Method for the dehydration of electrolytic magnesium raw material and its use
By using a vacuum low-temperature dehydration process to treat electrolytic magnesium raw materials in a closed reactor, the problems of low dehydration efficiency and equipment corrosion in existing technologies are solved, enabling the preparation of highly efficient and pure electrolytic magnesium raw materials, and improving electrolysis efficiency and environmental friendliness.
Patent Information
- Application Number
- CN202611432738.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing methods for dehydrating electrolytic magnesium raw materials are inefficient and complex, posing risks of equipment corrosion and environmental pollution. The dehydrated electrolytic raw materials are in a crystalline state, which affects the efficiency of subsequent electrolysis processes.
The process employs a vacuum low-temperature dehydration technique, in which the electrolytic magnesium raw material is evacuated to below 500 Pa in a closed reactor and heated to 80-180℃ for 30-100 min. This simplifies the process, avoids high-temperature hydrolysis and adhesion, and maintains the material in a dispersed state.
It achieves efficient dehydration, high product purity, avoids equipment corrosion and environmental pollution, improves subsequent electrolysis efficiency, and reduces energy consumption.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of magnesium metal preparation technology, specifically to a method for dehydrating electrolytic magnesium raw materials and its application. Background Technology
[0002] Magnesium (Mg) and its alloys are widely used in aerospace, automotive, electronics, and pharmaceutical industries due to their lightweight, high specific strength, high damping properties, strong electromagnetic shielding, excellent biocompatibility, and biodegradability. Currently, industrial production methods include thermal reduction and electrochemical methods. Thermal reduction involves reducing magnesium-containing minerals (such as dolomite) with a ferrosilicon alloy under high temperature and high vacuum conditions, resulting in large amounts of CO2 and SO2. x Emissions severely restrict its development. Electrochemical methods for preparing liquid magnesium by electrolyzing anhydrous MgCl2 or anhydrous potassium carnallite in a molten state are becoming increasingly popular due to their green and environmentally friendly nature.
[0003] Currently, in the process of potassium extraction from salt lakes, magnesium chloride hydrate can be prepared by natural evaporation of old brine. For example, the reserves of magnesium chloride hydrate in the Qarhan Salt Lake are approximately 3.16 billion tons. The pure crystalline MgCl2·6H2O produced after evaporation in this area has an extremely high content. However, the potassium extraction process generates a large amount of old brine, most of which is discharged back into the salt lake, resulting in resource waste and affecting the salt balance of the aquatic environment. Meanwhile, potash fertilizer plants can produce approximately 100,000 tons of potassium carnallite (MgCl2·KCl·6H2O) annually by mixing brine. From the perspective of downstream electrolysis, the raw materials for electrolytic magnesium can only be anhydrous magnesium chloride or anhydrous potassium carnallite. Existing experience shows that the presence of potassium salts is beneficial for dehydration, but the free water released from the electrolysis of crystal water can severely corrode the electrodes, leading to electrolysis shutdown. Therefore, it is urgent to develop new dehydration processes for electrolytic magnesium raw materials, which is of great significance for ensuring magnesium resource security and the sustainable development of salt lakes.
[0004] In the comprehensive development and utilization of magnesium resources in salt lakes, the efficient dehydration of magnesium chloride hydrate (MgCl2·6H2O) and potassium carnallite (MgCl2·KCl·6H2O) is a key technological step in the preparation of anhydrous magnesium chloride, and also one of the core constraints on the in-depth development of the magnesium industry chain. Traditional dehydration processes typically employ a stepped heating method to remove free water and water of crystallization sequentially. However, near the stage of complete dehydration, MgCl2 (including MgCl2 in potassium carnallite) is prone to hydrolysis, generating Mg(OH)Cl (basic magnesium chloride) or MgO (magnesium oxide), leading to a decrease in product purity and the release of corrosive hydrogen chloride gas, severely restricting industrial application. Below 200℃, magnesium chloride hydrate, upon heating, adheres to each other, reducing its specific surface area and further decreasing its evaporation rate.
