A method for preparing a copper alloy surface nickel copper / nickel copper phosphorus composite plating layer for grounding

By forming a double-layer structure of a nickel-copper transition layer and a nickel-copper-phosphorus composite coating on a copper alloy substrate, the problem of easy damage to grounding copper alloy materials in corrosive environments is solved, achieving a balance between corrosion resistance and conductivity, and reducing maintenance frequency and cost.

CN123153128APending Publication Date: 2026-11-24NANCHANG HANGKONG UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611313364.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing grounding copper alloy materials are prone to corrosion in acidic soils, chloride-containing and humid environments, resulting in high maintenance and replacement frequency and high costs. Existing platings are difficult to balance maintaining conductivity and connection stability.

Method used

A nickel-copper transition layer is first pre-plated on a copper alloy substrate, followed by electroplating of a nickel-copper-phosphorus composite coating. Through low-temperature heat treatment or sealing treatment, an inner and outer layer structure is formed. The inner layer improves the interfacial bonding, while the outer layer provides a barrier against corrosive media and controls changes in conductivity.

Benefits of technology

It improves the corrosion resistance of copper alloy materials in corrosive environments, reduces maintenance frequency and cost, while maintaining the stability of conductivity, and is suitable for batch processing of various grounding devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153128A_ABST
    Figure CN123153128A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface. The method involves first pre-plating a nickel-copper transition layer with controlled thickness on a copper alloy substrate, followed by electroplating a nickel-copper-phosphorus composite coating with controlled Cu and P content, and then post-processing to obtain the nickel-copper / nickel-copper-phosphorus composite coating on the grounding copper alloy surface. This method can control the overall conductivity change of the modified copper alloy substrate within a small range; low-temperature heat treatment or benzotriazole-silane sealing treatment can reduce internal stress or seal local pores, avoiding significant impacts on the microstructure of the copper alloy substrate caused by high-temperature diffusion processes; using conventional electroplating processes, rack plating, barrel plating, or continuous traction electroplating can be employed according to the morphology of the grounding copper alloy components, facilitating the batch processing of grounding electrodes, grounding leads, and connectors, and significantly reducing maintenance frequency by minimizing corrosion inspection and replacement, making it highly practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a copper alloy surface for grounding, specifically belonging to the fields of metal material surface engineering, electrodeposition technology, and electrochemical protection technology. The method of this invention is applicable to grounding devices in fields such as power systems, communication base stations, lightning protection engineering, new energy power plants, rail transit, and petrochemical facilities. Background Technology

[0002] Grounding components, buried in the soil for extended periods, need to maintain a stable cross-sectional area and connection status while conducting fault currents and lightning strike currents. Acidic red soil, high-salt coastal soils, and moist soils containing chloride and sulfate ions accelerate the uniform and localized corrosion of carbon steel, galvanized steel, and some copper alloys, thereby increasing the frequency of maintenance and replacement. Pure copper has good conductivity and corrosion resistance, but its material cost is high in large-scale grounding grids; copper alloys can balance cost, strength, and conductivity, but connection points, scratches, and areas with uneven structure can still become weak points for corrosion.

[0003] Ni-Cu-P coating itself is not a new material system. Liu and Zhao reported on electroless Ni-Cu-P coatings on copper, steel and stainless steel surfaces in Applied Surface Science 228 (2004) 57-62 and studied their corrosion resistance in hydrochloric acid and sodium chloride media; Liu et al. studied the corrosion behavior of electroless Ni-Cu-P coatings in flue gas condensate in Surface and Coatings Technology 204 (2010) 3382-3386; Junjun Liu et al. studied the effect of Cu content in electroless Ni-Cu-P coatings on microstructure and corrosion properties on ZK61M magnesium alloy surface in Applied Surface Science 356 (2015) 289-293.

