Zinc electrowinning aluminum cathode plate and preparation method thereof
By applying an epoxy insulating and anti-corrosion coating to the zinc electrolytic aluminum cathode plate, the corrosion problem at the interface between the aluminum substrate and the plastic edging strip is solved, achieving long-term protection and extended lifespan of the aluminum cathode plate, simplifying the production process, and reducing costs.
Patent Information
- Application Number
- CN202611432747.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing zinc-electrode aluminum cathode plates are prone to crevice corrosion at the interface between the aluminum substrate and the plastic edging strip, which limits their service life and accelerates corrosion and plate failure due to the large difference in thermal expansion coefficients.
An epoxy insulating and anti-corrosion coating is applied to the edge of the aluminum substrate and the liquid level area. The coating material includes epoxy resin, curing agent, antioxidant, lubricant and filler. A dense three-dimensional network structure is formed by electrostatic spraying, which closely adheres to the aluminum substrate and eliminates the tiny gaps caused by the difference in interfacial thermal stress.
It effectively reduces crevice corrosion, extends the service life of zinc electrolytic aluminum cathode plates, simplifies the production process, reduces costs, improves mechanical strength and insulation performance, and replaces the insulation protection of traditional plastic edge banding strips.
Smart Images

Figure CN123153121A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode materials technology, and more specifically, to a zinc-electrode aluminum cathode plate and its preparation method. Background Technology
[0002] Zinc electrowinning is the core process in the hydrometallurgical zinc refining process. It mainly uses direct current to reduce and deposit zinc ions in the electrolyte onto the cathode to obtain metallic zinc. The cathode material is usually aluminum or aluminum alloy. The following problems exist in the zinc electrowinning production of such cathode aluminum plates: (1) When the side of the cathode aluminum plate is exposed, there will be electric field concentration, which will cause zinc ions to be deposited on the edge of the plate, causing the electrowinning zinc on both sides of the cathode to be connected into a whole to form edge zinc, resulting in problems such as zinc stripping jamming, zinc sheet tearing, and electrode plate damage; (2) The edge of the electrode plate is a high-incidence area of electric field distortion, which is prone to local current density problems, resulting in defects such as nodules, burrs, and thick edges on the zinc sheet; (3) During production, the cathode plate will be subjected to severe impact and vibration during hoisting, collision in the tank, and mechanical zinc stripping, resulting in damage such as edge curling and chipping on the aluminum plate edge.
[0003] To address these issues, existing technologies typically employ injection molding or hot pressing processes to fix thermoplastic strips such as acrylonitrile-butadiene-styrene copolymer (ABS), polyphenylene oxide (PPO), polypropylene (PP), and polyethylene (PE) to the edges of aluminum plates. These insulating strips prevent zinc deposition on the sides, ensuring smooth zinc stripping. They also optimize the edge electric field distribution to improve zinc sheet quality and provide mechanical protection against edge damage. However, a tiny gap of 0.01mm to 0.5mm usually exists between the plastic strip and the aluminum substrate. When electrolyte seeps in, crevice corrosion occurs, forming corrosion pits on the aluminum substrate surface. Zinc deposition within these crevices further widens them, accelerating strip detachment and electrode failure, significantly limiting the lifespan of the aluminum cathode plate (typically only about 12 months). The existing improvement method involves a combination of brushing on liquid coatings (such as modified vinyl ester coatings) followed by injection molding of insulating strips. This involves manually brushing on the modified vinyl ester anti-corrosion coating at the edges of the electrode, near the edges, and near the liquid level. After the coating cures, injection molding of insulating strips is used to reduce interfacial gaps. However, this manual brushing method lacks automation, resulting in uneven coating thickness, insufficient density, poor batch consistency, and poor stability. Furthermore, micro-gaps within 0.01 mm remain in some areas after brushing. The modified vinyl ester coating has poor corrosion resistance, leading to embrittlement, peeling, and flaking during prolonged electrolyte immersion and cyclic zinc stripping, further increasing interfacial gaps. Simultaneously, the large difference in thermal expansion coefficients between the aluminum substrate, the anti-corrosion coating, and the plastic insulating strips makes them prone to thermal stress, which can further induce interfacial micro-cracks, exacerbating corrosion and electrode failure. Therefore, the traditional method of brush coating and injection molding edge strip cannot fundamentally prevent electrolyte interface gap corrosion, and thus cannot solve the problem of edge strip detachment and fall off after long-term service of aluminum cathode plates. In addition, the manual brush coating + injection molding process is cumbersome and costly. Summary of the Invention
[0004] The main objective of this invention is to provide a zinc electrolytic aluminum cathode plate and its preparation method, in order to solve the problems in the prior art where crevice corrosion easily occurs between the edge strip and the aluminum substrate, resulting in a limited service life of the electrode plate. At the same time, the large difference in the thermal expansion coefficients of aluminum and plastic further accelerates corrosion and electrode plate failure.
[0005] To achieve the above objectives, according to a first aspect of the present invention, a zinc electrowinning aluminum cathode plate is provided, comprising an aluminum substrate and an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate. The epoxy insulating and anti-corrosion coating is located in the coating coverage area of the aluminum substrate. The aluminum substrate has a first side, a second side, a third side, and a fourth side connected end-to-end in a circumferential direction. The first side and the third side are disposed opposite each other, and the second side and the fourth side are disposed opposite each other. The coating coverage area of the aluminum substrate includes a strip-shaped region extending inward from the edge of the first side for 15 mm to 30 mm, a strip-shaped region extending inward from the edge of the third side for 15 mm to 30 mm, a strip-shaped region extending inward from the edge of the second side for 90 mm to 100 mm, and the area where the first side and the third side are located. The raw material of the epoxy insulating and anti-corrosion coating comprises the following components in parts by weight:
[0006] 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler.
[0007] According to a second aspect of the present invention, a method for preparing a zinc-electrode aluminum cathode plate is provided, comprising the following steps:
[0008] The area outside the coating coverage area of the aluminum substrate is masked to form a masked area, thus obtaining a first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end in the circumferential direction. The first side and the third side are arranged opposite to each other, and the second side and the fourth side are arranged opposite to each other. The coating coverage area includes a strip-shaped area extending 15mm to 30mm inward from the edge of the first side, a strip-shaped area extending 15mm to 30mm inward from the edge of the third side, and a strip-shaped area extending 90mm to 100mm inward from the edge of the second side.
[0009] The coated area is roughened to form a roughened region, thus obtaining a second aluminum plate;
[0010] The second aluminum plate is preheated, and then the raw material of epoxy insulating and anti-corrosion coating is electrostatically sprayed onto the roughened area to form a molten layer, thus obtaining the intermediate aluminum plate.
[0011] The intermediate aluminum plate is cured to obtain a zinc-electrode aluminum cathode plate.
[0012] The raw materials for epoxy insulating and anti-corrosion coatings include the following components in parts by weight: 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler.
[0013] By applying the technical solution of this invention, an epoxy insulating and anti-corrosion coating is applied to the edge and liquid level area of the aluminum substrate. This facilitates a tight bond between the coating and the aluminum substrate, leveraging the similarity in thermal expansion coefficients. This eliminates the micro-gaps caused by interfacial thermal stress differences in the traditional "coating + plastic edging" process, effectively reducing crevice corrosion and extending the service life of the zinc electrowinning aluminum cathode plate. Furthermore, the coating exhibits excellent corrosion resistance, is not prone to embrittlement or peeling, and contributes to long-term protection. The epoxy insulating and anti-corrosion coating provided by this invention also possesses high volume resistivity and mechanical strength, contributing to both insulation and mechanical protection. To better achieve the above effects, this invention also specifies the raw material components and dosage of the coating, with each component working synergistically to further optimize coating performance. Specifically, the reaction between epoxy resin and curing agent forms a dense three-dimensional network structure, which helps to provide a stable polymer skeleton and significantly improve mechanical strength and chemical corrosion resistance. Among these factors, the mass ratio of epoxy resin to filler is particularly critical. This ratio not only helps to improve the volume resistivity and mechanical properties of the coating, but also helps to precisely adjust the coefficient of thermal expansion of the coating to match the aluminum substrate, thereby improving the interfacial stability between the coating and the aluminum substrate under thermal cycling conditions. In addition, an appropriate amount of antioxidant helps to maintain the chemical stability of the coating under high-temperature curing and service environments, while lubricant helps to improve the melt flowability of the raw materials and promote the uniform dispersion of components to reduce internal defects, thereby further improving the density and adhesion of the coating. Attached Figure Description
[0014] Figure 1 This is a schematic diagram of the zinc electrowinning aluminum cathode plate in Embodiment 1 of the present invention.
