A high-strength copper foil and a method for producing the same

By using a specific component electrodeposition solution and magnetron sputtering to form a cerium oxide layer and nitrogen doping, the problem of insufficient tensile strength and elongation of copper foil is solved, thereby improving the performance and safety of lithium-ion batteries.

CN123153124APending Publication Date: 2026-11-24JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611524313.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously improve the tensile strength and elongation of copper foil, which makes lithium-ion batteries prone to breakage during coating, slitting, and winding, as well as microcracks during battery cycling, affecting battery performance and safety.

Method used

Electrolytic copper foil is formed by electrodeposition using a specific composition of electrodeposition solution, including sodium chloride, sulfuric acid, carbon nanotubes, collagen, hydroxyethyl cellulose and cerium sulfate. A cerium oxide layer and nitrogen ion beam doping are then formed by magnetron sputtering to synergistically enhance the strength and conductivity of the copper foil.

Benefits of technology

It significantly improves the tensile strength and elongation of copper foil, enhances the interfacial bonding between copper foil and lithium, improves the conductivity and oxidation resistance of the battery, and enhances the reliability and electrical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application discloses a kind of high-strength copper foil and preparation method thereof, it is related to copper foil technical field, to solve the technical problem of low copper foil strength, affect lithium battery performance, its preparation method includes the following steps: step 1: sodium chloride, sulfuric acid, carbon nanotube, collagen, hydroxyethyl cellulose, cerium sulfate is added to copper sulfate aqueous solution, and is prepared into electrodeposition solution;Step 2: with pure titanium sheet as cathode, phosphor copper is anode, cathode and anode are placed in electrodeposition solution, electrodeposition is obtained electrolytic copper foil;Step 3: in argon oxygen mixed atmosphere, with metal cerium as target material, the surface of electrolytic copper foil is magnetron sputtering, and cerium oxide layer is formed;Nitrogen ion beam doping, obtain high-strength copper foil.The high-strength copper foil prepared by the application has higher tensile strength and elongation, and the prepared battery has good performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper foil technology, specifically a high-strength copper foil and its preparation method. Background Technology

[0002] Electrolytic copper foil refers to copper materials prepared by electrodeposition. It typically has good electrical and thermal conductivity and is often used as a negative electrode current collector in lithium-ion batteries. Its quality directly affects the performance of lithium batteries.

[0003] In existing technologies, mechanical properties are improved by adding organic additives to the plating bath. Commonly used additives include leveling agents (such as collagen and gelatin), brighteners (such as sodium polydithiopropane sulfonate), and wetting agents (such as hydroxyethyl cellulose). However, traditional additive systems have limited functions, and while combined additives can improve overall performance to some extent, the improvement is limited and it is difficult to simultaneously meet the requirements of high tensile strength and high elongation. Furthermore, existing technologies introduce carbon nanotubes for co-electrodeposition to improve strength; however, carbon nanotubes compete with other organic additives for adsorption, resulting in limited improvement.

[0004] However, in actual production and use, the tensile strength and elongation of copper foil directly affect the reliability and electrical performance of lithium-ion batteries. If the tensile strength of copper foil is insufficient, it is prone to breakage during coating, slitting, and winding. If the elongation is insufficient, microcracks are easily generated under the stress caused by volume expansion during battery cycling, leading to a decrease in battery performance and even affecting safety.

[0005] In summary, the preparation of a high-strength copper foil and its preparation method are of great significance in order to solve the above problems. Summary of the Invention

[0006] The present invention aims to provide a high-strength copper foil and its preparation method to solve the related technical problems existing in the prior art.

[0007] To achieve the above-mentioned objectives, the technical solution adopted by the present invention is as follows: A method for preparing high-strength copper foil includes the following steps: Step 1: Add sodium chloride, sulfuric acid, carbon nanotubes, collagen, hydroxyethyl cellulose, and cerium sulfate to an aqueous solution of copper sulfate to prepare an electrodeposition solution; Step 2: Using pure titanium sheet as cathode and phosphorus copper as anode, place the cathode and anode in the electrodeposition solution and perform electrodeposition to obtain electrolytic copper foil; Step 3: In an argon-oxygen mixed atmosphere, using metallic cerium as the target material, magnetron sputtering is performed on the surface of electrolytic copper foil to form a cerium oxide layer; nitrogen ion beam doping is then performed to obtain a high-strength copper foil.