[0004] The aforementioned studies primarily employed electroless plating, focusing on magnesium alloys, steel, or general copper materials. The emphasis was on plating solution stability, deposition rate, and coating performance under a single corrosive medium. Grounding copper alloys also require that the surface protective layer not significantly weaken the overall conductivity and contact conductivity at joints, and that the process be adaptable to rack plating, barrel plating, or continuous electroplating production of grounding rods, grounding leads, and connectors. Therefore, this application focuses not merely on the introduction of Cu into the Ni-P system, but on proposing a dual-layer electroplating scheme for grounding copper alloys. This scheme combines a nickel-copper inner layer with a nickel-copper-phosphorus outer layer of controlled thickness and controlled Cu / P content. The inner layer provides interfacial bonding and potential matching, while the outer layer provides corrosion barrier function. Low-temperature post-treatment controls conductivity changes and manufacturing costs. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on the surface of a copper alloy for grounding. Through an industrially achievable electroplating process, a Ni-Cu-P composite coating with controllable thickness, adjustable composition, and strong bonding is constructed on the surface of the copper alloy. While maintaining the main conductivity and mechanical properties of the grounding material, this method improves its corrosion resistance in acidic soils, chloride-containing media, and humid environments, thereby reducing the maintenance cost throughout the material's life cycle.

[0006] To achieve the above objectives, the present invention provides a method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface by first pre-plating a nickel-copper transition layer with controlled thickness on a copper alloy substrate, then electroplating a nickel-copper-phosphorus composite coating with controlled Cu and P content, and finally obtaining the nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface through post-processing. Specifically, the following steps are included: Step 1: Substrate Pretreatment The surface of the grounding copper alloy substrate is polished, degreased by alkaline washing, activated by acid washing, and cleaned with deionized water to obtain a clean and activated copper alloy substrate. Step 2: Pre-plating a nickel-copper transition layer A copper alloy substrate is used as the cathode and pre-plated in a pre-plating solution containing nickel and copper salts to form a nickel-copper transition layer with a thickness of 0.2~2.0 μm. Pre-plating nickel-copper transition layer process: The pH of the pre-plating solution is 3.0~5.0, the temperature is 35~65 ℃, the cathode current density is 0.5~5 A / dm², the time is 0.5~10 min, and the Cu content in the nickel-copper transition layer is 3~20 wt%. Step 3: Electroplating a nickel-copper-phosphorus composite coating A copper alloy substrate with a pre-plated nickel-copper transition layer is used as the cathode. Direct current electroplating or pulse electroplating is performed in a nickel-copper-phosphorus composite electroplating solution containing nickel salts, copper salts, and phosphorus compounds to form a nickel-copper-phosphorus composite coating with a thickness of 2–25 μm. The nickel-copper-phosphorus composite coating contains 5–25 wt% Cu and 4–12 wt% P. Step 4: Post-processing The copper alloy substrate with the electroplated nickel-copper-phosphorus composite coating is cleaned with deionized water, washed with hot water and dried, or further subjected to low-temperature heat treatment or sealing treatment to obtain a nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy.

[0007] In the aforementioned substrate pretreatment: the surface roughness Ra of the polished copper alloy substrate is controlled to be 0.1~2.0 μm; alkaline degreasing is performed in an alkaline degreasing solution at 40~80 ℃ for 3~20 min; acid pickling activation is performed in a 5 wt%~15 wt% sulfuric acid solution, a 5 wt%~10 wt% hydrochloric acid solution, or a sulfuric acid-hydrogen peroxide micro-etching solution for 10~120 s.

[0008] The pre-plating solution consists of NiSO4·6H2O, NiCl2·6H2O, CuSO4·5H2O, H3BO3, and sodium citrate at concentrations of 120~260 g / L, 20~70 g / L, 1~15 g / L, 20~50 g / L, and 5~30 g / L, respectively.

