Composite diaphragm and preparation method and application thereof

By using a specific amount of pore-forming agent containing ionizable groups in the composite membrane, the problems of easy peeling and uneven distribution of inorganic particles were solved, resulting in lower sheet resistance and higher porosity, thus improving the performance of the water electrolysis hydrogen production device.

CN123153111APending Publication Date: 2026-11-24SHENZHEN CREATOR H2 MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510624303.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing composite membranes suffer from problems such as easy shedding of inorganic particles, uneven distribution, poor hydrophilicity, and high surface resistivity, which affect the service life and safety of water electrolysis hydrogen production devices.

Method used

A coating layer is formed by mixing a pore-forming agent containing ionizable groups with inorganic particles and resin in a specific amount. This process inhibits the aggregation of inorganic particles, promotes their uniform distribution and enriches the microporous structure, and reduces the surface resistivity.

Benefits of technology

It effectively inhibits the shedding of inorganic particles, increases porosity, reduces surface resistivity, enhances ion conductivity, and improves the stability and safety of the membrane in use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention provides a composite membrane, its preparation method, and its application. The composite membrane includes a substrate and a coating layer disposed on at least one surface of the substrate. The coating layer slurry, by weight, comprises 1-25 parts resin, 10-45 parts inorganic particles, and 40-65 parts organic solvent. The coating layer slurry further includes 0.05-4.5 parts pore-forming agent per 100 parts by weight of the organic solvent. The pore-forming agent contains ionizable groups in its molecular structure. This composite membrane solves the problems of existing membranes used in water electrolysis for hydrogen production, such as easy powder shedding, uneven distribution of inorganic particles, poor hydrophilicity, and high sheet resistivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of water electrolysis for hydrogen production technology, specifically relating to a composite membrane, its preparation method, and its application. Background Technology

[0002] The production of renewable hydrogen through water electrolysis is one of the most reliable methods for industrial hydrogen production. The diaphragm is the core component of the water electrolysis device, primarily serving to separate the anode and cathode and to conduct ions. Therefore, the diaphragm generally requires good ion transport capacity, chemical stability, gas barrier properties, and mechanical stability.

[0003] Currently, traditional composite membranes still have the following defects: First, inorganic particles in the coating layer are easy to peel off from the surface of the composite membrane, affecting the service life of the electrolytic cell and even causing more serious safety hazards; Second, the disordered stacking of inorganic particles will also lead to insufficient microporous structure of the membrane, resulting in high sheet resistance; Third, the surface of the membrane is a dense thin layer formed by the phase transformation of resin. Due to the hydrophobicity and poor hydrophilicity of the resin, the sheet resistance is further high.

[0004] Therefore, developing a composite membrane with inorganic particles that are not easily peeled off, good hydrophilicity, and low surface resistance is an urgent problem to be solved in this field. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a composite membrane, its preparation method, and its application. The composite membrane solves the problems of existing membranes used in water electrolysis for hydrogen production, such as easy powder shedding, uneven distribution of inorganic particles, poor hydrophilicity, and high surface resistivity.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a composite membrane, the composite membrane comprising a substrate and a coating layer disposed on at least one surface of the substrate; the coating layer slurry comprises, by weight, 1 to 25 parts of resin, 10 to 45 parts of inorganic particles and 40 to 65 parts of organic solvent, wherein the coating layer slurry further comprises 0.05 to 4.5 parts of a pore-forming agent based on 100 parts by weight of the organic solvent, the pore-forming agent containing ionizable groups in its molecular structure.

[0008] In this invention, a specific amount of a pore-forming agent containing ionizable groups is used. This agent dissolves in water to form a charged compound that can interact with inorganic particles, inhibiting their aggregation and increasing the adhesion between the inorganic particles and the resin. This helps to suppress the peeling of inorganic particles. However, the inventors of this application have found that when the content of the pore-forming agent exceeds a certain level, the repulsive force between molecules in the slurry system will increase, and the optimal effect cannot be achieved. In addition, using a specific amount of a pore-forming agent containing ionizable groups can also promote the uniform distribution of inorganic particles and reduce the sheet resistance. Furthermore, it can also enrich the microporous structure of the membrane, increase the porosity of the membrane, facilitate ion transport, and further reduce the sheet resistance. In addition, the composite membrane also has a high bubble point.