[0015] Reference numerals: 1-First side; 2-Second side; 3-Third side; 4-Fourth side; 5-Conductive crossbeam. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0017] As described in the background of this invention, existing technologies are prone to crevice corrosion between the edge strip and the aluminum substrate, which limits the service life of the electrode plate. At the same time, the large difference in the coefficients of thermal expansion between aluminum and plastic further accelerates corrosion and electrode plate failure. To address the aforementioned problems, in a first typical embodiment of the present invention, a zinc electrowinning aluminum cathode plate is provided, comprising an aluminum substrate and an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate. The epoxy insulating and anti-corrosion coating is located in the coating coverage area of the aluminum substrate. The aluminum substrate has a first side, a second side, a third side, and a fourth side connected sequentially along its circumference. The first side and the third side are opposite to each other, and the second side and the fourth side are opposite to each other. The coating coverage area of the aluminum substrate includes a strip-shaped region extending inward from the edge of the first side for 15mm to 30mm, a strip-shaped region extending inward from the edge of the third side for 15mm to 30mm, a strip-shaped region extending inward from the edge of the second side for 90mm to 100mm, and the areas where the first and third sides are located. The raw material of the epoxy insulating and anti-corrosion coating comprises the following components in parts by weight:
[0018] 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler.
[0019] This invention utilizes an epoxy insulating and anti-corrosion coating applied to the edges and liquid level area of the aluminum substrate. This coating, with its similar coefficient of thermal expansion to the aluminum substrate, facilitates a tight bond between the two, eliminating the micro-gaps caused by interfacial thermal stress differences in the traditional "coating + plastic edging" process. This effectively reduces crevice corrosion and extends the service life of the zinc electrowinning aluminum cathode plate. Furthermore, the coating exhibits excellent corrosion resistance, is not prone to embrittlement or peeling, and contributes to long-term protection. The epoxy insulating and anti-corrosion coating provided by this invention also possesses high volume resistivity and mechanical strength. When the coating thickness meets the specified requirements, its insulation and mechanical protection properties are sufficient to replace traditional plastic insulating edging strips. Therefore, the injection molding or hot-pressing installation of plastic edging strips can be directly omitted, shortening the production process, improving production efficiency, and reducing equipment investment and labor costs. To better achieve the above effects, this invention also limits the raw material components and dosage of the coating, with each component working synergistically to further optimize coating performance. Specifically, the reaction between epoxy resin and curing agent forms a dense three-dimensional network structure, which helps to provide a stable polymer skeleton and significantly improve mechanical strength and chemical corrosion resistance. Among these factors, the mass ratio of epoxy resin to filler is particularly critical. This ratio not only helps to improve the volume resistivity and mechanical properties of the coating, but also helps to precisely adjust the coefficient of thermal expansion of the coating to match the aluminum substrate, thereby improving the interfacial stability between the coating and the aluminum substrate under thermal cycling conditions. In addition, an appropriate amount of antioxidant helps to maintain the chemical stability of the coating under high-temperature curing and service environments, while lubricant helps to improve the melt flowability of the raw materials and promote the uniform dispersion of components to reduce internal defects, thereby further improving the density and adhesion of the coating.
[0020] Typical, but not limiting, the epoxy resin in the raw materials of epoxy insulating and anti-corrosion coatings is in the range of 60 parts by weight, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, or any two of these values.
[0021] Typical, but not limiting, the curing agent in the raw materials of epoxy insulating and anti-corrosion coatings is in the range of 6 parts by weight, 6.1 parts, 6.2 parts, 6.3 parts, 6.4 parts, 6.5 parts, 6.6 parts, 6.7 parts, 6.8 parts, 6.9 parts, 7 parts, or any two of these values.
[0022] Typical, but not limited, amounts of antioxidant in the raw materials of epoxy insulating and anti-corrosion coatings are 2 parts by weight, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts, 4 parts, or any two of these values.
[0023] Typical, but not limiting, the lubricant in the raw materials of epoxy insulating and anti-corrosion coatings is 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, or any two of these values.
[0024] Typical, but not limiting, the filler weight in the raw materials of epoxy insulating and anti-corrosion coatings is 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, or any two of these values.
[0025] Specifically, the epoxy insulating and anti-corrosion coating is formed as follows: after preheating the aluminum substrate, the raw material for the epoxy insulating and anti-corrosion coating is electrostatically sprayed onto the intended coverage area to form a molten layer, followed by curing. This method helps to obtain a dense and continuous coating interface and improves the smoothness and thickness uniformity of the coating.
[0026] Specifically, the thickness of the epoxy insulating and anti-corrosion coating is ≥50μm.
[0027] Specifically, the zinc-electrode aluminum cathode plate also includes a conductive crossbeam located on the second side.
[0028] In some embodiments, when the thickness of the epoxy insulating anti-corrosion coating is ≥50μm and <3000μm, insulating strips are further provided on the first and third sides; the insulating strips include at least one of ABS strips, ethylene-acrylic acid copolymer (EAA) strips, PP strips, and PPO strips. In other embodiments, the thickness of the epoxy insulating anti-corrosion coating is 3000μm to 10mm, at which point the epoxy insulating anti-corrosion coating has sufficient insulation and mechanical protection properties, and there is no need to provide additional insulating strips.
[0029] In practical applications, the thickness of the epoxy insulating anti-corrosion coating can be rationally selected according to requirements. When the thickness of the epoxy insulating anti-corrosion coating is ≥50μm and <3000μm, using it in conjunction with insulating strips helps reduce crevice corrosion, extend the service life of the aluminum cathode plate, and the process is simple, efficient, and low-cost. When the thickness of the epoxy insulating anti-corrosion coating is 3000μm~10mm, its mechanical strength and insulation performance are similar to or better than the aforementioned insulating strips, and it can directly replace the aforementioned insulating strips. In addition to reducing crevice corrosion and extending the service life of the aluminum cathode plate, this solution also helps to shorten the production process, improve production efficiency, and significantly reduce costs.
[0030] In some embodiments, the coating coverage area also includes a strip-shaped region extending inward from the edge of the fourth side for 15mm to 30mm. Optionally, an insulating edge strip is also provided on the fourth side.
[0031] In some embodiments, the epoxy resin is selected from at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenolic epoxy resin, hydrogenated bisphenol A type epoxy resin, phenolic modified epoxy resin, and fluorine modified epoxy resin. Preferably, the epoxy resin is a bisphenol A type epoxy resin.
[0032] In the above embodiments of this application, by limiting the type of epoxy resin to the above range, it is helpful to form a continuous and dense polymer skeleton, which comprehensively improves the mechanical strength, corrosion resistance and insulation performance of the epoxy insulating and anti-corrosion coating. At the same time, it ensures that the epoxy insulating and anti-corrosion coating has good adhesion to the aluminum substrate, so that the epoxy insulating and anti-corrosion coating is tightly bonded to the aluminum substrate, thereby reducing interface corrosion and effectively extending the service life of the electrode plate.
[0033] In some embodiments, the curing agent is selected from at least one of dicyandiamide curing agents, phenolic curing agents, phenolic hydroxyl resin curing agents, and aromatic amine curing agents. By way of example and not limitation, dicyandiamide curing agents include dicyandiamide and its derivatives, phenolic curing agents include phenolic amines, and aromatic amine curing agents include 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, and m-phenylenediamine.
[0034] In the above embodiments of this application, by limiting the type of curing agent to the above range, it is helpful to form a dense three-dimensional network structure with good mechanical properties, improve the acid resistance, wear resistance and chemical corrosion resistance of the epoxy insulating anti-corrosion coating, and at the same time ensure good adhesion between the epoxy insulating anti-corrosion coating and the aluminum substrate, thereby extending the service life of the aluminum cathode plate.
[0035] In some embodiments, the filler is selected from at least one of silica and silicates. Preferably, the silicate is selected from at least one of mica, talc, kaolin, wollastonite, and montmorillonite.
[0036] In the above embodiments of this application, silicon oxide and silicates have good chemical stability, acid resistance and high insulation. By limiting the type of filler to the above range, on the one hand, it helps to form a stable inorganic reinforcing phase in the resin matrix, prolongs the diffusion path of the corrosive medium in the coating, thereby improving the hardness, density, insulation and corrosion resistance of the coating; on the other hand, it works synergistically with epoxy resin to regulate the coefficient of thermal expansion, so that it matches the coefficient of thermal expansion of the aluminum substrate, reduces thermal stress damage caused by inconsistent thermal expansion and contraction, thereby reducing the generation and propagation of microcracks at the interface, effectively reducing crevice corrosion and extending the service life of the aluminum cathode plate.