[0009] The nickel-copper-phosphorus composite electroplating solution comprises: NiSO4·6H2O 120~300 g / L, NiCl2·6H2O 10~80 g / L, CuSO4·5H2O 2~35 g / L, H3BO3 20~50 g / L, H3PO3 and / or NaH2PO2·H2O 5~50 g / L, complexing agent 5~60 g / L, grain refiner 0.1~5 g / L, and wetting agent 0.01~0.5 g / L; The complexing agent is at least one of sodium citrate, lactic acid, glycine, malic acid, potassium sodium tartrate, and disodium ethylenediaminetetraacetate; the grain refiner is at least one of sodium saccharin, butynediol, and coumarin; and the wetting agent is at least one of sodium dodecyl sulfate, polyethylene glycol Tween 80, and fatty alcohol polyoxyethylene ether AEO-9.

[0010] The DC electroplating process is as follows: the pH of the nickel-copper-phosphorus composite electroplating solution is 1.5~4.5, the temperature is 40~75 ℃, the average cathode current density is 0.5~6 A / dm², the electroplating time is 5~90 ​​min, and the cathode moving speed is 0.05~0.5 m / s or the mechanical stirring speed is 100~600 r / min.

[0011] The pulse electroplating process is as follows: pulse electroplating frequency 50~2000 Hz, duty cycle 20~80%, peak current density 2~12 A / dm², and average current density 0.5~5 A / dm².

[0012] The sealing treatment involves treating the nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy in an aqueous sealing solution containing 0.5–3 g / L benzotriazole and 1–10 g / L γ-glycidyl oxypropyltrimethoxysilane for 5–15 min, followed by drying at 70–90 °C for 30–60 min.

[0013] The aforementioned low-temperature heat treatment involves heat-treating the nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy at a temperature of 160~280 ℃ for 0.5~3 h.

[0014] The grounding copper alloy substrate can be Cu-Al-Ni-Zn-Sn-Mn-RE series copper alloy, aluminum bronze, nickel-aluminum bronze, tin bronze, or copper-clad steel with an outer copper alloy layer.

[0015] The beneficial effects of this invention are: 1. The present invention sets up a two-layer structure with clearly defined functions, with the inner layer of nickel-copper and the outer layer of nickel-copper-phosphorus. The inner layer mainly improves the interfacial bonding, while the outer layer mainly provides barrier protection in acidic soil and chlorine-containing media.

[0016] 2. This invention limits the thickness of the nickel-copper-phosphorus outer layer and the Cu / P content, so that the copper alloy substrate remains the main conductive carrier. Its conductivity changes from 11.4% IACS to 10.7% IACS, with a retention rate of 93.9%. This indicates that the surface-modified copper alloy substrate does not increase its intrinsic conductivity and can control the change in overall conductivity within a small range.

[0017] 3. Low-temperature heat treatment or benzotriazole-silane sealing treatment can reduce internal stress or seal local pores, avoiding the significant impact of high-temperature diffusion processes on the microstructure of copper alloy substrates.

[0018] 4. The method of the present invention adopts conventional electroplating process, and can use rack plating, barrel plating or continuous traction electroplating according to the shape of the grounding copper alloy component. It is convenient for batch processing of grounding electrode, grounding lead and connector, and can significantly reduce maintenance frequency by reducing corrosion inspection and replacement, which is highly practical. Attached Figure Description

[0019] Figure 1 SEM image of the nickel-copper-phosphorus composite coating obtained in Example 1 of this invention; Figure 2 SEM image of the cross section of the nickel-copper-phosphorus composite coating obtained in Example 1 of this invention; Figure 3 A comparison of polarization curves of the copper alloy material without surface modification and the copper alloy material after surface modification with a nickel-copper-phosphorus composite coating in this invention; Figure 4 Electrochemical impedance Nyquist comparison diagram of the copper alloy material without surface modification and the copper alloy material after surface modification with nickel-copper-phosphorus composite coating; Figure 5 Comparison of electrochemical impedance frequency-modulus between the unmodified copper alloy material and the copper alloy material after surface modification with nickel-copper-phosphorus composite coating; Figure 6 Comparison of electrochemical impedance frequency-phase angle between the unmodified copper alloy material and the copper alloy material after surface modification with nickel-copper-phosphorus composite coating; Figure 7 The diagram shows the change in electrical conductivity of copper alloy materials after surface modification with a nickel-copper-phosphorus composite coating according to the present invention. Detailed Implementation