[0009] Secondly, the present invention provides a method for preparing the composite separator described in the first aspect, the method comprising the following steps:

[0010] S1: Mix resin, inorganic particles, pore-forming agent and organic solvent to obtain slurry;

[0011] S2: The slurry obtained in S1 is coated onto at least one surface of the substrate to obtain a coated substrate;

[0012] S3: The coated substrate obtained in S2 is subjected to phase transformation to obtain the composite membrane.

[0013] Thirdly, the present invention provides an alkaline water electrolysis hydrogen production device, wherein the alkaline water electrolysis hydrogen production device includes the composite membrane described in the first aspect.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0015] The composite membrane provided by this invention uses a coating layer containing a specific amount of a pore-forming agent with ionizable groups, which can inhibit the shedding of inorganic particles in the composite membrane, making the inorganic particles uniformly distributed in the composite membrane, enriching the microporous structure of the composite membrane, and increasing the porosity. This not only reduces the sheet resistance of the composite membrane but also improves the ion conductivity of the membrane. In addition, the composite membrane also has a high bubble point. Detailed Implementation

[0016] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0017] The present invention provides a composite membrane, the composite membrane comprising a substrate and a coating layer disposed on at least one surface of the substrate; the coating layer slurry comprises, by weight, 1-25 parts resin, 10-45 parts inorganic particles and 40-65 parts organic solvent, wherein the coating layer slurry further comprises 0.05-4.5 parts pore-forming agent based on 100 parts by weight of organic solvent, the pore-forming agent containing ionizable groups in its molecular structure.

[0018] In this invention, a specific amount of a pore-forming agent containing ionizable groups is used. This agent dissolves in water to form a charged compound that can interact with inorganic particles, inhibiting their aggregation and increasing the adhesion between the inorganic particles and the resin, thereby helping to suppress the peeling of inorganic particles. It can also promote the uniform distribution of inorganic particles and reduce surface resistivity. Furthermore, the use of a pore-forming agent with a specific structure can enrich the microporous structure of the membrane, increase its porosity, facilitate ion transport, and reduce surface resistivity. In addition, the composite membrane also has a high bubble point.

[0019] In this invention, 1 to 25 parts of resin can be, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 25 parts, or any combination thereof.

[0020] In this invention, 10 to 45 parts of inorganic particles can be, for example, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 45 parts, or any combination thereof.

[0021] In this invention, the pore-forming agent, in a mass of 100 parts of organic solvent, is 0.05 to 4.5 parts, for example, 0.05 parts, 0.06 parts, 0.08 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, or any combination thereof.

[0022] In this invention, the content of the pore-forming agent is within the above-mentioned range, which can effectively inhibit the shedding of inorganic particles, making the distribution of inorganic particles more uniform, the pore structure of the composite membrane more abundant, the contact angle of the membrane surface lower, which is more conducive to reducing the surface resistance of the membrane and improving the ion conductivity.

[0023] In this invention, 40 to 65 parts of organic solvent can be, for example, a range of 40 parts, 42 parts, 45 parts, 48 ​​parts, 50 parts, 52 parts, 55 parts, 58 parts, 60 parts, 65 parts, or any two of these.

[0024] Preferably, the ionizable group includes at least one of quaternary ammonium group, primary amine group, secondary amine group, tertiary amine group, carboxyl group or thiol group.

[0025] Preferably, the pore-forming agent comprises at least one of a long-chain alkyl quaternary ammonium salt, branched polyethyleneimine (BPEI), or mercaptopropionic acid (MPA).

[0026] Preferably, the long-chain alkyl quaternary ammonium salt comprises a quaternary ammonium salt with 12 or more alkyl carbon atoms (for example, it can be a range of 12, 13, 14, 15, 16, 17, 18, 19, 20 or any two of these).

[0027] Preferably, the long-chain alkyl quaternary ammonium salt comprises hexadecyltrimethylammonium bromide (CTAB).