[0037] In practical applications, the filler can also contain appropriate amounts of micro-nano alumina, silicon carbide, ceramic powder, and other materials to enhance the wear resistance and insulation of the epoxy insulating and anti-corrosion coating.
[0038] In some embodiments, the antioxidant is selected from at least one of phosphite antioxidants and hindered phenolic antioxidants, wherein the phosphite antioxidant is selected from at least one of tris(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphite, and the hindered phenolic antioxidant is selected from at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and 2,6-di-tert-butyl-4-methylphenol.
[0039] In the above embodiments of this application, by limiting the types of antioxidants to the above range, it is helpful to improve the thermal stability of the coating raw materials during the melting and curing stages, and at the same time improve the aging resistance of the epoxy insulating anti-corrosion coating in high temperature acidic environment, thereby extending the service life of zinc electrolytic aluminum cathode plates.
[0040] In some embodiments, the antioxidant is selected from phosphite antioxidants and hindered phenolic antioxidants, with the mass ratio of phosphite antioxidants to hindered phenolic antioxidants being 1:(0.5~2).
[0041] In the above embodiments of this application, by compounding phosphite antioxidants and hindered phenolic antioxidants in the above mass ratio, it is helpful to enable the epoxy insulating anti-corrosion coating to maintain chemical stability over a wide temperature range for a long time, thereby extending the service life of the aluminum cathode plate.
[0042] In some embodiments, the lubricant is an amide lubricant, and the amide lubricant is selected from at least one of ethylene bis-stearamide, oleamide, erucamide, stearamide, N,N'-ethylene bis-oleamide, and N,N'-ethylene bis-stearamide.
[0043] In the embodiments described above in this application, amide-based lubricants refer to lubricating agents containing amide groups. By limiting the types of lubricants to the above range, it is helpful to improve the leveling and wettability of the raw materials of the epoxy insulating anti-corrosion coating during the melting process, while promoting the uniform dispersion of each component, thereby reducing internal and surface defects, improving density, enhancing the corrosion resistance of the coating, and extending the service life of the zinc electrowinning aluminum cathode plate.
[0044] In some embodiments, the raw materials of the epoxy insulating and anti-corrosion coating further include 0.1 to 1 part of a colorant, which is selected from at least one of titanium dioxide, carbon black, iron oxide red, iron oxide yellow, cobalt blue, chrome green, and titanium nickel yellow.
[0045] In the above embodiments of this application, by adding an appropriate amount of colorant, it is helpful to provide visual identification, thereby facilitating the identification of the coating coverage, thickness uniformity and local defects, so as to monitor the coating status of the epoxy insulating anti-corrosion coating, and at the same time to monitor quality and thickness.
[0046] In some embodiments, the aluminum substrate has a plurality of holes penetrating along the thickness direction, and the center of each hole is 4mm to 8mm away from the edge of the aluminum substrate. Preferably, the diameter of each hole is 4mm to 8mm. Preferably, the spacing between any adjacent holes is 5cm to 8cm. Specifically, the aforementioned plurality of holes includes a first through hole and a second through hole, the center of the first through hole being 4mm to 8mm away from the edge of the first side, and the center of the second through hole being 4mm to 8mm away from the edge of the third side. Optionally, when the coating coverage area includes a strip-shaped area extending inward from the edge of the fourth side for 15mm to 30mm, the aforementioned plurality of holes further includes a third through hole, the center of the third through hole being 4mm to 8mm away from the edge of the fourth side.
[0047] In the above embodiments of this application, the aforementioned holes are all located within the coverage area of the epoxy insulating and anti-corrosion coating. After the coating material cures on the hole walls, it forms a mechanical anchor with the aluminum substrate, which helps to enhance the bonding force between the epoxy insulating and anti-corrosion coating and the aluminum substrate, improve the structural stability of the coating, and thus extend the service life of the aluminum cathode plate. By limiting the hole diameter within the above range, it helps to promote the full flow of the coating material into the holes in a molten state, enhance the bonding force between the epoxy insulating and anti-corrosion coating and the aluminum substrate, and maintain the edge structural stability of the aluminum substrate. By limiting the hole spacing within the above range, it helps to improve the mechanical anchoring strength, while ensuring that the edge of the aluminum substrate and its vicinity still have sufficient mechanical properties. When insulating strips are provided on the first, third, and fourth sides (if any), the injection molding material cures within the holes, which helps to improve the bonding force between the insulating strips and the aluminum substrate and improve the structural stability of the electrode plate edge.
[0048] In some embodiments, the coating coverage area of the aluminum substrate also includes a strip-shaped area extending inward from the edge for 15 mm to 30 mm along the fourth side.
[0049] In some embodiments, the coating area of the aluminum substrate also has an anchor pattern with a depth of 10 μm to 100 μm.
[0050] In the above embodiments of this application, the anchor pattern structure helps to increase the surface roughness of the coating coverage area, and at the same time significantly increases the actual contact area between the coating and the aluminum substrate, thereby significantly enhancing the interfacial bonding force between the coating and the aluminum substrate.
[0051] In a second typical embodiment of the present invention, a method for preparing a zinc-electrode aluminum cathode plate in the first typical embodiment is provided, which includes the following steps:
[0052] The area outside the coating coverage area of the aluminum substrate is masked to form a masked area, thus obtaining a first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end in the circumferential direction. The first side and the third side are arranged opposite to each other, and the second side and the fourth side are arranged opposite to each other. The coating coverage area includes a strip-shaped area extending 15mm to 30mm inward from the edge of the first side, a strip-shaped area extending 15mm to 30mm inward from the edge of the third side, and a strip-shaped area extending 90mm to 100mm inward from the edge of the second side.
[0053] The coated area is roughened to form a roughened region, thus obtaining a second aluminum plate;
[0054] The second aluminum plate is preheated, and then the raw material of epoxy insulating and anti-corrosion coating is electrostatically sprayed onto the roughened area to form a molten layer, thus obtaining the intermediate aluminum plate.
[0055] The intermediate aluminum plate is cured to obtain a zinc-electrode aluminum cathode plate.
[0056] The raw materials for the epoxy insulating and anti-corrosion coating comprise the following components in parts by weight: 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler. Preferably, the raw materials for the epoxy insulating and anti-corrosion coating further comprise 0.1-1 parts colorant.
[0057] In this invention, through specific pretreatment, preheating, electrostatic spraying and curing processes, the epoxy insulating and anti-corrosion coating and the aluminum substrate are integrated, which effectively solves the problems of corrosion and edge strip detachment caused by interface gaps in the traditional coating and insulating edge strip combination process, and simplifies the production process.
[0058] First, masking areas that do not require coating ensures that the epoxy insulating and anti-corrosion coating only covers areas prone to electric field distortion, preventing contamination of the effective working area of the aluminum cathode plate and guaranteeing electrowinning efficiency. Roughening treatment not only helps remove oxide films and oil stains from the aluminum substrate surface but also creates a uniform anchor pattern structure, increasing the surface roughness of the coated area. This significantly increases the actual contact area between the coating and the substrate, allowing the molten epoxy resin to penetrate into the grooves on the aluminum substrate surface, improving coating adhesion and extending the service life of the aluminum cathode plate.
[0059] Secondly, the synergy between preheating and electrostatic spraying helps to integrate the epoxy insulating and anti-corrosion coating into a single unit. This not only ensures a tight bond between the coating and the aluminum plate, reducing crevice corrosion and extending plate life, but also shortens the process and reduces equipment and labor costs. In this invention, the aluminum substrate is first preheated to a suitable temperature. Then, a high-voltage electrostatic field attracts negatively charged coating particles to the positively charged aluminum substrate, achieving uniform adsorption of the raw material powder on the aluminum plate surface. The temperature of the aluminum substrate then completely melts the raw material powder into a highly fluid resin melt, fully wetting and filling the microscopic unevenness of the aluminum substrate surface. The resulting epoxy insulating and anti-corrosion coating powder adheres uniformly and has a controllable thickness. The coating is uniform and regular at the plate edges and liquid level areas, facilitating tight adhesion of the subsequent injection molding edge banding and reducing secondary voids at the double-layer interface. Furthermore, due to the dense packing of powder particles under electrostatic action, internal pores and defects are reduced, which is beneficial for forming a dense, pinhole-free continuous coating during the subsequent melting and leveling process. This significantly improves the mechanical properties and corrosion resistance of the coating. Simultaneously, because the coefficient of thermal expansion of the formed coating matches that of the aluminum substrate, thermal stress during the curing and cooling process is reduced, which also helps to lower the risk of coating cracking. It should be noted that electrostatic spraying is the most suitable spraying technology for the present invention, but in practical applications, the spraying technology is not limited to electrostatic spraying. As long as the raw material of the epoxy insulating and anti-corrosion coating forms a uniform molten layer on the aluminum plate surface, flame spraying technology or any of the spraying technologies included in the fusion powder coating process can also be used.