[0021] Example 1 DC electroplating of nickel-copper / nickel-copper-phosphorus composite coatings

[0022] A Cu-9Al-4Ni-1Zn-0.5Sn-0.3Mn-0.07Ce (wt%) copper alloy plate was selected as the substrate, with dimensions of 30mm × 20mm × 3mm.

[0023] The surface was polished with 800#, 1200# and 2000# sandpaper in sequence, then degreased in an alkaline degreasing solution at 60 ℃ for 10 min, rinsed with deionized water, and activated in 10 wt% H2SO4 solution for 60 s.

[0024] The composition of the pre-plating solution for the pre-plating nickel-copper transition layer is as follows: The concentrations of NiSO4·6H2O 200 g / L, NiCl2·6H2O 40 g / L, CuSO4·5H2O 5 g / L, H3BO3 35 g / L, and sodium citrate 10 g / L were used, with a pH of 4.0 and a temperature of 50 ℃.

[0025] Using the aforementioned copper alloy plate as the cathode and the electrolytic nickel plate as the anode, with a cathode current density of 2 A / dm², and a pre-plating time of 3 min, a nickel-copper transition layer of approximately 0.8 μm was obtained.

[0026] The composition of the nickel-copper-phosphorus composite electroplating solution is as follows: The concentrations of the reagents are as follows: NiSO4·6H2O 220 g / L, NiCl2·6H2O 35 g / L, CuSO4·5H2O 12 g / L, H3BO3 35 g / L, H3PO3 20 g / L, sodium citrate 20 g / L, sodium saccharin 1.0 g / L, sodium dodecyl sulfate 0.05 g / L, pH 2.6, and temperature 60 ℃.

[0027] Direct current electroplating was used with a cathode current density of 1 A / dm² and an electroplating time of 10 min to obtain a Ni-Cu-P composite coating with a thickness of about 15 μm, a Cu content of about 12 wt%, and a P content of about 7 wt%.

[0028] After electroplating a Ni-Cu-P composite coating, the copper alloy plate is cleaned with deionized water, washed with hot water at 60 ℃, and dried at 80 ℃ for 30 min to obtain a copper alloy material for grounding with a nickel-copper / nickel-copper-phosphorus composite coating on the surface.

[0029] The above process is applicable to grounding copper alloy components that require both corrosion resistance and conductivity retention.

[0030] Example 2 Pulse electroplating for preparing nickel-copper / nickel-copper-phosphorus composite coatings

[0031] The difference between this embodiment and Embodiment 1 is that the nickel-copper / nickel-copper-phosphorus composite coating is prepared by pulse electroplating.

[0032] The composition of the nickel-copper-phosphorus composite electroplating solution is as follows: The concentrations of the reagents are as follows: NiSO4·6H2O 240 g / L, NiCl2·6H2O 45 g / L, CuSO4·5H2O 18 g / L, H3BO3 40 g / L, H3PO3 30 g / L, lactic acid 10 mL / L, sodium citrate 15 g / L, sodium saccharin 1.5 g / L, sodium dodecyl sulfate 0.08 g / L, pH 2.3, and temperature 60 ℃.

[0033] The pulse frequency was 500 Hz, the duty cycle was 50%, the peak current density was 6 A / dm², the average current density was 3 A / dm², and the electroplating time was 15 min.

[0034] The resulting nickel-copper-phosphorus composite coating is approximately 10 μm thick, with a Cu content of approximately 15 wt% and a P content of approximately 9 wt%. The surface is more uniform and dense, making it suitable for grounding electrodes or grounding connectors in acidic red soil and chloride-containing environments.