[0028] In this invention, CTAB has charged long-chain molecules, which can play a role in steric repulsion on the one hand, and increase the potential of ZETA on the other hand, thus enhancing the charge repulsion effect. This can effectively promote the dispersion of inorganic particles, thereby promoting the adhesion between inorganic particles and resin, further suppressing powder shedding, and reducing the surface resistivity of the composite membrane.

[0029] Preferably, the pore-forming agent is a mixture of pore-forming agent and water, wherein the mass ratio of pore-forming agent to water in the mixture is 1:(0.5-5), and the specific values ​​of (0.5-5) can be, for example, 0.5, 0.52, 0.54, 0.56, 0.58, 0.6, 0.62, 0.65, 0.68, 0.7, 0.72, 0.75, 0.78, 0.8, 0.82, 0.85, 0.88, 0.9, 0.92, 0.95, 0.98, 1 The range is 1:(1.3 to 3.5), consisting of 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, or any two of these ranges, preferably 1:(1.3 to 3.5).

[0030] In this invention, a mixture of pore-forming agent and water is used. The introduction of water enhances wettability, facilitates the penetration and conduction of alkaline aqueous solutions, and further reduces sheet resistance, solving the problem of poor wettability and high sheet resistance caused by the hydrophobic dense layer formed by the resin. Furthermore, when the mass ratio of the pore-forming agent to water is within the aforementioned range, it can effectively inhibit the shedding of inorganic particles, resulting in a more uniform distribution of inorganic particles, a richer pore structure in the composite membrane, and better surface wettability, which is more conducive to reducing the sheet resistance of the membrane. Too little pore-forming agent will result in poor improvement; too much pore-forming agent will lead to enhanced charge repulsion, reduce particle dispersion stability, and thus be detrimental to reducing sheet resistance.

[0031] Preferably, the resin comprises any one or a combination of at least two of polysulfone, polyethersulfone, polyphenylsulfone, polyether, polyamide, polyetheretherketone, or polyvinylidene fluoride, more preferably any one or at least two of polysulfone, polyethersulfone, or polyphenylsulfone.

[0032] Preferably, the weight-average molecular weight of the resin is 28,000 to 300,000, for example, it can be 28,000, 30,000, 32,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, 90,000, 100,000, 110,000, 120,000, 130,000, 140,000, 150,000, 160,000, 180,000, 200,000, 220,000, 240,000, 260,000, 280,000, 300,000 or any combination thereof.

[0033] Preferably, the inorganic particles include any one or a combination of at least two of zirconium oxide, magnesium oxide, aluminum oxide, titanium oxide, silicon oxide, zirconium hydroxide, or magnesium hydroxide.

[0034] Preferably, the D50 particle size of the inorganic particles is 30 to 100 nm, for example, it can be a range of 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm or any combination thereof.

[0035] In this invention, the D50 particle size of the inorganic particles can be obtained by testing with a ZETA potential and particle size analyzer; the D50 particle size of the inorganic particles is within the above range, which is beneficial to further reduce the sheet resistance of the composite membrane.

[0036] Preferably, the organic solvent includes any one or a combination of at least two of N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide.

[0037] Preferably, the substrate is a porous polymer membrane or nonwoven fabric comprising at least one of the following polymers: polyolefin, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, or polyethylene naphthalate.

[0038] In this invention, the polyolefin may be, for example, polyethylene, polypropylene, etc.

[0039] Preferably, the thickness of the substrate is 50 to 400 μm, for example, it can be a range of 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm or any combination thereof.

[0040] Preferably, the thickness of the single-sided coating layer is 40 to 200 μm, for example, it can be a range of 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm or any combination thereof.

[0041] Preferably, the thickness of the composite membrane is 150–520 μm, for example, it can be a range of 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 455 μm, 460 μm, 465 μm, 470 μm, 475 μm, 480 μm, 485 μm, 490 μm, 495 μm, 500 μm, 505 μm, 510 μm, 515 μm, 520 μm or any combination thereof.

[0042] In this invention, the thickness of the coating layer is within the above-mentioned range, which helps to balance the surface resistivity and gas barrier properties of the composite diaphragm, while also taking into account good mechanical strength.