[0008] In a more optimized manner, the electrodeposition solution comprises the following components by mass: sodium chloride 45~56 mg / L, sulfuric acid 70~100 g / L, carbon nanotubes 80~150 mg / L, collagen 10~15 mg / L, hydroxyethyl cellulose 4~6 mg / L, cerium sulfate 5~7 mg / L, and copper sulfate aqueous solution 195~205 g / L.

[0009] In a more optimized manner, carbon nanotubes are pre-modified for use in the electrodeposition solution; the preparation method is as follows: Step 1: Polyethylene glycol methyl ether mercapto group and 3-ethoxypropylamine are clicked to obtain an amino-containing methoxy polyethylene glycol sulfide derivative. Step 2: Acyl chloride carbon nanotubes are obtained by reacting carboxylated carbon nanotubes with thionyl chloride. Step 3: Acyl chloride carbon nanotubes are sequentially amidated with 2-aminopyridine and an amino-containing methoxy polyethylene glycol sulfide derivative to obtain modified carbon nanotubes.

[0010] In a more optimized manner, the carboxylated carbon nanotubes have a carboxyl content of 1.5~2.5wt%, an outer diameter of 10~20nm, an inner diameter of 5~10nm, and a length of 10~30μm; the methoxy polyethylene glycol thiol has a molecular weight of 500~1200.

[0011] In a more optimized manner, the preparation process of the modified carbon nanotubes is as follows: Step 1: By weight, add 500-1200 parts of polyethylene glycol methyl ether mercapto, 86-88 parts of 3-ethoxypropylamine, and 2.5-6.0 parts of photoinitiator to 750-850 parts of tetrahydrofuran, and heat at 100-120 mW / cm². 2 The reaction was carried out for 1.5 to 2.5 hours, and the product was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative. Step 2: By weight, add 0.2-0.3 parts of carboxylated carbon nanotubes to 97-99 parts of thionyl chloride, add 1.5-2.5 parts of N,N-dimethylformamide, react at 60-70℃ for 20-28h, cool, wash, and dry to obtain acyl chloride carbon nanotubes; Step 3: By weight, add 4-7 parts of acyl chloride carbon nanotubes to 90-110 parts of N-methylpyrrolidone, react with 0.5-1 parts of 2-aminopyridine at 0-35℃ for 6-10 h, add 4-7 parts of amino-containing methoxy polyethylene glycol sulfide derivative, react at constant temperature for 8-14 h, purify and dry to obtain modified carbon nanotubes.

[0012] In a further embodiment, the synthesis mechanism of modified carbon nanotubes is as follows: First, a click reaction is carried out between the thiol group in polyethylene glycol methyl ether mercaptoyl group of a specific molecular weight and the vinyl group in 3-ethyleneoxypropylamine to form an amino-containing methoxy polyethylene glycol sulfide derivative; second, carboxylated carbon nanotubes are acyl-chlorinated with thionyl chloride to form acyl-chlorinated carbon nanotubes; finally, the acyl-chlorinated carbon nanotubes undergo amidation reactions with the amino groups in 2-aminopyridine and the amino-containing methoxy polyethylene glycol sulfide derivative, respectively, to obtain modified carbon nanotubes. The above modifications have the following effects: the PEG segments in the methoxy polyethylene glycol sulfide derivative have high hydrophilicity, which can improve the dispersibility of modified carbon nanotubes in the electrodeposition solution and prevent agglomeration; the flexible segments such as PEG segments, sulfide bonds, and methoxy groups can enhance the flexibility of carbon nanotubes, and at the same time, they can buffer the internal stress generated during electrodeposition and subsequent magnetron sputtering, avoiding stress concentration that could lead to structural defects, thereby improving the structural stability of the copper foil; sulfide bonds and PEG segments can partially replace organic additives such as sodium polydisulfide dipropane sulfonate, which can improve grain refinement while avoiding competitive adsorption of multiple components, thus improving tensile strength and elongation; furthermore, the pyridine ring can form coordination bonds with copper through π-π stacking, enhancing the interfacial bonding between carbon nanotubes and copper; at the same time, the pyridine ring, as a lithiophilic functional group, can provide sufficient lithiophilic sites to guide uniform lithium nucleation and improve conductivity; in addition, the synergistic effect of pyridine nitrogen and subsequent nitrogen ion beam doping is conducive to the formation of a continuous electronic structure and improves strength.