[0035] Example 3 Rapid electroplating of Ni-Cu-P composite coatings

[0036] Copper alloy wire or rod for grounding is selected as the base material. After mechanical rust removal, alkaline washing and degreasing, and acid washing and activation, a pre-plated nickel-copper transition layer and nickel-copper-phosphorus composite electroplating treatment are adopted.

[0037] The composition of the nickel-copper-phosphorus composite electroplating solution is as follows: The concentrations of the reagents are as follows: NiSO4·6H2O 180 g / L, NiCl2·6H2O 30 g / L, CuSO4·5H2O 6 g / L, H3BO3 30 g / L, NaH2PO2·H2O 15 g / L, sodium citrate 15 g / L, sodium saccharin 0.5 g / L, sodium dodecyl sulfate 0.03 g / L, pH 4.0, and temperature 50 ℃.

[0038] DC electroplating was used with a cathode current density of 1.5 A / dm² and an electroplating time of 8-12 min to obtain a nickel-copper-phosphorus composite coating with a thickness of about 3-5 μm.

[0039] The above process can reduce nickel salt consumption and processing time, and is suitable for grounding components with strict cost control and moderate service corrosion intensity.

[0040] Example 4 Preparation of nickel-copper-phosphorus composite coatings under conditions of increased copper salt concentration

[0041] This embodiment increases the copper salt concentration in the electroplating solution compared to Example 1. The concentration of CuSO4·5H2O in the nickel-copper-phosphorus composite electroplating solution is 25 g / L, the concentration of sodium citrate is 35 g / L, and the other components and operating conditions are the same as in Example 1.

[0042] The resulting nickel-copper-phosphorus composite coating has a thickness of approximately 8-12 μm, a Cu content of approximately 20 wt%, and a P content of approximately 6 wt%.

[0043] This coating has good conductivity retention and is suitable for corrosion protection of grounding connectors, copper busbar connections, or the ends of grounding leads where high contact conductivity is required. Example 5 Low-temperature heat treatment enhances the stability of nickel-copper-phosphorus composite coatings

[0044] The copper alloy sheet with the electroplated nickel-copper-phosphorus composite coating obtained in Example 1 was placed in a forced-air drying oven or a protective atmosphere furnace and held at 220 °C for 1 h before being air-cooled. After low-temperature heat treatment, the internal stress of the nickel-copper-phosphorus composite coating was reduced and the interfacial bonding force was improved. At the same time, the treatment temperature was lower than the heat treatment temperature of the copper alloy substrate, so it did not significantly change the solid solution and precipitated phase structure of the copper alloy substrate.

[0045] Products that have undergone low-temperature heat treatment are suitable for applications requiring high coating adhesion and corrosion resistance, such as long-term underground service, humid and acidic soil environments, and grounding grid connection points.

[0046] Example 6 Sealing process to improve corrosion resistance at coating defects

[0047] The nickel-copper-phosphorus composite coating product obtained in Example 2 was placed in an aqueous sealing solution containing 0.5-3 g / L benzotriazole and 1-10 g / L γ-glycidyl oxypropyltrimethoxysilane for 5-15 min, and then dried at 80 °C for 30-60 min.

[0048] Sealing treatment can further reduce the risk of corrosive media penetration at micropores and pinholes, and is suitable for coastal high-salt and humid soils or industrial polluted soil environments.

[0049] Comparative Example 1 The grounding copper alloy material, which has not undergone surface modification, is only mechanically polished, degreased, pickled, and dried.

[0050] Comparative Example 2 The surface of the grounding copper alloy material is only electroplated with a common nickel layer, without adding copper salts or phosphorus compounds, and the plating thickness is about 8 μm.