[0043] Preferably, the porosity of the composite membrane is 40-70%, for example, it can be a range of 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, or any combination thereof.

[0044] In this invention, the porosity of the composite membrane can be obtained by testing using the method in the national standard GB / T 33052-2016; the porosity being within the above range is beneficial for further reducing the sheet resistance of the composite membrane, while also ensuring good gas barrier properties of the membrane.

[0045] This invention provides a method for preparing the composite separator, the method comprising the following steps:

[0046] S1: Mix resin, inorganic particles, pore-forming agent and organic solvent to obtain slurry;

[0047] S2: The slurry obtained in S1 is coated onto at least one surface of the substrate to obtain a coated substrate;

[0048] S3: The coated substrate obtained in S2 is subjected to phase transformation to obtain the composite membrane.

[0049] Preferably, the mixing in S1 includes premixing the inorganic particles, organic solvent, and pore-forming agent before adding them to the resin for dissolution.

[0050] In this invention, coating can also be replaced by casting in step S2, and the same applies.

[0051] Preferably, the phase transformation includes immersing the coated substrate in a non-solvent bath to perform the phase transformation, wherein the non-solvent bath contains a non-solvent.

[0052] Preferably, the non-solvent includes one or a mixture of two or more of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, or tert-butanol.

[0053] Preferably, the phase transition time is 5 to 24 hours, for example, it can be a range of 5 hours, 6 hours, 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, 24 hours or any combination thereof.

[0054] The present invention provides an alkaline water electrolysis hydrogen production device, wherein the alkaline water electrolysis hydrogen production device includes the composite membrane.

[0055] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0056] The technical solutions provided by the present invention will be clearly and completely described below with reference to embodiments and comparative examples. Obviously, the specific embodiments described are only some embodiments of the present invention, and not all embodiments.

[0057] All materials used in this invention can be obtained commercially or prepared by conventional methods.

[0058] Example 1

[0059] This embodiment provides a composite membrane, comprising a substrate (purchased from Saifa Filtration Technology (Suzhou) Co., Ltd., Ryton PPS model, thickness 260 μm) and coating layers disposed on both surfaces of the substrate; by weight, the slurry of the coating layer comprises 13.82 parts polysulfone (purchased from Wharton Technology Co., Ltd., VG2000, weight average molecular weight 78000), 34.56 parts zirconium oxide (purchased from Shandong Guoci Functional Materials Co., Ltd., GMZ-B65, D50 particle size 50 nm) and 48.39 parts NMP; 3.24 parts CTAB aqueous solution are added based on 100 parts NMP, wherein the mass ratio of CTAB (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., H108984) to water in the CTAB aqueous solution is 1:1.3; the thickness of the single-sided coating layer is 120 μm, resulting in a composite membrane thickness of 500 μm.

[0060] This embodiment provides a method for preparing a composite separator, specifically including the following steps:

[0061] Zirconia, NMP, and an aqueous solution of a pore-forming agent were stirred for 6 hours until homogeneous. Polysulfone was then added and stirred for 12 hours until completely dissolved to obtain a uniformly dispersed slurry. The slurry was coated onto both surfaces of a substrate and then immersed in a non-solvent bath (containing water) for 15 hours for phase inversion to obtain the composite membrane.

[0062] Example 2

[0063] This embodiment provides a composite membrane, including a substrate and a coating layer disposed on two surfaces of the substrate; by weight, the slurry of the coating layer includes 5 parts of polyetheretherketone (purchased from Evonik Specialty Chemicals (Shanghai) Co., Ltd.) The following materials were used: 4000g of silica (JR-NSP30T, D50 particle size 50nm, purchased from Xuancheng Jingrui New Materials Co., Ltd.), 55 parts of NMP, and 3.6 parts of BPEI aqueous solution (BPEI purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., P434400) were added based on 100 parts of NMP. The mass ratio of BPEI to water in the BPEI aqueous solution was 1:1.3. The thickness of the single-sided coating was 95μm, and the thickness of the composite film was 450μm. Other materials remained the same as in Example 1.

[0064] This embodiment provides a method for preparing a composite membrane, which differs from Example 1 only in that the phase transformation time is 10 hours, while the other step parameters are the same as in Example 1.