[0060] Finally, this method, by optimizing the raw material composition and ratio and combining it with electrostatic spraying, enables the prepared epoxy insulating and anti-corrosion coating to possess sufficient mechanical strength and insulation properties. In particular, when the coating thickness meets the set requirements, its protective performance is sufficient to replace traditional plastic insulating edging strips, thus eliminating the complex injection molding and hot-pressing installation processes in the production flow. This not only significantly improves efficiency but also reduces equipment investment and labor costs. Simultaneously, because the coating is integrated with the aluminum substrate, the corrosion resistance of the epoxy insulating and anti-corrosion coating is significantly improved, effectively reducing crevice corrosion and extending the service life of zinc electrowinning aluminum cathode plates, thereby improving the overall efficiency and economy of zinc electrowinning production.
[0061] In some embodiments, the roughening treatment includes a degreasing treatment and a mechanical roughening treatment performed sequentially, wherein the mechanical roughening treatment includes any one of sandblasting, shot blasting, and grinding.
[0062] In the above embodiments of this application, the purpose of degreasing treatment is to remove oxide film, oil stains and impurities from the surface of the aluminum substrate, and the purpose of mechanical roughening treatment is to form anchor patterns on the surface of the aluminum substrate, thereby increasing the effective contact area and mechanical interlocking force between the epoxy insulating anti-corrosion coating and the aluminum substrate, enhancing the interfacial bonding force between the two, thereby reducing crevice corrosion and extending the service life of the aluminum cathode plate.
[0063] In some embodiments, the abrasive used in the sandblasting process is aluminum oxide (Al2O3).
[0064] In the embodiments described above, aluminum oxide (Al₂O₃) possesses high hardness and stable chemical properties. The abrasive used in the sandblasting process, Al₂O₃, helps to efficiently remove oxide films, oil stains, and impurities from the aluminum plate surface, while simultaneously forming uniform anchor patterns on the aluminum plate surface, thereby enhancing the adhesion between the epoxy insulating and anti-corrosion coating and the aluminum substrate. Further limiting the particle size of the aluminum oxide within the aforementioned range helps to control the surface roughness of the aluminum plate to a suitable range, forming uniform anchor patterns of appropriate depth. This balances the adhesion between the coating and the aluminum substrate, the smoothness of the coating surface, and the uniformity of the coating thickness, thereby extending the service life of the zinc electrowinning aluminum cathode plate.
[0065] In some implementations, the sandblasting pressure is 0.5 MPa to 0.7 MPa.
[0066] In the above embodiments of this application, by limiting the sandblasting pressure within the above range, it helps to provide sufficient kinetic energy to clean the surface of the aluminum plate and form a uniform and moderate roughness, thereby improving the adhesion between the coating and the aluminum substrate. At the same time, the appropriate sandblasting pressure can also ensure that the aluminum substrate maintains structural stability and mechanical property stability during the sandblasting process.
[0067] In some implementations, the roughened region has anchor patterns with a depth of 10 μm to 100 μm.
[0068] In the embodiments described above, the anchor pattern is a micro-uneven structure formed after roughening treatment. By limiting the depth of the anchor pattern within the aforementioned range, it helps to balance the bonding force between the epoxy insulating and anti-corrosion coating and the aluminum substrate, the smoothness of the coating, and the uniformity of the coating thickness. This allows the epoxy insulating and anti-corrosion coating to maintain structural stability for a long time in a high-temperature acidic corrosive environment, while maintaining a tight interface between the coating and the aluminum substrate, thereby extending the service life of the zinc electrowinning aluminum cathode plate.
[0069] In some embodiments, the sandblasting process also includes purging or ultrasonic cleaning after sandblasting, with compressed air used for purging.
[0070] In the embodiments described above, purging or ultrasonic cleaning helps to thoroughly remove abrasive particles, dust, and impurities remaining on the surface and in the pores of the aluminum plate, thereby reducing coating defects. Using compressed air purging helps to quickly and thoroughly clean the aluminum plate surface, enhancing the adhesion between the epoxy insulating and anti-corrosion coating and the aluminum plate.
[0071] In some embodiments, the masking process involves using a metal masking plate to mask the area of the aluminum substrate other than the coating area; the metal masking plate is selected from at least one of stainless steel masking plates, aluminum alloy masking plates, and titanium masking plates.
[0072] In the above embodiments of this application, shielding plates made of metals such as stainless steel, aluminum alloy, and titanium have excellent high-temperature resistance, which helps to maintain shape stability and chemical stability during subsequent preheating and curing processes, thereby ensuring clear and neat coating boundaries and improving the appearance quality and process consistency of the aluminum cathode plate.
[0073] In some embodiments, the preheating temperature is 160℃~220℃, and the holding time is 10min~40min. Preferably, it is 180℃~200℃, and the holding time is 15min~25min.
[0074] In the embodiments described above, by limiting the preheating temperature and time within the aforementioned range, it helps the raw materials of the epoxy insulating and anti-corrosion coating to melt rapidly and spread evenly upon contact with the aluminum plate, thereby improving the thickness uniformity and density of the resulting coating, effectively protecting the edges of the aluminum cathode plate and extending its service life. Furthermore, preheating within the aforementioned range also helps maintain the structural and shape stability of the aluminum plate, thereby improving the overall quality of the aluminum cathode plate.
[0075] In some embodiments, the curing temperature is 160℃~220℃, and the holding time is 15min~60min. Preferably, it is 180℃~200℃, and the holding time is 25min~40min.
[0076] In the embodiments described above, limiting the curing temperature and time within the aforementioned range helps to promote the full cross-linking and curing of the epoxy resin, forming a stable and dense three-dimensional network structure. This improves the mechanical properties, corrosion resistance, insulation properties, and interfacial bonding strength between the epoxy insulating and anti-corrosion coating and the aluminum substrate, thereby enhancing the edge protection capability of the zinc electrowinning aluminum cathode plate. Furthermore, this temperature range also helps to maintain the structural and shape stability of the aluminum plate, thus improving the overall quality of the aluminum cathode plate.
[0077] In some embodiments, the method for preparing the zinc-electrode aluminum cathode plate further includes performing a silane coupling treatment on the roughened region after the roughening treatment. The silane coupling treatment method includes: spraying a silane coupling agent solution onto the roughened region, allowing it to stand for 1 to 5 minutes, and then drying it at 100°C to 180°C for 5 to 40 minutes to form a silane-treated region. Preferably, the silane coupling agent solution contains a silane coupling agent selected from at least one of γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and γ-mercaptopropyltrimethoxysilane, and the mass concentration of the silane coupling agent in the silane coupling agent solution is 0.5 wt% to 2.0 wt%. The solvent of the silane coupling agent solution is water.
[0078] In the embodiments described above, performing silane coupling treatment before electrostatic spraying helps form a transitional bonding layer between the aluminum substrate and the epoxy insulating anti-corrosion coating, thereby improving their interfacial compatibility and bonding strength. This reduces electrolyte penetration, delays corrosion, and effectively extends the service life of the aluminum cathode plate. By limiting the process conditions of the silane coupling treatment within the aforementioned range, it helps the silane coupling agent to fully adhere to and uniformly cover the aluminum plate surface. This allows the silane coupling agent to fully interact with the epoxy resin during subsequent spraying and curing, further improving the interfacial bonding strength between the epoxy insulating anti-corrosion coating and the aluminum substrate, and extending the service life of the aluminum cathode plate. By limiting the type and concentration of the silane coupling agent, it helps to control the content of silane coupling agent adhering to the aluminum plate surface to a suitable range and promotes the full reaction between the silane coupling agent and the epoxy resin, improving the anti-peeling ability of the epoxy insulating anti-corrosion coating under high-temperature acidic corrosion environments.
