control Example 5, urea in the hydrothermal process was replaced with ammonium chloride. Due to the rapid decomposition of ammonium chloride, it leads to agglomerated and dense structures. In addition, Cl... - It can poison the active sites, leading to a decrease in the oxidation performance of furfural.
[0042]
[0043] (ii) The modified catalyst of Example 4 was used as the working electrode. 20 mL of 1M KOH electrolyte was added to two electrolytic cells A and B. 1 mmol of furfural (FF) was added to electrolytic cell A. The test voltage was 1.50 V. The electrolyte was replaced every 2 hours. A total of six cycles of stability test were performed.
[0044] Figure 5 The figure shows the cycle stability test results for the catalyst in Example 4. Based on the results of six cycles, it can be seen that the six stage curves of the MnS / Ni3S2 / NF catalyst prepared in Example 4 of this invention show relatively small changes, indicating that the catalyst of this invention has good stability after forming the Ni3S2 / NF and MnS / NF heterojunction.
Claims
1. A heterojunction catalyst MnS / Ni3S2 / NF, characterized in that: The catalyst is based on NF, on which Ni3S2 nanosheets and MnS nanoparticle heterojunctions are grown in situ.
2. A method for preparing the heterojunction catalyst MnS / Ni3S2 / NF as described in claim 1, characterized in that, The preparation steps are as follows: (1) After cutting the nickel foam, pickle and dry it for later use; (2) Mix the nickel salt, manganese salt, sulfur source, urea and water together to obtain a mixed solution; (3) Transfer the nickel foam obtained in step (1) and the mixed solution obtained in step (2) to the hydrothermal reaction device and immerse the nickel foam in the mixed solution. Seal the hydrothermal reaction device and perform hydrothermal reaction at 120~260℃ for 5~25h. (4) After the reaction in step (3) is completed, cool naturally to room temperature, remove the nickel foam, dry it, and the target catalyst is obtained; Among them, the nickel salt is calculated based on the nickel element provided, the manganese salt is calculated based on the manganese element provided, and the sulfur source is calculated based on the sulfur element provided: the raw material usage ratio is nickel salt: manganese salt: sulfur source: urea: water = (0.5~3.5) mmol: (0.5~3.5) mmol: (1~6) mmol: (6~18) mmol: (15~35) mL, and the total molar sum of nickel salt and manganese salt is 4 mmol; in step (3), the area of the foamed nickel is 1~5 cm². 2 / 4mmol (nickel salt + manganese salt).
3. The preparation method of the heterojunction catalyst MnS / Ni3S2 / NF as described in claim 2, characterized in that: The nickel salt is nickel nitrate, nickel sulfate, or nickel acetate.
4. The preparation method of the heterojunction catalyst MnS / Ni3S2 / NF as described in claim 2, characterized in that: The manganese salt is manganese sulfate, manganese acetate, or manganese nitrate.
5. The preparation method of the heterojunction catalyst MnS / Ni3S2 / NF as described in claim 2, characterized in that: The sulfur source is thiourea.