[0065] Example 3

[0066] This embodiment provides a composite membrane, comprising a substrate and coating layers disposed on two surfaces of the substrate. By weight, the slurry of the coating layer comprises 18.2 parts polyvinylidene fluoride (purchased from Arkema, France, weight average molecular weight 300,000), 15.5 parts magnesium hydroxide (purchased from Xuancheng Jingrui New Materials Co., Ltd., VK-MHT01, D50 particle size 30nm), and 40 parts NMP. 4.5 parts of an MPA aqueous solution (MPA purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., M103035) are added per 100 parts of NMP, with the mass ratio of MPA to water in the MPA aqueous solution being 1:1.3. The thickness of the composite membrane is 500 μm. Other materials remain consistent with those in Example 1.

[0067] This embodiment provides a method for preparing a composite membrane, which differs from Example 1 only in that the phase transformation time is 20 hours, while the other steps are the same as in Example 1.

[0068] Example 4

[0069] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the total mass of the CTAB aqueous solution remains unchanged, the mass ratio of CTAB to water is 1:3, and the other components, dosages, and preparation methods are the same as in Embodiment 1.

[0070] Example 5

[0071] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the total mass of the CTAB aqueous solution remains unchanged, the mass ratio of CTAB to water is 1:2, and the other components, dosages, and preparation methods are the same as in Embodiment 1.

[0072] Example 6

[0073] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the total mass of the CTAB aqueous solution remains unchanged, the mass ratio of CTAB to water is 1:4, and the other components, dosages, and preparation methods are the same as in Embodiment 1.

[0074] Example 7

[0075] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the total mass of the CTAB aqueous solution remains unchanged, the mass ratio of CTAB to water is 1:0.8, and the other components, dosages, and preparation methods are the same as in Embodiment 1.

[0076] Example 8

[0077] This embodiment provides a composite membrane, which differs from Example 1 only in that CTAB is replaced with an equal mass of dodecyl dimethyl benzyl ammonium chloride (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. B100950). The other components, dosages, and preparation methods are the same as in Example 1.

[0078] Example 9

[0079] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the zirconium oxide is replaced with zirconium oxide with a D50 particle size of 20 nm (purchased from Shandong Guoci Functional Materials Co., Ltd.). The other components, dosages, and preparation methods are the same as in Embodiment 1.

[0080] Example 10

[0081] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the zirconium oxide is replaced with zirconium oxide with a D50 particle size of 120 nm (purchased from Shandong Guoci Functional Materials Co., Ltd.). The other components, dosages, and preparation methods are the same as in Embodiment 1.

[0082] Example 11

[0083] This embodiment provides a composite diaphragm, which differs from Embodiment 1 only in that the substrate thickness is 50 μm, the single-sided coating thickness is 45 μm, and the composite diaphragm thickness is 140 μm. Other components, dosages, and preparation methods are the same as in Embodiment 1.

[0084] Example 12

[0085] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the thickness of the single-sided coating layer is 170 μm and the thickness of the composite membrane is 600 μm. The other components, dosages, and preparation methods are the same as in Embodiment 1.

[0086] Example 13

[0087] This embodiment provides a composite diaphragm, which differs from Embodiment 1 only in that the substrate thickness is 100 μm, the single-sided coating thickness is 200 μm, and the composite diaphragm thickness is 500 μm. Other components, dosages, and preparation methods are the same as in Embodiment 1.

[0088] Example 14

[0089] This embodiment provides a composite diaphragm, which differs from Embodiment 1 only in that the substrate thickness is 400 μm, the single-sided coating thickness is 50 μm, and the composite diaphragm thickness is 500 μm. Other components, dosages, and preparation methods are the same as in Embodiment 1.

[0090] Example 15

[0091] This embodiment provides a composite membrane, which differs from Embodiment 1 only in that the CTAB aqueous solution in the coating slurry is replaced with an equal mass of CTAB, while the other components, dosages, and preparation methods are the same as in Embodiment 1.

[0092] Example 16

[0093] This embodiment provides a composite membrane, which differs from Example 1 only in that the phase transformation time in the preparation method of the composite membrane is 3 hours, while the other components, amounts, and preparation methods are the same as in Example 1.