[0079] In some embodiments, the method for preparing the zinc electrowinning aluminum cathode plate further includes punching holes in the coating area before the masking process. Specifically, the center of the punched hole is 4 mm to 8 mm away from the edge of the aluminum substrate.
[0080] In the embodiments described above, the punching process plays a crucial role in subsequent processes: molten epoxy material flows into these holes penetrating the thickness of the aluminum substrate during preheating and curing, and solidifies on the hole walls. This allows the epoxy insulating and anti-corrosion coatings on both sides of the aluminum plate to connect through the coating material within the holes, forming a mechanical anchoring structure similar to a latch. This not only enhances the bonding force between the epoxy insulating and anti-corrosion coating and the aluminum substrate in the thickness direction but also effectively improves the structural stability of the coating when subjected to the mechanical impact of zinc stripping, making the coating less prone to curling or peeling, thereby extending the service life of the aluminum cathode plate. In actual operation, the punching can also be adjusted according to process requirements, where the coating-covered area of the aluminum substrate is punched after the shielding treatment. When insulating strips are provided on the first, third, and fourth sides (if any), the injection molding material solidifies within the aforementioned holes, which helps to improve the bonding force between the insulating strips and the aluminum substrate, and enhances the structural stability of the electrode edge.
[0081] Specifically, the punching equipment only needs to meet the requirements for hole diameter and hole spacing; it can be a punching blanking machine. In practical applications, after punching, the edges of the holes are usually ground and deburred to obtain a smoother surface.
[0082] In some embodiments, when the thickness of the epoxy insulating anti-corrosion coating is ≥50μm and less than 3000μm, the material obtained after curing is referred to as a semi-finished aluminum cathode plate. Insulating strips are then installed at the edges of the zinc-electrodelated aluminum cathode plate using an injection molding process. The injection molding process specifically includes the following steps:
[0083] The semi-finished aluminum cathode plate is placed into the injection mold as an insert, and the insert is preheated to 75℃~150℃;
[0084] The temperature of the injection molding barrel is controlled at 180℃~250℃ for mold filling, and the total mold filling time is 1s~10s. When the cavity is filled to 94%~97%, the injection method is changed from constant speed injection to holding pressure stage to avoid overfilling and generating residual internal stress.
[0085] The molding process employs a two-stage pressure holding and shrinkage compensation process. The first-stage pressure holding is set at 45 bar to 85 bar and the holding time is 3 to 15 seconds. The second-stage pressure holding is set at 25 bar to 55 bar and the holding time is 3 to 15 seconds. The total holding time is 6 to 30 seconds, in order to compensate for the volume shrinkage caused by the cooling of the plastic and to compact the aluminum-plastic interface.
[0086] Finally, after cooling and shaping at 15℃~25℃ for 60s~100s, the plate is demolded to obtain a zinc-electrode aluminum cathode plate.
[0087] Injection molding materials include at least one of ABS, EAA, PP, and PPO.
[0088] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0089] Example 1
[0090] This embodiment provides a zinc-electrode aluminum cathode plate, the preparation method of which is as follows:
[0091] Step S1: Punch holes in the coating area of the aluminum substrate to form several holes (including a first through hole and a second through hole). The diameter of each hole is 6 mm, the spacing between adjacent holes is 6.5 cm, and the center of the hole is 6 mm away from the edge of the aluminum plate. Then, use an aluminum alloy shielding plate to shield the area outside the coating area to form a shielded area, thus obtaining the first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end along the circumference. The first side and the third side are opposite to each other, and the second side and the fourth side are opposite to each other. The coating area includes a strip-shaped area extending 23 mm inward from the edge of the first side, a strip-shaped area extending 23 mm inward from the edge of the third side, and a strip-shaped area extending 90 mm inward from the edge of the second side. The center of the first through hole is 6 mm away from the edge of the first side, and the center of the second through hole is 6 mm away from the edge of the third side.
[0092] Step S2: The coating area is subjected to degreasing and sandblasting treatments in sequence to form a roughened area with anchor patterns. In the degreasing treatment, an alkaline degreasing solution is used to remove oil stains and processing residues from the surface of the coating area. In the sandblasting treatment, aluminum oxide is used as the abrasive, the pressure is 0.6 MPa, and the depth of the resulting anchor pattern is 50 μm.
[0093] Step S3: Spray the silane coupling agent solution onto the roughened area, let it stand for 3 minutes, and then dry it at 140°C for 25 minutes to form a silane-treated area, obtaining the second aluminum plate. The silane coupling agent solution is prepared using γ-aminopropyltriethoxysilane and deionized water, with a γ-aminopropyltriethoxysilane mass concentration of 1.2 wt%. Next, the second aluminum plate is preheated at 200°C for 20 minutes. Then, the epoxy insulating and anti-corrosion coating material is electrostatically sprayed onto the silane-treated area to form a molten layer, obtaining the intermediate aluminum plate. The intermediate aluminum plate is cured at 200°C for 32 minutes to form an epoxy insulating and anti-corrosion coating with a thickness of 3000 μm. After curing, the aluminum alloy shielding plate is removed, obtaining the zinc-electrode aluminum cathode plate. The zinc electrowinning aluminum cathode plate comprises an aluminum substrate, an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate, and a conductive crossbeam. The epoxy insulating and anti-corrosion coating is located within the coating-covered area of the aluminum substrate. The dimensions of the aluminum substrate are 1200mm × 800mm × 7mm (length × width × thickness). Figure 1As shown, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end-to-end along the circumference. The first side and the third side are positioned opposite each other, and the second side and the fourth side are positioned opposite each other. The coating coverage area includes a strip-shaped region extending 23 mm inward from the edge along the first side, a strip-shaped region extending 23 mm inward from the edge along the third side, a strip-shaped region extending 90 mm inward from the edge along the second side, and the areas containing the first and third sides. The conductive beam is located on the second side of the aluminum substrate.
[0094] The epoxy insulating and anti-corrosion coating contains the following components in parts by weight: 65 parts solid bisphenol A epoxy resin, 6.5 parts 4,4'-diaminodiphenylmethane, 1.5 parts tris(2,4-di-tert-butylphenyl)phosphite, 1.5 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1 part micronized ethylene bis-stearamide, 8.5 parts fused silica micronized powder, 8.5 parts potassium aluminum layered mica powder, and 0.5 parts carbon black powder.
[0095] Example 2
[0096] The difference between this embodiment and Embodiment 1 is that the preparation method of the zinc electrowinning aluminum cathode plate is as follows:
[0097] Step S1: Punch holes in the coating area of the aluminum substrate to form several holes (including a first through hole and a second through hole). The diameter of each hole is 4 mm, the spacing between adjacent holes is 5 cm, and the center of the hole is 4 mm away from the edge of the aluminum plate. Then, a stainless steel shielding plate is used to shield the area outside the coating area to form a shielded area, thus obtaining the first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end along the circumference. The first side and the third side are opposite to each other, and the second side and the fourth side are opposite to each other. The coating area includes a strip-shaped area extending 15 mm inward from the edge of the first side, a strip-shaped area extending 15 mm inward from the edge of the third side, and a strip-shaped area extending 100 mm inward from the edge of the second side. The center of the first through hole is 5 mm away from the edge of the first side, and the center of the second through hole is 5 mm away from the edge of the third side.
[0098] Step S2: The coating area is subjected to degreasing and sandblasting treatments in sequence to form a roughened area with anchor patterns. In the degreasing treatment, an alkaline degreasing solution is used to remove oil stains and processing residues from the surface of the coating area. In the sandblasting treatment, aluminum oxide is used as the abrasive, the pressure is 0.5 MPa, and the depth of the resulting anchor pattern is 10 μm.
[0099] Step S3: Spray the silane coupling agent solution onto the roughened area, let it stand for 1 min, and then dry it at 100℃ for 40 min to form a silane-treated area, obtaining the second aluminum plate. The silane coupling agent solution is prepared using γ-aminopropyltriethoxysilane and deionized water, with a γ-aminopropyltriethoxysilane mass concentration of 0.5 wt%. Next, the second aluminum plate is preheated at 180℃ for 25 min, and then the epoxy insulating and anti-corrosion coating material is electrostatically sprayed onto the silane-treated area to form a molten layer, obtaining the intermediate aluminum plate. The intermediate aluminum plate is cured at 180℃ for 40 min to form an epoxy insulating and anti-corrosion coating with a thickness of 5000 μm. After curing, the stainless steel shielding plate is removed, obtaining the zinc electrowinning aluminum cathode plate. The zinc electrowinning aluminum cathode plate comprises an aluminum substrate, an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate, and a conductive beam. The epoxy insulating and anti-corrosion coating is located within the coating-covered area of the aluminum substrate. The aluminum substrate measures 1200mm × 800mm × 7mm (length × width × thickness) and has four sides arranged sequentially along its circumference: a first side, a second side, a third side, and a fourth side. The first and third sides are opposite each other, as are the second and fourth sides. The coating-covered area includes a strip extending 15mm inward from the edge along the first side, a strip extending 15mm inward from the edge along the third side, a strip extending 100mm inward from the edge along the second side, and the areas containing the first and third sides. The conductive beam is located on the second side of the aluminum substrate.