[0013] In a further proposed scheme, the photoinitiator is azobisisobutyronitrile (AIBN); the purity of the cerium target material is 99.99%.

[0014] More optimally, the electrodeposition process parameters are as follows: temperature 25~35℃, current density 10~25A / dm³. 2 .

[0015] To optimize this process, the magnetron sputtering parameters are set as follows: vacuum degree ≤ 1.0 × 10⁻⁶. -4 Pa, the argon flow rate in the mixed atmosphere is 30~40 cm⁻¹ 3 / min, oxygen flow rate 4~8cm 3 The sputtering frequency is 50~100W / min, and the sputtering temperature is 50~70℃.

[0016] More optimally, the nitrogen ion beam doping process parameters are: nitrogen ion beam 80~100 keV, ion flux 1×10⁻⁶. 15 ~1×10 16 ions / cm².

[0017] Ideally, the thickness of the cerium oxide layer is 0.1~0.2 μm.

[0018] Ideally, the thickness of the high-strength copper foil is 7.5~8.5μm.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: The present application utilizes an electrodeposition solution with specific components to electrodeposit an electrolytic copper foil containing cerium; and further forms a cerium oxide layer and nitrogen doping, the two working together to improve the tensile strength and elongation of the copper foil and improve the conductivity of the battery.

[0020] 1. Adding pre-modified carbon nanotubes to electrodeposition solutions with specific components can partially replace organic additives to prevent competitive adsorption, thereby improving tensile strength and elongation.

[0021] 2. In electrodeposition solutions with specific components, cerium sulfate, as a rare earth additive, has a grain-refining effect, which can improve flatness and is beneficial to improve the tensile strength and elongation of electrolytic copper foil from the inside. At the same time, cerium sulfate is co-deposited in the copper foil in a trace form during the electrodeposition process, which can make the electrolytic copper foil and the subsequently formed cerium oxide layer and nitrogen doping form the same element transition, which is beneficial to alleviate the thermal stress mismatch at the interface and enhance the bonding force between the functional layer and the substrate.

[0022] 3. Based on electrolytic copper foil, a stable interfacial bond is formed with the copper substrate through magnetron sputtering and nitrogen doping. Cerium oxide can improve the surface oxidation resistance of copper foil to prevent copper foil oxidation, which affects tensile strength and elongation. However, cerium oxide has poor conductivity at room temperature and lacks a certain degree of lithiophilic effect, which will affect the uniform deposition of lithium and thus affect conductivity. Therefore, nitrogen doping is further introduced to enhance the surface lithiophilic effect and improve conductivity. On the other hand, nitrogen doping can effectively buffer volume expansion, suppress cracks, and improve tensile strength and elongation. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the embodiments described are only some, not all, implementations of the present invention. Other implementations that can be obtained by those skilled in the art based on the embodiments of the present invention without creative effort all fall within the protection scope of the present invention.