[0094] Comparative Example 1

[0095] This comparative example provides a composite membrane, which differs from Example 1 only in that the CTAB aqueous solution in the coating slurry is replaced with an equal mass of polyvinylpyrrolidone (PVP, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. K30). The other components, dosages, and preparation methods are the same as in Example 1.

[0096] Comparative Example 2

[0097] This comparative example provides a composite membrane, which differs from Example 1 only in that the CTAB aqueous solution in the coating slurry is replaced with an equal mass of PVP aqueous solution (the mass ratio of PVP to water is 1:1.3). All other components, dosages, and preparation methods are the same as in Example 1.

[0098] Comparative Example 3

[0099] This comparative example provides a composite membrane, which differs from Example 1 only in that, based on 100 parts of NMP, the mass of the CTAB aqueous solution is 0.02 parts (CTAB to water mass ratio 1:1.3). Other components, amounts, and preparation methods are the same as in Example 1.

[0100] Comparative Example 4

[0101] This comparative example provides a composite membrane, which differs from Example 1 only in that, based on 100 parts of NMP, the mass of the CTAB aqueous solution is 9 parts (CTAB to water mass ratio 1:1.3). Other components, amounts, and preparation methods are the same as in Example 1.

[0102] Performance testing

[0103] (1) Powder shedding rate: Characterized by the change in mass of the composite diaphragm before and after use; The specific method is as follows: After drying in an oven at 80℃ for 6 hours, the initial weight of the composite diaphragm is recorded as m0 by an analytical balance. Then, the composite diaphragm is placed in a high-pressure reactor, and 30% KOH is added. Then, it is heated at 100℃ for 48 hours. After the reaction is completed, the composite diaphragm is soaked in deionized water for 2 hours to clean the residual alkali solution. The composite diaphragm is then taken out and rinsed with deionized water to remove the residual liquid on the surface. After drying in an oven at 80℃ for 6 hours, the weight of the composite diaphragm is recorded as m1 by an analytical balance. Powder shedding rate = (m0-m1) / m0×100%. The lower the powder shedding rate, the better the effect of inhibiting powder shedding.

[0104] (2) Water absorption rate: After drying the composite membrane in an oven at 80℃ for 6 hours, the initial weight of the composite membrane was weighed by an analytical balance and recorded as m0. Then, the composite membrane was soaked in 30% KOH for 2 hours. After taking it out, the surface alkaline solution was gently wiped off. Then, the mass of the composite membrane after absorbing the liquid was weighed and recorded as m1. The water absorption rate was calculated using the formula water absorption rate = (m1-m0) / m0×100%.

[0105] (3) Sheet resistance: Four diaphragm samples with a diameter of 4 cm were cut from a flat area of ​​the composite diaphragm. The samples were immersed in 30% KOH solution for 24 hours, then removed and placed in a sheet resistance testing fixture (test diameter 2 cm). The four-probe method of an electrochemical workstation was used to test the resistance at 25°C. The four diaphragms were placed in the fixture one after another to obtain the resistance values ​​of the four diaphragms. The average resistance value of the four diaphragms was then taken, and the average resistance value was multiplied by the test area of ​​the diaphragm (3.14 cm²). 2 ), that is, the surface resistance (Ω·cm) is obtained. 2 ).

[0106] (4) Porosity: Tested according to GB / T 33052-2016.

[0107] (5) Bubble point: Tested according to GB / T 32361-2015.

[0108] The specific test results are shown in Table 1.

[0109] Table 1

[0110]

[0111] As shown in Table 1, the composite membrane provided by this invention uses a coating layer containing a specific amount of a pore-forming agent with ionizable groups, which can suppress the shedding of inorganic particles in the composite membrane. The powder shedding rate of the composite membrane before and after use is ≤1.159%; it also effectively reduces the sheet resistance of the composite membrane to ≤0.69Ω·cm. 2 Furthermore, the resulting composite membrane has a high bubble point, ≥3 bar.

[0112] As can be seen from Comparative Example 1, compared with traditional diaphragms, the composite diaphragm provided by the present invention has a lower sheet resistance and the powder shedding can be effectively suppressed.