[0005] In recent years, innovative processes such as novel fluidized bed dehydration, spray pyrolysis, and microwave-assisted dehydration have emerged, demonstrating significant potential in improving dehydration efficiency, reducing energy consumption, and enhancing product purity. These advancements provide important technological pathways for the high-value and green utilization of magnesium resources in salt lakes. While these efforts have achieved some success in inhibiting hydrolysis during magnesium chloride dehydration, maintaining high dehydration efficiency remains challenging. Therefore, there is an urgent need to develop a new, highly efficient magnesium chloride dehydration system to meet the raw material standards for magnesium chloride electrolysis and achieve the efficient development and utilization of magnesium resources in salt lakes. Summary of the Invention
[0006] The purpose of this invention is to overcome the problems of low dehydration efficiency, complex processes, and risks of equipment corrosion and environmental pollution associated with existing dehydration methods for electrolytic magnesium raw materials. Furthermore, the crystalline state of the dehydrated raw material affects the efficiency of subsequent electrolysis processes. This invention provides a dehydration method for electrolytic magnesium raw materials and its application. This method combines a vacuum (reduced pressure) environment with a heating process to form a targeted new vacuum low-temperature dehydration process. This process eliminates the need for segmented heating, effectively simplifying the dehydration process. It not only achieves high dehydration efficiency and high purity of the dehydrated product but also eliminates the risks of equipment corrosion and environmental pollution. Simultaneously, the dehydrated electrolytic magnesium raw material exhibits a well-dispersed state, laying a solid foundation for improving the efficiency of subsequent electrolysis processes.
[0007] To achieve the above objectives, the present invention provides a method for dehydrating electrolytic magnesium raw materials. The dehydration method is carried out in a closed reactor and includes: spreading the electrolytic magnesium raw materials evenly in the closed reactor, then evacuating the closed reactor to an absolute pressure of less than 500 Pa, and then heating it to 80-180°C and maintaining the temperature for 30-100 min.
[0008] Among them, the raw materials for electrolytic magnesium are magnesium chloride and / or potassium carnallite.
[0009] Furthermore, the electrolytic magnesium feedstock accounts for 30-50% of the total volume of the closed reactor.
[0010] Furthermore, the D50 particle size of the electrolytic magnesium raw material is 100-800μm, preferably 200-600μm.
[0011] Furthermore, the absolute pressure in the closed reactor is 0.5-100 Pa.
[0012] Furthermore, the heating temperature is 100-160℃.
[0013] Furthermore, the constant temperature treatment time is 40-80 minutes.
[0014] Furthermore, the heating rate during the heating process is 1-10℃ / min, preferably 2-5℃ / min.
[0015] The second aspect of the present invention provides a method for preparing liquid magnesium by electrolysis, the method comprising: dehydrating the electrolytic magnesium raw material according to the dehydration method described above to obtain anhydrous electrolytic magnesium raw material, and then electrolyzing the anhydrous electrolytic magnesium raw material.
[0016] Furthermore, the raw material for anhydrous electrolytic magnesium is anhydrous magnesium chloride, and an electrolyte is added during the electrolysis process, wherein the molar ratio of anhydrous magnesium chloride to electrolyte is 1:2-4.
[0017] Preferably, the electrolyte is selected from at least one of NaCl, KCl and CaF2.
[0018] Furthermore, the electrolysis conditions include: a temperature of 650-800℃ and a cathode current density of 0.2-1 A / cm². 2 The operating voltage is 4-7V.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] (1) This invention systematically applies the physicochemical principle that the boiling point of a substance decreases with decreasing pressure to the dehydration process of electrolytic magnesium raw materials: by combining vacuum (depressurization) environment with heating, a new targeted vacuum low-temperature dehydration process is formed, which does not require segmented heating (boiling dehydration + chlorination roasting), simplifying the process and equipment; it can achieve the effect of two dehydrations in the existing process in one dehydration stage.
[0021] (2) This invention reduces the temperature required for dehydration by reducing the system pressure, thereby effectively avoiding the problem that MgCl2 is easily hydrolyzed to generate Mg(OH)Cl or MgO in the traditional high-temperature dehydration process. The existing atmospheric pressure dehydration process inevitably produces basic magnesium chloride and magnesium oxide. These impurities have extremely high melting points and will form non-melting precipitates in the electrolysis section, which will hinder the electrolysis reaction and reduce the current effect. At the same time, it reduces the generation of corrosive HCl gas and the decrease in product purity from the source, and prevents material adhesion.
[0022] (3) The present invention utilizes a vacuum environment to prevent electrolytic magnesium raw materials from sticking together and clumping together due to surface moisture evaporation in the early stage of dehydration, thereby maintaining the loose state and large specific surface area of the material and solving the problem of reduced evaporation rate caused by traditional heating.