[0024] Example 1: A high-strength copper foil and its preparation method, comprising the following steps: Pre-preparation: (1) By weight, 1000 parts of polyethylene glycol methyl ether mercapto, 87 parts of 3-ethyleneoxypropylamine, and 5 parts of azobisisobutyronitrile were added to 800 parts of tetrahydrofuran, and the mixture was heated at 110 mW / cm 2(1) After reacting for 2 hours, the mixture was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative; (2) By mass, 0.25 parts of carboxylated carbon nanotubes were added to 98 parts of thionyl chloride, and 2 parts of N,N-dimethylformamide were added and reacted at 65°C for 24 hours. After cooling, washing, and drying, acyl chloride carbon nanotubes were obtained; (3) By mass, 5.5 parts of acyl chloride carbon nanotubes were added to 100 parts of N-methylpyrrolidone and reacted with 0.8 parts of 2-aminopyridine at 0°C for 8 hours. Then, 5.5 parts of amino-containing methoxy polyethylene glycol sulfide derivatives were added and reacted at a constant temperature for 11 hours. After purification and drying, modified carbon nanotubes were obtained. Step 1: Prepare an electrodeposition solution according to the following components: sodium chloride 45 mg / L, sulfuric acid 70 g / L, carbon nanotubes 80 mg / L, collagen 10 mg / L, hydroxyethyl cellulose 4 mg / L, cerium sulfate 5 mg / L, and copper sulfate aqueous solution 195 g / L. Step 2: Add the electrodeposition solution to a 1L electroplating tank, using pure titanium sheet as the cathode and phosphor bronze as the anode, and connect them to the negative and positive terminals of the power supply respectively; set the current density to 10A / dm³. 2 Electrodeposition was performed at 35°C to obtain electrolytic copper foil; Step 3: Set the vacuum level to 1.0 × 10⁻⁶ -4 In an atmosphere of argon and oxygen mixed at Pa, the argon flow rate is 35 cm⁻¹. 3 / min, oxygen flow rate 6cm 3 At a sputtering frequency of 80 W / min, using metallic cerium as the target, magnetron sputtering was performed on the surface of electrolytic copper foil at 60 °C to form a cerium oxide layer with a thickness of 0.15 μm. After the magnetron sputtering was completed, the nitrogen ion beam was 100 keV and the ion flux was 1 × 10⁻⁶. 15 Nitrogen ion beam doping with ions / cm² was used to obtain a high-strength copper foil with a thickness of 8μm. In Example 1 above, the molecular weight of polyethylene glycol methyl ether mercapto is 1000; the carboxyl content of the carboxylated carbon nanotube is 2wt%, the outer diameter is 10nm, the inner diameter is 5nm, and the length is 10μm.

[0025] Example 2: A high-strength copper foil and its preparation method, comprising the following steps: Pre-preparation: (1) By weight, 1000 parts of polyethylene glycol methyl ether mercapto, 87 parts of 3-ethyleneoxypropylamine, and 5 parts of azobisisobutyronitrile were added to 800 parts of tetrahydrofuran, and the mixture was heated at 110 mW / cm 2(1) After reacting for 2 hours, the mixture was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative; (2) By mass, 0.25 parts of carboxylated carbon nanotubes were added to 98 parts of thionyl chloride, and 2 parts of N,N-dimethylformamide were added and reacted at 65°C for 24 hours. After cooling, washing, and drying, acyl chloride carbon nanotubes were obtained; (3) By mass, 5.5 parts of acyl chloride carbon nanotubes were added to 100 parts of N-methylpyrrolidone and reacted with 0.8 parts of 2-aminopyridine at 0°C for 8 hours. Then, 5.5 parts of amino-containing methoxy polyethylene glycol sulfide derivatives were added and reacted at a constant temperature for 11 hours. After purification and drying, modified carbon nanotubes were obtained. Step 1: Prepare an electrodeposition solution according to the following components: sodium chloride 50 mg / L, sulfuric acid 85 g / L, carbon nanotubes 115 mg / L, collagen 12.5 mg / L, hydroxyethyl cellulose 5 mg / L, cerium sulfate 6 mg / L, and copper sulfate aqueous solution 200 g / L; Step 2: Add the electrodeposition solution to a 1L electroplating tank, using pure titanium sheet as the cathode and phosphor bronze as the anode, and connect them to the negative and positive terminals of the power supply respectively; set the current density to 17A / dm³. 2 Electrodeposition was performed at 35°C to obtain electrolytic copper foil; Step 3: Set the vacuum level to 1.0 × 10⁻⁶ -4 In an atmosphere of argon and oxygen mixed at Pa, the argon flow rate is 35 cm⁻¹. 3 / min, oxygen flow rate 6cm 3 At a sputtering frequency of 80 W / min, using metallic cerium as the target, magnetron sputtering was performed on the surface of electrolytic copper foil at 60 °C to form a cerium oxide layer with a thickness of 0.15 μm. After the magnetron sputtering was completed, the nitrogen ion beam was 100 keV and the ion flux was 1 × 10⁻⁶. 15 Nitrogen ion beam doping with ions / cm² was used to obtain a high-strength copper foil with a thickness of 8μm. In Example 2 above, the molecular weight of polyethylene glycol methyl ether mercapto is 1000; the carboxyl content of the carboxylated carbon nanotube is 2wt%, the outer diameter is 10nm, the inner diameter is 5nm, and the length is 10μm.