[0100] The epoxy insulating and anti-corrosion coating contains the following components in parts by weight: 60 parts of solid bisphenol A type epoxy resin, 6 parts of 4,4'-diaminodiphenylmethane, 1 part of tris(2,4-di-tert-butylphenyl)phosphite, 1 part of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1.5 parts of micronized ethylene bis-stearamide, 10 parts of fused silica micronized powder, 10 parts of potassium aluminum layered mica powder, and 1 part of carbon black powder.
[0101] Example 3
[0102] The difference between this embodiment and Embodiment 1 is that the preparation method of the zinc electrowinning aluminum cathode plate is as follows:
[0103] Step S1: Punch holes in the coating area of the aluminum substrate to form several holes (including a first through hole and a second through hole). The diameter of each hole is 8 mm, the spacing between adjacent holes is 8 cm, and the center of the hole is 8 mm away from the edge of the aluminum plate. Then, a titanium shielding plate is used to shield the area outside the coating area to form a shielded area, thus obtaining the first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end along the circumference. The first side and the third side are opposite to each other, and the second side and the fourth side are opposite to each other. The coating area includes a strip-shaped area extending 30 mm inward from the edge of the first side, a strip-shaped area extending 30 mm inward from the edge of the third side, and a strip-shaped area extending 95 mm inward from the edge of the second side. The center of the first through hole is 8 mm away from the edge of the first side, and the center of the second through hole is 8 mm away from the edge of the third side.
[0104] Step S2: The coating area is subjected to degreasing and sandblasting treatments in sequence to form a roughened area with anchor patterns. In the degreasing treatment, an alkaline degreasing solution is used to remove oil stains and processing residues from the surface of the coating area. In the sandblasting treatment, aluminum oxide is used as the abrasive, the pressure is 0.7 MPa, and the depth of the resulting anchor pattern is 100 μm.
[0105] Step S3: Spray the silane coupling agent solution onto the roughened area, let it stand for 5 minutes, and then dry it at 180°C for 5 minutes to form a silane-treated area, obtaining the third aluminum plate. The silane coupling agent solution is prepared using γ-aminopropyltriethoxysilane and deionized water, with a γ-aminopropyltriethoxysilane mass concentration of 2.0 wt%. Next, the second aluminum plate is preheated at 200°C for 15 minutes. Then, the epoxy insulating and anti-corrosion coating material is electrostatically sprayed onto the silane-treated area to form a molten layer, obtaining the intermediate aluminum plate. The intermediate aluminum plate is cured at 200°C for 25 minutes to form a 10 mm thick epoxy insulating and anti-corrosion coating. After curing, the titanium shielding plate is removed, obtaining the zinc electrowinning aluminum cathode plate. The zinc electrowinning aluminum cathode plate comprises an aluminum substrate, an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate, and a conductive beam. The epoxy insulating and anti-corrosion coating is located within the coating-covered area of the aluminum substrate. The aluminum substrate measures 1200mm × 800mm × 7mm (length × width × thickness) and has four sides arranged sequentially along its circumference: a first side, a second side, a third side, and a fourth side. The first and third sides are opposite each other, as are the second and fourth sides. The coating-covered area includes a strip extending 30mm inward from the edge along the first side, a strip extending 30mm inward from the edge along the third side, a strip extending 95mm inward from the edge along the second side, and the areas containing the first and third sides. The conductive beam is located on the second side of the aluminum substrate.
[0106] The epoxy insulating and anti-corrosion coating contains the following components in parts by weight: 70 parts of solid bisphenol A type epoxy resin, 7 parts of 4,4'-diaminodiphenylmethane, 2 parts of tris(2,4-di-tert-butylphenyl)phosphite, 2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 0.5 parts of micronized ethylene bis-stearamide, 7.5 parts of fused silica micronized powder, 8 parts of potassium aluminum layered mica powder, and 0.1 parts of carbon black powder.
[0107] Example 4
[0108] The difference between this embodiment and Embodiment 1 is that in step S3, the thickness of the epoxy insulating and anti-corrosion coating is 800μm. After the curing process is completed, the aluminum alloy shielding plate is removed to obtain the aluminum cathode plate semi-finished product. Then, ABS insulating strips are installed on the edge of the aluminum cathode plate semi-finished product using an injection molding process. The injection molding process is as follows:
[0109] The aforementioned aluminum cathode plate semi-finished product was placed into the injection mold as an insert, and the insert was preheated to 110°C. Subsequently, the injection barrel temperature was controlled at 210°C for mold filling, with a total filling time of 5 seconds. When the cavity was 95% filled, the injection method was switched from constant-speed injection to a holding pressure stage to avoid overfilling and residual internal stress. The molding process adopted a two-stage holding pressure compensation process. The first stage holding pressure was set at 65 bar with a holding time of 9 seconds, and the second stage holding pressure was set at 40 bar with a holding time of 9 seconds, for a total holding time of 18 seconds, to compensate for the volume shrinkage caused by plastic cooling and to compact the aluminum-plastic interface. Finally, after cooling and setting at 25°C for 60 seconds, the plate was demolded to obtain the zinc electrowinning aluminum cathode plate.
[0110] The zinc electrowinning aluminum cathode plate comprises an aluminum substrate, an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate, an ABS insulating edging strip covering the edges of the aluminum substrate, and a conductive beam. The epoxy insulating and anti-corrosion coating is located within the coating-covered area of the aluminum substrate. The aluminum substrate measures 1200mm × 800mm × 7mm (length × width × thickness) and has four sides arranged sequentially along its circumference: a first side, a second side, a third side, and a fourth side. The first and third sides are opposite each other, as are the second and fourth sides. The coating-covered area includes a strip extending 23mm inward from the edge along the first side, a strip extending 23mm inward from the edge along the third side, a strip extending 90mm inward from the edge along the second side, and the areas containing the first and third sides. The ABS insulating edging strip is located on the first and third sides of the aluminum substrate, and the conductive beam is located on the second side of the aluminum substrate.
[0111] Example 5
[0112] The difference between this embodiment and Embodiment 1 is that in step S3, the preheating temperature is 160°C and the holding time is 40 min; the curing temperature is 160°C and the holding time is 60 min.
[0113] Example 6
[0114] The difference between this embodiment and Embodiment 1 is that in step S3, the preheating temperature is 220°C and the holding time is 10 min; the curing temperature is 220°C and the holding time is 15 min.
[0115] Example 7
[0116] The difference between this embodiment and Embodiment 1 is that silane coupling treatment is not performed in step S3, and the aluminum plate obtained after sandblasting is directly preheated.
[0117] Example 8
[0118] The difference between this embodiment and Embodiment 1 is that in step S1, the aluminum substrate is not punched, and the area outside the coating coverage area is directly masked.
[0119] Comparative Example 1
[0120] The difference between this comparative example and Example 1 is that a modified vinyl coating combined with an insulating edge strip is used to protect the edge of the zinc electrowinning aluminum cathode plate. Specifically, in the preparation method, steps S1 to S2 are the same as in Example 1, but in step S3, silane coupling treatment is not performed, and the modified vinyl coating is directly brushed onto the roughened area, including the following steps:
[0121] A transparent vinyl ester primer and hardener were uniformly mixed at a mass ratio of 50:1 and brushed onto the roughened area. The mixture was then allowed to dry naturally at 25°C for 45 minutes, until the primer surface was completely cured. Next, a white vinyl ester topcoat and hardener were mixed at the same mass ratio of 50:1 and brushed onto the primer surface. The mixture was then dried at 25°C for 1 hour. Once the coating reached a non-flowing state, it was cured at 60°C for 8 hours, forming a modified vinyl ester coating with a thickness of 800 μm (primer to topcoat thickness ratio of 3:1), resulting in a semi-finished aluminum cathode plate. Finally, ABS insulating strips were installed along the edges of the semi-finished aluminum cathode plate using an injection molding process.