[0023] (4) The vacuum environment in this invention not only lowers the boiling point of water and accelerates the evaporation and removal of water, but also makes the heat conduction and mass transfer processes more efficient by preventing adhesion, thus accelerating the overall dehydration reaction rate. This method can achieve efficient dehydration at a lower temperature, while taking into account the two goals that are difficult to balance in traditional processes: high efficiency and low hydrolysis. Detailed Implementation
[0024] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.
[0025] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0026] As analyzed in the background section of this application, the existing methods for dehydrating electrolytic magnesium raw materials have problems such as low dehydration efficiency, complex processes, and risks of equipment corrosion and environmental pollution. In addition, the dehydrated electrolytic raw materials are in a crystalline state, which affects the electrolysis efficiency of subsequent electrolysis processes. In order to solve the above problems, this application provides a method for dehydrating electrolytic magnesium raw materials and its application.
[0027] In a typical embodiment of this application, a method for dehydrating electrolytic magnesium raw material is provided. The dehydration method is carried out in a closed reactor and includes: spreading the electrolytic magnesium raw material evenly in the closed reactor, then evacuating the closed reactor to an absolute pressure of less than 500 Pa, then heating it to 80-180°C and maintaining the temperature for 30-100 min; wherein the electrolytic magnesium raw material is magnesium chloride and / or potassium carnallite.
[0028] In some embodiments, the electrolytic magnesium feedstock accounts for 30-50% of the total volume of the closed reactor, preferably 35-45%. As specific examples, the electrolytic magnesium feedstock accounts for 35%, 37%, 39%, 40%, 42%, 44%, or 45% of the total volume of the closed reactor.
[0029] In some preferred embodiments, the electrolytic magnesium feedstock is magnesium chloride hydrate or potassium carnallite. The D50 particle size of the electrolytic magnesium feedstock is 100-800 μm, preferably 200-600 μm, and more preferably 200-300 μm. As a specific example, the D50 particle size of the electrolytic magnesium feedstock can be 200 μm, 220 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, or 300 μm.
[0030] In some preferred embodiments, the absolute pressure in the closed reactor is 0.5-100 Pa, more preferably 5-50 Pa. As specific examples, the absolute pressure in the closed reactor can be 5 Pa, 10 Pa, 15 Pa, 20 Pa, 25 Pa, 30 Pa, 35 Pa, 40 Pa, 45 Pa, or 50 Pa.
[0031] In some preferred embodiments, the heating temperature is 100-160°C, more preferably 100-150°C. As specific examples, the heating temperature can be 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C.
[0032] In some preferred embodiments, the isothermal treatment time is 40-80 minutes, preferably 45-75 minutes. As specific examples, the isothermal treatment time can be 45 minutes, 50 minutes, 55 minutes, 60 minutes, 65 minutes, 70 minutes, or 75 minutes.
[0033] In some embodiments, the heating rate is 1-10°C / min, preferably 2-5°C / min. As specific examples, the heating rate can be 2°C / min, 3°C / min, 4°C / min, or 5°C / min.
[0034] In the dehydration method of this invention, the specific type of closed reactor is not particularly limited; any reactor conventionally used in the art that can withstand vacuum heating conditions is suitable for this invention. In some embodiments, the closed reactor may be selected from equipment including but not limited to reaction vessels, vacuum metallurgical furnaces, vacuum distillation furnaces, etc.
[0035] In the dehydration method of the present invention, there is no limitation on the type of equipment used for vacuuming the closed reactor. Conventional vacuuming equipment in the art can be used, such as rotary vane vacuum pumps, slide valve vacuum pumps, Roots vacuum pumps, etc., as long as the set vacuum level in the closed reactor can be stably maintained and the pumping rate requirements of the dehydration process are met.
[0036] In the dehydration method of the present invention, during the continuous vacuum heating process, the water of crystallization contained in the electrolytic magnesium raw material will be gradually removed and converted into water vapor. The water vapor will be continuously drawn out of the sealed reactor by the vacuum pumping action of the vacuum equipment, thereby achieving efficient removal of water of crystallization. At the same time, it avoids water vapor residue in the furnace, which may cause the raw material to absorb water or hydrolyze again, further ensuring the dehydration effect and product purity.