[0026] Example 3: A high-strength copper foil and its preparation method, comprising the following steps: Pre-preparation: (1) By weight, 1000 parts of polyethylene glycol methyl ether mercapto, 87 parts of 3-ethyleneoxypropylamine, and 5 parts of azobisisobutyronitrile were added to 800 parts of tetrahydrofuran, and the mixture was heated at 110 mW / cm 2(1) After reacting for 2 hours, the mixture was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative; (2) By mass, 0.25 parts of carboxylated carbon nanotubes were added to 98 parts of thionyl chloride, and 2 parts of N,N-dimethylformamide were added and reacted at 65°C for 24 hours. After cooling, washing, and drying, acyl chloride carbon nanotubes were obtained; (3) By mass, 5.5 parts of acyl chloride carbon nanotubes were added to 100 parts of N-methylpyrrolidone and reacted with 0.8 parts of 2-aminopyridine at 0°C for 8 hours. Then, 5.5 parts of amino-containing methoxy polyethylene glycol sulfide derivatives were added and reacted at a constant temperature for 11 hours. After purification and drying, modified carbon nanotubes were obtained. Step 1: Prepare an electrodeposition solution according to the following components: sodium chloride 56 mg / L, sulfuric acid 100 g / L, carbon nanotubes 150 mg / L, collagen 15 mg / L, hydroxyethyl cellulose 6 mg / L, cerium sulfate 7 mg / L, and copper sulfate aqueous solution 205 g / L. Step 2: Add the electrodeposition solution to a 1L electroplating tank, using pure titanium sheet as the cathode and phosphor bronze as the anode, and connect them to the negative and positive terminals of the power supply respectively; set the current density to 25A / dm³. 2 Electrodeposition was performed at 35°C to obtain electrolytic copper foil; Step 3: Set the vacuum level to 1.0 × 10⁻⁶ -4 In an atmosphere of argon and oxygen mixed at Pa, the argon flow rate is 35 cm⁻¹. 3 / min, oxygen flow rate 6cm 3 At a sputtering frequency of 80 W / min, using metallic cerium as the target, magnetron sputtering was performed on the surface of electrolytic copper foil at 60 °C to form a cerium oxide layer with a thickness of 0.15 μm. After the magnetron sputtering was completed, the nitrogen ion beam was 100 keV and the ion flux was 1 × 10⁻⁶. 15 Nitrogen ion beam doping with ions / cm² was used to obtain a high-strength copper foil with a thickness of 8μm. In Example 3 above, the molecular weight of polyethylene glycol methyl ether mercapto is 1000; the carboxyl content of the carboxylated carbon nanotube is 2wt%, the outer diameter is 10nm, the inner diameter is 5nm, and the length is 10μm.

[0027] Example 4: A high-strength copper foil and its preparation method, comprising the following steps: Pre-preparation: (1) By weight, 1000 parts of polyethylene glycol methyl ether mercapto, 87 parts of 3-ethyleneoxypropylamine, and 5 parts of azobisisobutyronitrile were added to 800 parts of tetrahydrofuran, and the mixture was heated at 110 mW / cm 2(1) After reacting for 2 hours, the product was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative; (2) By mass, 0.25 parts of carboxylated carbon nanotubes were added to 98 parts of thionyl chloride, and 2 parts of N,N-dimethylformamide were added and reacted at 65°C for 24 hours. After cooling, washing, and drying, acyl chloride carbon nanotubes were obtained; (3) By mass, 4 parts of acyl chloride carbon nanotubes were added to 100 parts of N-methylpyrrolidone and reacted with 0.5 parts of 2-aminopyridine at 0°C for 8 hours. 4 parts of amino-containing methoxy polyethylene glycol sulfide derivatives were added and reacted at a constant temperature for 11 hours. After purification and drying, modified carbon nanotubes were obtained. Step 1: Prepare an electrodeposition solution according to the following components: sodium chloride 45 mg / L, sulfuric acid 70 g / L, carbon nanotubes 80 mg / L, collagen 10 mg / L, hydroxyethyl cellulose 4 mg / L, cerium sulfate 5 mg / L, and copper sulfate aqueous solution 195 g / L. Step 2: Add the electrodeposition solution to a 1L electroplating tank, using pure titanium sheet as the cathode and phosphor bronze as the anode, and connect them to the negative and positive terminals of the power supply respectively; set the current density to 10A / dm³. 2 Electrodeposition was performed at 35°C to obtain electrolytic copper foil; Step 3: Set the vacuum level to 1.0 × 10⁻⁶ -4 In an atmosphere of argon and oxygen mixed at Pa, the argon flow rate is 35 cm⁻¹. 3 / min, oxygen flow rate 6cm 3 At a sputtering frequency of 80 W / min, using metallic cerium as the target, magnetron sputtering was performed on the surface of electrolytic copper foil at 60 °C to form a cerium oxide layer with a thickness of 0.15 μm. After the magnetron sputtering was completed, the nitrogen ion beam was 100 keV and the ion flux was 1 × 10⁻⁶. 15 Nitrogen ion beam doping with ions / cm² was used to obtain a high-strength copper foil with a thickness of 8μm. In Example 4 above, the molecular weight of polyethylene glycol methyl ether mercapto is 1000; the carboxyl content of the carboxylated carbon nanotube is 2wt%, the outer diameter is 10nm, the inner diameter is 5nm, and the length is 10μm.