[0122] The injection molding process is as follows:
[0123] The aforementioned aluminum cathode plate semi-finished product was placed into the injection mold as an insert, and the insert was preheated to 110°C. Subsequently, the injection barrel temperature was controlled at 210°C for mold filling, with a total filling time of 5 seconds. When the cavity was 95% filled, the injection method was switched from constant-speed injection to a holding pressure stage to avoid overfilling and residual internal stress. The molding process adopted a two-stage holding pressure compensation process. The first stage holding pressure was set at 65 bar with a holding time of 9 seconds, and the second stage holding pressure was set at 40 bar with a holding time of 9 seconds, for a total holding time of 18 seconds, to compensate for the volume shrinkage caused by plastic cooling and to compact the aluminum-plastic interface. Finally, after cooling and setting at 25°C for 60 seconds, the plate was demolded to obtain the zinc electrowinning aluminum cathode plate.
[0124] The zinc electrowinning aluminum cathode plate comprises an aluminum substrate, an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate, an ABS insulating edging strip covering the edges of the aluminum substrate, and a conductive beam. The epoxy insulating and anti-corrosion coating is located within the coating-covered area of the aluminum substrate. The aluminum substrate measures 1200mm × 800mm × 7mm (length × width × thickness) and has four sides arranged sequentially along its circumference: a first side, a second side, a third side, and a fourth side. The first and third sides are opposite each other, as are the second and fourth sides. The coating-covered area includes a strip extending 23mm inward from the edge along the first side, a strip extending 23mm inward from the edge along the third side, a strip extending 90mm inward from the edge along the second side, and the areas containing the first and third sides. The ABS insulating edging strip is located on the first and third sides of the aluminum substrate, and the conductive beam is located on the second side of the aluminum substrate.
[0125] Comparative Example 2
[0126] The difference between this comparative example and Example 4 is that the zinc electrolytic aluminum cathode plate has no epoxy insulating and anti-corrosion coating, and the first and third sides of the aluminum substrate are equipped with ABS insulating strips (the aluminum substrate is directly injection molded).
[0127] Comparative Example 3
[0128] The difference between this comparative example and Example 1 is that, in the raw materials of the epoxy insulating and anti-corrosion coating, the weight parts of solid bisphenol A type epoxy resin are 75 parts, the weight parts of fused silica micro powder are 7.5 parts, and the weight parts of potassium aluminum layered mica powder are 7.5 parts.
[0129] Comparative Example 4
[0130] The difference between this comparative example and Example 1 is that in step S3, electrostatic spraying is not used. Instead, manual powdering is used to deposit the raw material of the epoxy insulating and anti-corrosion coating onto the silane treatment area of the second aluminum plate to form a molten layer and obtain the intermediate aluminum plate.
[0131] Comparative Example 5
[0132] The difference between this comparative example and Example 1 is that, instead of degreasing and sandblasting, the silane coupling agent solution is directly sprayed onto the area of the first aluminum plate, excluding the shielded area.
[0133] Performance testing
[0134] The corrosion resistance of the zinc electrowinning aluminum cathode plates prepared in Examples 1-8 and Comparative Examples 1-5 was tested.
[0135] Test methods
[0136] (1) Corrosion resistance test (laboratory):
[0137] A high-concentration electrolyte was prepared, using a zinc-electrode aluminum cathode plate as the cathode and a lead-silver alloy anode plate as the anode. The system was operated at 60℃ to accelerate cyclic electrodeposition. Every 3 hours, the aluminum cathode plate was removed, the edge condition was recorded, and the electrolyte was replaced. The time it took for corrosion cracks to appear on the aluminum plate edge and reach a length of 1 cm was recorded as the corrosion resistance time. The longer this time, the better the corrosion resistance of the zinc-electrode aluminum cathode plate. The current density was 600 A / m. 2 The electrolyte formula is as follows:
[0138] ZnSO4 60g / L;
[0139] H2SO4 180g / L;
[0140] Cl - 800 mg / L;
[0141] F - 200 mg / L.
[0142] (2) Corrosion resistance test (actual working conditions):
[0143] The zinc-electrode aluminum cathode plates prepared in Example 1 and Comparative Example 2 were put into actual operation verification on a zinc electrodeposition production line for 3 months (90 days). The zinc-electrode aluminum cathode plate served as the cathode, and the lead-silver alloy electrode plate served as the anode. The operating temperature was 50°C, and the current density was 600 A / m. 2 The electrolyte formula is as follows:
[0144] ZnSO4 60g / L;
[0145] H2SO4 150g / L;
[0146] Cl - 800 mg / L;
[0147] F - 200 mg / L.
[0148] After the operation is completed, the edge condition of the zinc electrowinning aluminum cathode plate is evaluated according to Table 1.
[0149] Table 1
[0150]
[0151] The performance test results of the above embodiments and comparative examples are shown in Table 2.
[0152] Table 2
[0153]
[0154] As shown in Table 2, the zinc-electrode aluminum cathode plates prepared in Examples 1-8 exhibit significantly better corrosion resistance than those in Comparative Examples 1-5. Their corrosion resistance in high-concentration electrolyte in the laboratory reaches 78-132 hours. After 90 days of operation under actual working conditions, the coating shows no peeling, and the aluminum cathode plate exhibits good side morphology (no visible gaps or gap length < 5 cm at the interface between the aluminum substrate and the coating, and no corrosion pits on the aluminum substrate surface). This indicates that the zinc-electrode aluminum cathode plate provided by this invention can effectively solve the corrosion and edge strip peeling problems caused by interface gaps in traditional processes, significantly improving the corrosion resistance of the cathode plate and extending its service life. Furthermore, comparing Examples 1-3 with Example 4, it can be seen that when the thickness of the epoxy insulating anti-corrosion coating is 3000μm~10mm, the zinc electrolytic aluminum cathode plate can be put into normal use without the installation of plastic insulating edging strips. This indicates that its mechanical strength and insulation performance are sufficient to replace the traditional plastic insulating edging strips, and the process of injection molding or hot pressing to install plastic edging strips can be directly omitted, thereby shortening the production process, improving production efficiency, and significantly reducing costs.
[0155] Compared with Examples 5-6, Examples 1-4 further optimized the preheating temperature and curing temperature. On the one hand, this helps to promote the timely melting and uniform spreading of the raw material powder after it is adsorbed on the surface of the aluminum plate, thereby improving the thickness uniformity and density of the obtained epoxy insulating anti-corrosion coating. At the same time, the moderate temperature also helps to maintain the structural and shape stability of the aluminum plate, which is more conducive to the tight adhesion of the coating to the aluminum plate, further improving the corrosion resistance and the overall quality of the aluminum cathode plate.
[0156] Compared with Example 7, Examples 1-4 added a silane coupling treatment step. By forming a transition bonding layer between the aluminum substrate and the epoxy insulating anti-corrosion coating, it helps to improve the interfacial compatibility and interfacial bonding force between the two, thereby reducing electrolyte penetration, delaying corrosion, and effectively extending the service life of the aluminum cathode plate.
[0157] Compared with Example 8, Examples 1-4 added a punching process to the edge area. The molten epoxy material flows into the hole during the curing process to form a mechanical anchoring structure, which helps to enhance the bonding force between the epoxy insulating anti-corrosion coating and the aluminum substrate in the thickness direction, thereby improving the structural stability of the coating when subjected to the mechanical impact of zinc stripping and preventing the edge coating from curling or falling off.
[0158] In Comparative Example 1, the traditional modified vinyl coating combined with ABS insulating strips was used to protect the edge of the zinc electrowinning aluminum cathode plate. Due to the large difference in the coefficients of thermal expansion between the aluminum substrate and the ABS insulating strip, thermal stress easily induced microcracks at the interface. Furthermore, small gaps still existed in some parts of the coating, and the coating was prone to embrittlement and peeling failure under long-term immersion, resulting in poor corrosion resistance. Consequently, the aluminum cathode plate had a corrosion resistance time of only 27 hours in the high-concentration electrolyte in the laboratory. Under actual working conditions, after 90 days of operation, corrosion gaps formed at the interface between the aluminum substrate and the coating, with a gap length ≥10cm and a coating peeling area ≥20%, severely limiting its service life.