[0037] In some embodiments, the dehydration method further includes: maintaining a constant pressure within the sealed reactor, cooling the deheated material to room temperature, and then removing it. In this invention, the cooling process is not limited. In the technical solution of this invention, conventional cooling methods in the art can be selected according to actual production needs. These can be either natural cooling, allowing the material to slowly cool to room temperature along with the sealed reactor, or controlled cooling, gradually reducing the temperature inside the reactor by adjusting the temperature control system until the material reaches room temperature. Regardless of the cooling method used, as long as the cooling process is stable, avoiding agglomeration or deterioration of the dehydrated material due to excessively rapid cooling, or secondary water absorption and oxidation of the material due to premature air entering the furnace during cooling, it can be applied to this invention. This further ensures the dispersion state and purity of the dehydrated material, ensuring it can smoothly meet the process requirements of subsequent electrolytic magnesium production.
[0038] The anhydrous electrolytic magnesium raw material obtained by the dehydration method of the present invention has a moisture content of ≤0.5wt% and a magnesium oxide content of ≤0.5wt%, and all indicators fully meet the standard requirements for raw materials required for electrolytic magnesium production. At the same time, the material after dehydration still maintains a good dispersion state and has no obvious agglomeration phenomenon, which can effectively reduce the viscosity of the electrolyte system and reduce the mass transfer resistance during subsequent electrolysis, thereby significantly improving the efficiency of subsequent electrolytic magnesium production and reducing production energy consumption.
[0039] In another typical embodiment of this application, a method for preparing liquid magnesium by electrolysis is provided. The method includes: dehydrating the electrolytic magnesium raw material according to the dehydration method described above to obtain anhydrous electrolytic magnesium raw material, and then electrolyzing the anhydrous electrolytic magnesium raw material.
[0040] In some embodiments, the raw material for anhydrous electrolytic magnesium is anhydrous magnesium chloride, and an electrolyte is added during the electrolysis process. The molar ratio of anhydrous magnesium chloride to electrolyte is 1:2-4, preferably 1:2.5-3.5.
[0041] In some preferred embodiments, the electrolyte is selected from at least one of NaCl, KCl, and CaF2. In a further preferred embodiment, the electrolyte is KCl.
[0042] In some embodiments, the conditions for the electrolysis process include: a temperature of 650-800°C, preferably 700-750°C; and a cathode current density of 0.2-1 A / cm². 2 Preferably, it is 0.5-0.75 A / cm. 2 The operating voltage is 4-7V, preferably 5-6V.
[0043] The following examples further illustrate the dehydration method for electrolytic magnesium raw materials of the present invention and its application. These examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.
[0044] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.
[0045] In the following examples and comparative examples, hydrated magnesium chloride and potassium carnallite were both sourced from Qinghai Salt Lake Industry Co., Ltd., with water contents of 51.5 wt% and 33 wt%, respectively.
[0046] Example 1
[0047] (1) Spread 1 kg of magnesium chloride water (D50 200 μm) evenly in the reactor, with the magnesium chloride water accounting for 40% of the total volume of the reactor; then evacuate the reactor to an absolute pressure of 10 Pa, then heat it to 150 °C at a heating rate of 3 °C / min and keep it at a constant temperature for 60 min. Then keep the pressure of the reactor constant and let the treated material cool naturally to room temperature to obtain anhydrous electrolytic magnesium raw material.
[0048] (2) At a temperature of 700℃, the cathode current density is 0.75 A / cm. 2 Under the condition of working voltage of 5V, the anhydrous electrolytic magnesium raw material obtained in step (1) is electrolyzed, and KCl is added during the electrolysis process. The molar ratio of dehydrated material to KCl is 1:2.5.
[0049] Example 2
[0050] (1) Spread 1 kg of magnesium chloride water (D50 300 μm) evenly in the reaction tank of the reactor. The magnesium chloride water accounts for 35% of the total volume of the reactor. Then, evacuate the reactor to an absolute pressure of 5 Pa, heat it to 100 °C at a heating rate of 2 °C / min and keep it at a constant temperature for 75 min. Then, keep the pressure of the reactor constant and let the treated material cool naturally to room temperature to obtain anhydrous electrolytic magnesium raw material.
[0051] (2) The temperature is 700℃ and the cathode current density is 0.75A / cm. 2 Under the condition of working voltage of 5V, the anhydrous electrolytic magnesium raw material obtained in step (1) is electrolyzed, and KCl is added during the electrolysis process. The molar ratio of dehydrated material to KCl is 1:2.5.