[0051] Comparative Example 3 A standard nickel-phosphorus coating was prepared on the surface of a copper alloy material for grounding, without the addition of copper salts, with a coating thickness of approximately 8 μm. The standard nickel-phosphorus coating exhibits good corrosion resistance, but its conductivity retention and interfacial potential matching are inferior to those of a copper-containing nickel-copper-phosphorus composite coating.

[0052] Comparative Example 4 A nickel-copper-phosphorus composite coating with a thickness greater than 30 μm was prepared on the surface of a copper alloy material for grounding. Although the thick coating can provide a stronger barrier effect, it increases the consumption of metal salts, prolongs the deposition time, and may cause an increase in contact resistance in some connection scenarios, which is not conducive to cost reduction and efficiency improvement.

[0053] Comparative Example 5 A Cu-9Al-4Ni-1Zn-0.5Sn-0.3Mn-0.07Ce copper alloy plate, identical to that used in Example 1, was selected as the substrate. Pretreatment was performed according to the mechanical polishing, alkaline cleaning, and acid activation steps of Example 1, but the pre-plating of the Ni-Cu inner layer was omitted. The activated copper alloy substrate was directly placed in the nickel-copper-phosphorus composite electroplating solution described in Example 1 and DC electroplated for 10 min at 60 ℃ and a cathode current density of 1 A / dm² to ensure the deposition conditions of the Ni-Cu-P outer layer remained consistent with Example 1. After electroplating, the substrate was sequentially rinsed with deionized water, washed with hot water at 60 ℃, and dried at 80 ℃ for 30 min to obtain a comparative sample containing only the Ni-Cu-P layer but not the Ni-Cu inner layer. This comparative example was used to compare the effect of the Ni-Cu inner layer on interfacial bonding, corrosion resistance, and conductivity retention with Example 1.

[0054] Performance testing and results analysis

[0055] Electrochemical tests were conducted on the samples from the examples and comparative examples in simulated acidic soil solutions. The pH of the simulated solutions was controlled between 4.5 and 6.0, and they contained a certain concentration of Cl. - and SO4 2- The open-circuit potential, potentiodynamic polarization curves, and electrochemical impedance spectroscopy were measured using a three-electrode system; the material conductivity was measured using an eddy current conductivity meter. ;

[0056] The results above show that after surface modification using the method of this invention, the corrosion potential of the grounding copper alloy material shifts positively and the corrosion current density decreases, indicating that its corrosion resistance is improved. Meanwhile, because the thickness of the nickel-copper-phosphorus composite coating is controlled and the Cu element helps reduce the coating resistivity, the copper alloy substrate still serves as the main conductive carrier. The material's conductivity retention rate and contact resistance variation are both within acceptable engineering ranges, thus achieving a balance between improved corrosion resistance and stable conductivity.

[0057] The method described in this invention is compatible with existing electroplating production lines. For plates or bars, rack plating can be used; for wires or strips, continuous traction electroplating can be used; for small connectors, barrel plating or fixture electroplating can be used. The electroplating solution mainly consists of conventional nickel salts, copper salts, phosphorus sources, and additives. The process temperature is relatively low, eliminating the need for high-temperature diffusion treatment, resulting in lower equipment investment and energy consumption.

[0058] The surface-modified copper alloy material obtained by this invention can be used as grounding electrodes, grounding grids, grounding down conductors, grounding connectors, and lightning protection grounding components in acidic soils, saline-alkali soils, coastal high-salt and humid environments, and soils containing industrial pollutants. It can reduce the frequency of maintenance and replacement caused by corrosion, significantly reduce the maintenance frequency, and has good cost reduction and efficiency improvement and industrial promotion value.

[0059] This invention forms a composite structure of "copper alloy substrate - nickel-copper transition layer - nickel-copper-phosphorus composite coating" by electroplating a nickel-copper-phosphorus alloy layer onto the surface of a grounding copper alloy material. This structure utilizes the copper alloy substrate to provide the main conductivity and mechanical support, and the nickel-copper-phosphorus composite coating to provide a corrosion barrier. Material cost and conductivity variations are controlled through thin-layer processing and low-temperature operation. This method is simple, has controllable parameters, and is easy to apply industrially, providing an effective solution for increasing the durability and cost of grounding materials.