[0028] Example 5: A high-strength copper foil and its preparation method, comprising the following steps: Pre-preparation: (1) By weight, 1000 parts of polyethylene glycol methyl ether mercapto, 87 parts of 3-ethyleneoxypropylamine, and 5 parts of azobisisobutyronitrile were added to 800 parts of tetrahydrofuran, and the mixture was heated at 110 mW / cm 2(1) After reacting for 2 hours, the product was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative; (2) By mass, 0.25 parts of carboxylated carbon nanotubes were added to 98 parts of thionyl chloride, and 2 parts of N,N-dimethylformamide were added and reacted at 65°C for 24 hours. After cooling, washing, and drying, acyl chloride carbon nanotubes were obtained; (3) By mass, 7 parts of acyl chloride carbon nanotubes were added to 100 parts of N-methylpyrrolidone and reacted with 1 part of 2-aminopyridine at 0°C for 8 hours. 7 parts of amino-containing methoxy polyethylene glycol sulfide derivatives were added and reacted at a constant temperature for 11 hours. After purification and drying, modified carbon nanotubes were obtained. Step 1: Prepare an electrodeposition solution according to the following components: sodium chloride 45 mg / L, sulfuric acid 70 g / L, carbon nanotubes 80 mg / L, collagen 10 mg / L, hydroxyethyl cellulose 4 mg / L, cerium sulfate 5 mg / L, and copper sulfate aqueous solution 195 g / L. Step 2: Add the electrodeposition solution to a 1L electroplating tank, using pure titanium sheet as the cathode and phosphor bronze as the anode, and connect them to the negative and positive terminals of the power supply respectively; set the current density to 10A / dm³. 2 Electrodeposition was performed at 35°C to obtain electrolytic copper foil; Step 3: Set the vacuum level to 1.0 × 10⁻⁶ -4 In an atmosphere of argon and oxygen mixed at Pa, the argon flow rate is 35 cm⁻¹. 3 / min, oxygen flow rate 6cm 3 At a sputtering frequency of 80 W / min, using metallic cerium as the target, magnetron sputtering was performed on the surface of electrolytic copper foil at 60 °C to form a cerium oxide layer with a thickness of 0.15 μm. After the magnetron sputtering was completed, the nitrogen ion beam was 100 keV and the ion flux was 1 × 10⁻⁶. 15 Nitrogen ion beam doping with ions / cm² was used to obtain a high-strength copper foil with a thickness of 8μm. In Example 5 above, the molecular weight of polyethylene glycol methyl ether mercapto is 1000; the carboxyl content of the carboxylated carbon nanotube is 2wt%, the outer diameter is 10nm, the inner diameter is 5nm, and the length is 10μm.

[0029] Comparative Example 1: Sodium polydisulfide dipropane sulfonate 4.5 mg / L and polyethylene glycol 5 mg / L were added to the electrodeposition solution. The molecular weight of polyethylene glycol was 1000. The rest was the same as in Example 2.