[0052] Example 3
[0053] (1) Spread 1 kg of magnesium chloride water (D50 200 μm) evenly in the reaction tank of the reactor. The magnesium chloride water accounts for 45% of the total volume of the reactor. Then, evacuate the reactor to an absolute pressure of 50 Pa, heat it to 130 °C at a heating rate of 5 °C / min and keep it at a constant temperature for 65 min. Then, keep the pressure of the reactor constant and let the treated material cool naturally to room temperature. This is anhydrous electrolytic magnesium raw material.
[0054] (2) The temperature is 700℃ and the cathode current density is 0.75A / cm. 2 Under the condition of working voltage of 5V, the anhydrous electrolytic magnesium raw material obtained in step (1) is electrolyzed, and KCl is added during the electrolysis process. The molar ratio of dehydrated material to KCl is 1:2.5.
[0055] Example 4
[0056] The method is implemented according to Example 2, except that in step (1), the absolute pressure inside the closed reactor is 100 Pa.
[0057] Example 5
[0058] The method is implemented according to Example 1, except that in step (1), the heating temperature is 180°C.
[0059] Example 6
[0060] The method is implemented according to Example 1, except that in step (1), the electrolytic magnesium raw material accounts for 60% of the total volume of the closed reactor.
[0061] Example 7
[0062] The method is implemented according to Example 1, except that in step (1), the electrolytic magnesium raw material is potassium carnallite.
[0063] Example 8
[0064] The method is implemented according to Example 1, except that in step (1), the heating rate is 10°C / min.
[0065] Comparative Example 1
[0066] The method is implemented according to Example 1, except that in step (1), the absolute pressure inside the closed reactor is 500 Pa.
[0067] Comparative Example 2
[0068] The method is implemented according to Example 1, except that in step (1), the heating temperature is 200°C.
[0069] Test method:
[0070] (1) The present invention uses Karl Fischer method and chemical titration method to test the water content and magnesium oxide content in the electrolytic magnesium raw materials obtained in the examples and comparative examples. The results are shown in Table 1.
[0071] (2) The present invention uses the ratio of actual magnesium production per unit time to theoretical magnesium production to test the current efficiency of anhydrous magnesium raw material electrolysis process in the examples and comparative examples. The results are shown in Table 1.
[0072] Table 1
[0073]
[0074] The results in Table 1 show that increasing the vacuum level is beneficial for achieving dehydration at low temperatures. The lower the temperature, the fewer the dehydration side reactions, which is more conducive to improving the current effect in subsequent electrolysis.
[0075] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for dehydrating electrolytic magnesium raw materials, characterized in that, The dehydration method is carried out in a closed reactor and includes: spreading the electrolytic magnesium raw material evenly in the closed reactor, then evacuating the closed reactor to an absolute pressure of less than 500 Pa, then heating it to 80-180°C and maintaining the temperature for 30-100 min. The electrolytic magnesium raw material is magnesium chloride hydrate and / or potassium carnallite.
2. The dehydration method according to claim 1, characterized in that, The electrolytic magnesium raw material accounts for 30-50% of the total volume of the closed reactor.
3. The dehydration method according to claim 1 or 2, characterized in that, The D50 particle size of the electrolytic magnesium raw material is 100-800μm, preferably 200-600μm.
4. The dehydration method according to any one of claims 1 to 3, characterized in that, The absolute pressure in the closed reactor is 0.5-100 Pa.
5. The dehydration method according to any one of claims 1 to 4, characterized in that, The heating temperature is 100-160℃.
6. The dehydration method according to any one of claims 1 to 5, characterized in that, The constant temperature treatment lasts for 40-80 minutes.
7. The dehydration method according to any one of claims 1 to 6, characterized in that, The heating rate is 1-10℃ / min, preferably 2-5℃ / min.
8. A method for preparing liquid magnesium by electrolysis, characterized in that, The preparation method includes: dehydrating the electrolytic magnesium raw material according to any one of claims 1 to 7 to obtain anhydrous electrolytic magnesium raw material, and then electrolyzing the anhydrous electrolytic magnesium raw material.
9. The preparation method according to claim 8, characterized in that, The anhydrous electrolytic magnesium raw material is anhydrous magnesium chloride. An electrolyte is added during the electrolysis process, wherein the molar ratio of the anhydrous magnesium chloride to the electrolyte is 1:2-4. Preferably, the electrolyte is selected from at least one of NaCl, KCl and CaF2.
10. The preparation method according to claim 8 or 9, characterized in that, The electrolysis conditions include: a temperature of 650-800℃ and a cathode current density of 0.2-1 A / cm². 2 The operating voltage is 4-7V.