[0113] As can be seen from Example 15 and Comparative Example 2, the slurry of the composite diaphragm does not contain a pore-forming agent with a specific structure or water, resulting in severe powder shedding and / or increased surface resistivity of the composite diaphragm.

[0114] As can be seen from Comparative Examples 3 and 4, the content of pore-forming agent in the slurry of the composite diaphragm is not within a specific range, and the composite diaphragm suffers from severe powder shedding and / or increased surface resistivity.

[0115] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A composite diaphragm, characterized in that, The composite membrane includes a substrate and a coating layer disposed on at least one surface of the substrate; By weight, the slurry of the coating layer comprises 1-25 parts resin, 10-45 parts inorganic particles, and 40-65 parts organic solvent. The coating slurry further includes 0.05 to 4.5 parts of a pore-forming agent, calculated as 100 parts by weight of an organic solvent, wherein the pore-forming agent contains ionizable groups in its molecular structure.

2. The composite diaphragm according to claim 1, characterized in that, The ionizable group includes at least one of quaternary ammonium group, primary amine group, secondary amine group, tertiary amine group, carboxyl group or mercapto group; Preferably, the pore-forming agent comprises at least one of a long-chain alkyl quaternary ammonium salt, branched polyethyleneimine, or mercaptopropionic acid; Preferably, the long-chain alkyl quaternary ammonium salt includes quaternary ammonium salts with alkyl carbon atoms ≥ 12; Preferably, the long-chain alkyl quaternary ammonium salt comprises hexadecyltrimethylammonium bromide.

3. The composite diaphragm according to claim 1 or 2, characterized in that, The pore-forming agent is a mixture of pore-forming agent and water, wherein the mass ratio of pore-forming agent to water in the mixture is 1:(0.5-5), more preferably 1:(1.3-3.5).

4. The composite diaphragm according to any one of claims 1 to 3, characterized in that, The resin includes any one or a combination of at least two of polysulfone, polyethersulfone, polyphenylsulfone, polyether, polyamide, polyetheretherketone or polyvinylidene fluoride, more preferably any one or at least two of polysulfone, polyethersulfone, or polyphenylsulfone. Preferably, the weight-average molecular weight of the resin is 28,000 to 300,000.

5. The composite diaphragm according to any one of claims 1 to 4, characterized in that, The inorganic particles include any one or a combination of at least two of zirconium oxide, magnesium oxide, aluminum oxide, titanium oxide, silicon oxide, zirconium hydroxide, or magnesium hydroxide. Preferably, the D50 particle size of the inorganic particles is 30-100 nm.

6. The composite diaphragm according to any one of claims 1 to 5, characterized in that, The substrate is a porous polymer membrane or nonwoven fabric comprising at least one of the following polymers: polyolefin, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, or polyethylene naphthalate. Preferably, the thickness of the substrate is 50–400 μm.

7. The composite diaphragm according to any one of claims 1 to 6, characterized in that, The thickness of the composite diaphragm is 150–520 μm; Preferably, the porosity of the composite membrane is 40-70%.

8. A method for preparing a composite diaphragm according to any one of claims 1 to 7, characterized in that, The preparation method includes the following steps: S1: Mix resin, inorganic particles, pore-forming agent and organic solvent to obtain slurry; S2: The slurry obtained in S1 is coated onto at least one surface of the substrate to obtain a coated substrate; S3: The coated substrate obtained in S2 is subjected to phase transformation to obtain the composite membrane.

9. The preparation method according to claim 8, characterized in that, The mixing described in S1 includes premixing inorganic particles, organic solvents, and pore-forming agents before adding them to the resin for dissolution. Preferably, the phase transformation includes immersing the coated substrate in a non-solvent bath for phase transformation, wherein the non-solvent bath includes a non-solvent. Preferably, the non-solvent includes one or a mixture of two or more of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, or tert-butanol. Preferably, the phase transformation time is 5 to 24 hours.

10. An alkaline water electrolysis hydrogen production device, characterized in that, The alkaline water electrolysis hydrogen production device includes the composite membrane described in any one of claims 1 to 7.