[0030] Comparative Example 2: The modified carbon nanotubes were replaced with carbon nanotubes; the rest was the same as in Example 2.

[0031] Comparative Example 3: No cerium sulfate added; otherwise the same as Example 2.

[0032] Comparative Example 4: The molecular weight of polyethylene glycol methyl ether mercapto group is 5000; the rest is the same as in Example 2.

[0033] Comparative Example 5: Only a cerium oxide layer was formed; the rest was the same as in Example 2.

[0034] Comparative Example 6: The electrolytic copper foil was adjusted to a high-strength copper foil; the rest was the same as in Example 2.

[0035] Performance Test 1: Using a universal testing machine, the high-strength copper foils prepared in Examples 1-5 and Comparative Examples 1-6 were used as samples to test the tensile strength and elongation of the samples respectively. (1) Tensile strength: At room temperature, the tensile strength was set to 2 mm / min. The two ends of the sample were fixed with epoxy resin, and aluminum sheets were glued to both sides. The test was performed 5 times and the average value was taken. The test results are shown in Table 1. (2) Elongation: At room temperature, the length of the sample before and after stretching was recorded, and the elongation was calculated by the formula; the formula for elongation is the deformation of the sample at tensile fracture / original gauge length; the test results are shown in Table 1. Table 1

[0036] Performance Test 2: The high-strength copper foil prepared in Examples 1-5 and Comparative Examples 1-6 was used to prepare the negative electrode and assembled into a button cell: polyvinylidene fluoride, carbon nanotubes, Ketjen black and graphite were added to N-methylpyrrolidone in a mass ratio of 1:1:1:7 and stirred to form a conductive slurry; the slurry was coated on the surface of the high-strength copper foil, dried at 90°C for 6 hours and at 110°C for 4 hours to obtain the negative electrode; under an argon atmosphere, the battery was assembled in the order of battery case, spring, negative electrode, separator and lithium sheet, and electrolyte was added dropwise to obtain the button cell; The performance of each component was tested separately; the test results are shown in Table 2; at a 1C rate, after 250 cycles, the capacity retention rate before and after the cycles was calculated. The above-mentioned diaphragm is a PP diaphragm, and the electrolyte is composed of 1% vinylene carbonate, 1 mol / L lithium hexafluorophosphate, and ethyl methyl carbonate, ethylene carbonate, and dimethyl carbonate in a mass ratio of 1:1:1.

[0037] Table 2

[0038] Conclusions: According to Tables 1 and 2 above, the high-strength copper foil prepared in this application has high tensile strength and elongation, and the prepared battery has good electrochemical performance. According to the data in Comparative Example 1, the addition of sodium polydisulfide dipropane sulfonate (4.5 mg / L) and polyethylene glycol (5 mg / L) to the electrodeposition solution resulted in competitive adsorption and a decrease in overall performance. According to the data in Comparative Example 2, adjusting the modified carbon nanotubes to carbon nanotubes led to agglomeration, weak interfacial bonding, and internal stress problems, resulting in a decrease in overall performance. According to the data in Comparative Example 3, without the addition of high-cerium sulfuric acid, there was no grain refinement or cerium element transition, leading to a decrease in flatness and overall performance. According to the data in Comparative Example 4, the molecular weight of polyethylene glycol methyl ether mercaptoyl groups was 5000, which was too long, resulting in a decrease in overall performance. According to the data in Comparative Example 5, only a cerium oxide layer was formed without nitrogen doping, lacking sufficient buffering, resulting in poor surface conductivity and a decrease in overall performance. According to the data in Comparative Example 6, adjusting the electrolytic copper foil to high-strength copper foil resulted in poor oxidation resistance and a decrease in overall performance.

[0039] It will be apparent to those skilled in the art that the present invention is not limited to the specific details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit and core features of the invention. Therefore, the above embodiments should be considered exemplary rather than restrictive in any respect. The scope of protection of the present invention is defined by the appended claims, not by the foregoing description, and is therefore intended to encompass all variations in the meaning and scope of the equivalents of the claims within the scope of the present invention.