[0159] In Comparative Example 2, the aluminum cathode plate was uncoated, with only ABS insulating strips wrapped around its edges. A tiny gap of 0.01mm to 0.5mm existed between the aluminum substrate and the insulating strips. During zinc electrowinning, the electrolyte seeped into these gaps, causing zinc to deposit within them and continuously widening the gaps. This further led to the formation of corrosion pits on the aluminum substrate surface covered by the insulating strips, accelerating the strips' detachment and the plate's failure, ultimately resulting in rapid plate failure. This comparative example exhibited extremely poor corrosion resistance, with a corrosion resistance time of only 9 hours in a high-concentration electrolyte solution in the laboratory.
[0160] In Comparative Example 3, the epoxy resin content in the epoxy insulating and anti-corrosion coating raw material was too high, while the filler content was too low. This resulted in the coating's coefficient of thermal expansion not matching that of the aluminum substrate, leading to poor interfacial stability under thermal cycling conditions. This resulted in thermal stress damage and microcracks, reducing the coating's stability. Prolonged immersion in the electrolyte easily caused large-area peeling, leading to crevice corrosion. This comparative example showed a corrosion resistance time of only 21 hours in a high-concentration electrolyte in the laboratory. Under actual operating conditions, after 90 days of operation, the length of the corrosion crevice formed was ≥10 cm, and the coating peeling area was ≥5% and <10%.
[0161] Comparative Example 4 used a manual powdering method to deposit the epoxy insulating and anti-corrosion coating material, which resulted in uneven distribution of the material on the aluminum plate surface, numerous internal defects and poor density of the coating, making it easy for electrolyte to penetrate, which seriously affected the corrosion resistance and stability.
[0162] In Comparative Example 5, the roughening treatment step was omitted. Because the aluminum substrate surface was smooth and the oxide film was not removed, the coating could not form an effective mechanical anchor. The adhesion between the coating and the aluminum substrate was extremely poor. Under the scouring of the electrolyte or mechanical vibration, interface gaps were easily formed, and even large-area peeling occurred, causing the cathode plate to lose protection and thus fail rapidly.
[0163] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A zinc-electrode aluminum cathode plate, characterized in that, The zinc electrowinning aluminum cathode plate comprises an aluminum substrate and an epoxy insulating and anti-corrosion coating covering a portion of the surface of the aluminum substrate. The epoxy insulating and anti-corrosion coating is located in the coating coverage area of the aluminum substrate. The aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end in a circumferential direction. The first side and the third side are opposite to each other, and the second side and the fourth side are opposite to each other. The coating coverage area of the aluminum substrate includes a strip-shaped region extending inward from the edge of the first side for 15mm to 30mm, a strip-shaped region extending inward from the edge of the third side for 15mm to 30mm, a strip-shaped region extending inward from the edge of the second side for 90mm to 100mm, and the area where the first side and the third side are located. The raw material of the epoxy insulating and anti-corrosion coating comprises the following components in parts by weight: 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler.
2. The zinc-electrode aluminum cathode plate according to claim 1, characterized in that, When the thickness of the epoxy insulating and anti-corrosion coating is ≥50μm and <3000μm, the first side and the third side are further provided with insulating edge strips; the insulating edge strips include at least one of ABS edge strips, EAA edge strips, PP edge strips, and PPO edge strips; or, The thickness of the epoxy insulating and anti-corrosion coating is 3000μm~10mm.
3. The zinc electrowinning aluminum cathode plate according to claim 1 or 2, characterized in that, The aluminum substrate has a plurality of holes penetrating along the thickness direction, and the center of each hole is 4 mm to 8 mm away from the edge of the aluminum substrate.
4. The zinc-electrode aluminum cathode plate according to claim 3, characterized in that, At least one of the following conditions must be met: (1) The diameter of each hole is 4mm~8mm; (2) The distance between any two adjacent holes is 5cm to 8cm.
5. The zinc electrowinning aluminum cathode plate according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The epoxy resin is selected from at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenolic epoxy resin, hydrogenated bisphenol A type epoxy resin, phenolic modified epoxy resin, and fluorine modified epoxy resin. (2) The curing agent is selected from at least one of dicyandiamide curing agents, phenolic curing agents, phenolic hydroxyl resin curing agents, and aromatic amine curing agents; (3) The filler is selected from at least one of silicon oxide and silicates; (4) The antioxidant is selected from at least one of phosphite antioxidants and hindered phenolic antioxidants, and the phosphite antioxidant is selected from at least one of tris(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphite, and the hindered phenolic antioxidant is selected from at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and 2,6-di-tert-butyl-4-methylphenol; (5) The antioxidant is selected from phosphite antioxidants and hindered phenolic antioxidants, and the mass ratio of the phosphite antioxidant to the hindered phenolic antioxidant is 1:(0.5~2). (6) The lubricant is an amide lubricant, and the amide lubricant is selected from at least one of ethylene bis-stearamide, oleamide, erucamide, stearamide, N,N'-ethylene bis-oleamide, and N,N'-ethylene bis-stearamide; (7) The raw materials of the epoxy insulating and anti-corrosion coating also include 0.1 to 1 part of colorant, wherein the colorant is selected from at least one of titanium dioxide, carbon black, iron oxide red, iron oxide yellow, cobalt blue, chrome green and titanium nickel yellow.
6. A method for preparing a zinc-electrode aluminum cathode plate according to any one of claims 1 to 5, characterized in that, The method for preparing the zinc-electrode aluminum cathode plate includes the following steps: The area outside the coating coverage area of the aluminum substrate is masked to form a masked area, thus obtaining a first aluminum plate. Specifically, the aluminum substrate has a first side, a second side, a third side, and a fourth side connected end to end in the circumferential direction. The first side and the third side are arranged opposite to each other, and the second side and the fourth side are arranged opposite to each other. The coating coverage area includes a strip-shaped area extending 15mm to 30mm inward from the edge of the first side, a strip-shaped area extending 15mm to 30mm inward from the edge of the third side, and a strip-shaped area extending 90mm to 100mm inward from the edge of the second side. The coating-covered area is roughened to form a roughened region, thus obtaining a second aluminum plate; The second aluminum plate is preheated, and then the raw material of epoxy insulating and anti-corrosion coating is electrostatically sprayed onto the roughened area to form a molten layer, thus obtaining the intermediate aluminum plate. The intermediate aluminum plate is cured to obtain the zinc-electrode aluminum cathode plate; The raw materials of the epoxy insulating and anti-corrosion coating include the following components in parts by weight: 60-70 parts epoxy resin, 6-7 parts curing agent, 2-4 parts antioxidant, 0.5-1.5 parts lubricant, and 15-25 parts filler.
7. The method for preparing a zinc-electrode aluminum cathode plate according to claim 6, characterized in that, The roughening treatment includes a degreasing treatment and a mechanical roughening treatment performed sequentially. The mechanical roughening treatment includes any one of sandblasting, shot blasting, and grinding, and satisfies at least one of the following conditions: (1) The roughened region has anchor patterns, and the depth of the anchor patterns is 10μm~100μm; (2) The sandblasting process also includes blowing or ultrasonic cleaning after sandblasting, wherein the blowing gas is compressed air; (3) The raw materials of the epoxy insulating and anti-corrosion coating also include 0.1 to 1 part of colorant.
8. The method for preparing a zinc-electrode aluminum cathode plate according to claim 6, characterized in that, At least one of the following conditions must be met: (1) The shielding treatment is performed by using a metal shielding plate to shield the area of the aluminum substrate other than the coating coverage area; the metal shielding plate is selected from at least one of stainless steel shielding plate, aluminum alloy shielding plate, and titanium shielding plate; (2) The temperature of the preheating treatment is 160℃~220℃, and the holding time is 10min~40min; (3) The curing temperature is 160℃~220℃ and the holding time is 15min~60min.
9. The method for preparing a zinc-electrode aluminum cathode plate according to any one of claims 6 to 8, characterized in that, The method for preparing the zinc electrowinning aluminum cathode plate further includes performing a silane coupling treatment on the roughened region after the roughening treatment, and the method for the silane coupling treatment includes: spraying a silane coupling agent solution onto the roughened region, letting it stand for 1 min to 5 min, and then drying it at 100℃ to 180℃ for 5 min to 40 min to form a silane-treated region. Preferably, the silane coupling agent solution contains a silane coupling agent selected from at least one of γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and γ-mercaptopropyltrimethoxysilane, and the mass concentration of the silane coupling agent in the silane coupling agent solution is 0.5wt% to 2.0wt%.
10. The method for preparing a zinc-electrode aluminum cathode plate according to any one of claims 7 to 8, characterized in that, The method for preparing the zinc electrowinning aluminum cathode plate further includes punching holes in the coating coverage area before performing the shielding treatment.