Claims

1. A method for preparing high-strength copper foil, characterized in that: Includes the following steps: Step 1: Add sodium chloride, sulfuric acid, carbon nanotubes, collagen, hydroxyethyl cellulose, and cerium sulfate to an aqueous solution of copper sulfate to prepare an electrodeposition solution; Step 2: Using pure titanium sheet as cathode and phosphorus copper as anode, place the cathode and anode in the electrodeposition solution and perform electrodeposition to obtain electrolytic copper foil; Step 3: In an argon-oxygen mixed atmosphere, using metallic cerium as the target material, magnetron sputtering is performed on the surface of electrolytic copper foil to form a cerium oxide layer; nitrogen ion beam doping is then performed to obtain a high-strength copper foil.

2. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The electrodeposition solution comprises the following components by mass: sodium chloride 45~56 mg / L, sulfuric acid 70~100 g / L, carbon nanotubes 80~150 mg / L, collagen 10~15 mg / L, hydroxyethyl cellulose 4~6 mg / L, cerium sulfate 5~7 mg / L, and copper sulfate aqueous solution 195~205 g / L.

3. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The carbon nanotubes are pre-modified and used in the electrodeposition solution; the preparation method is as follows: Step 1: Polyethylene glycol methyl ether mercapto group and 3-ethoxypropylamine are clicked to obtain an amino-containing methoxy polyethylene glycol sulfide derivative. Step 2: Acyl chloride carbon nanotubes are obtained by reacting carboxylated carbon nanotubes with thionyl chloride. Step 3: Acyl chloride carbon nanotubes are sequentially amidated with 2-aminopyridine and an amino-containing methoxy polyethylene glycol sulfide derivative to obtain modified carbon nanotubes.

4. The method for preparing a high-strength copper foil according to claim 3, characterized in that: The carboxylated carbon nanotubes have a carboxyl content of 1.5-2.5 wt%, an outer diameter of 10-20 nm, an inner diameter of 5-10 nm, and a length of 10-30 μm; the methoxy polyethylene glycol thiol has a molecular weight of 500-1200.

5. The method for preparing a high-strength copper foil according to claim 3, characterized in that: The specific preparation process of the modified carbon nanotubes is as follows: Step 1: By weight, add 500-1200 parts of polyethylene glycol methyl ether mercapto, 86-88 parts of 3-ethoxypropylamine, and 2.5-6.0 parts of photoinitiator to 750-850 parts of tetrahydrofuran, and heat at 100-120 mW / cm². 2 The reaction was carried out for 1.5 to 2.5 hours, and the product was purified and dried to obtain an amino-containing methoxy polyethylene glycol sulfide derivative. Step 2: By weight, add 0.2-0.3 parts of carboxylated carbon nanotubes to 97-99 parts of thionyl chloride, add 1.5-2.5 parts of N,N-dimethylformamide, react at 60-70℃ for 20-28h, cool, wash, and dry to obtain acyl chloride carbon nanotubes; Step 3: By weight, add 4-7 parts of acyl chloride carbon nanotubes to 90-110 parts of N-methylpyrrolidone, react with 0.5-1 parts of 2-aminopyridine at 0-35℃ for 6-10 h, add 4-7 parts of amino-containing methoxy polyethylene glycol sulfide derivative, react at constant temperature for 8-14 h, purify and dry to obtain modified carbon nanotubes.

6. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The specific electrodeposition process parameters are: temperature 25~35℃, current density 10~25A / dm³. 2 .

7. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The process parameters for magnetron sputtering are: vacuum degree ≤ 1.0 × 10⁻⁶. -4 Pa, the argon flow rate in the mixed atmosphere is 30~40 cm⁻¹ 3 / min, oxygen flow rate 4~8cm 3 The sputtering frequency is 50~100W / min, and the sputtering temperature is 50~70℃.

8. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The process parameters for nitrogen ion beam doping are: nitrogen ion beam 80~100 keV, ion flux 1×10⁻⁶. 15 ~1×10 16 ions / cm².

9. The method for preparing a high-strength copper foil according to claim 1, characterized in that: The thickness of the cerium oxide layer is 0.1~0.2μm.

10. The high-strength copper foil prepared by the method for preparing high-strength copper foil according to any one of claims 1 to 9, characterized in that: The thickness of the high-strength copper foil is 7.5~8.5μm.