Claims

1. A method for producing a copper alloy surface nickel copper / nickel copper phosphorus composite plating layer for grounding, characterized by: The preparation method involves first pre-plating a nickel-copper transition layer with controlled thickness on a copper alloy substrate, then electroplating a nickel-copper-phosphorus composite coating with controlled Cu and P content, and finally obtaining a nickel-copper / nickel-copper-phosphorus composite coating on the surface of a grounding copper alloy after post-treatment. Specifically, the following steps are included: Step 1: Substrate Pretreatment The surface of the grounding copper alloy substrate is polished, degreased by alkaline washing, activated by acid washing, and cleaned with deionized water to obtain a clean and activated copper alloy substrate. Step 2: Pre-plating a nickel-copper transition layer A copper alloy substrate is used as the cathode and pre-plated in a pre-plating solution containing nickel and copper salts to form a nickel-copper transition layer with a thickness of 0.2~2.0 μm. Pre-plating nickel-copper transition layer process: The pH of the pre-plating solution is 3.0~5.0, the temperature is 35~65 ℃, the cathode current density is 0.5~5 A / dm², the time is 0.5~10 min, and the Cu content in the nickel-copper transition layer is 3~20 wt%. Step 3: Electroplating a nickel-copper-phosphorus composite coating A copper alloy substrate with a pre-plated nickel-copper transition layer is used as the cathode. Direct current electroplating or pulse electroplating is performed in a nickel-copper-phosphorus composite electroplating solution containing nickel salts, copper salts, and phosphorus compounds to form a nickel-copper-phosphorus composite coating with a thickness of 2–25 μm. The nickel-copper-phosphorus composite coating contains 5–25 wt% Cu and 4–12 wt% P. Step 4: Post-processing The copper alloy substrate with electroplated nickel-copper-phosphorus composite coating is cleaned with deionized water, washed with hot water and dried, or further subjected to low-temperature heat treatment or sealing treatment to obtain a nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy.

2. The method for preparing a surface nickel-copper / nickel-copper-phosphorus composite plating layer of a copper alloy for grounding according to claim 1, characterized in that: In the aforementioned substrate pretreatment: the surface roughness Ra of the polished copper alloy substrate is controlled to be 0.1~2.0 μm; alkaline degreasing is performed in an alkaline degreasing solution at 40~80 ℃ for 3~20 min; acid pickling activation is performed in a 5 wt%~15 wt% sulfuric acid solution, a 5 wt%~10 wt% hydrochloric acid solution, or a sulfuric acid-hydrogen peroxide micro-etching solution for 10~120 s.

3. The method for preparing a surface nickel-copper / nickel-copper-phosphorus composite plating layer of a copper alloy for grounding according to claim 1, characterized in that: The pre-plating solution Composition: NiSO4·6H2O, NiCl2·6H2O, CuSO4·5H2O, H3BO3 and sodium citrate are 120~260 g / L, 20~70 g / L, 1~15 g / L, 20~50 g / L and 5~30 g / L respectively.

4. The method for preparing a surface nickel-copper / nickel-copper-phosphorus composite plating layer of a copper alloy for grounding according to claim 1, characterized in that: The nickel-copper-phosphorus composite electroplating solution comprises: NiSO4·6H2O 120~300 g / L, NiCl2·6H2O 10~80 g / L, CuSO4·5H2O 2~35 g / L, H3BO3 20~50 g / L, H3PO3 and / or NaH2PO2·H2O 5~50 g / L, complexing agent 5~60 g / L, grain refiner 0.1~5 g / L, and wetting agent 0.01~0.5 g / L; The complexing agent is at least one of sodium citrate, lactic acid, glycine, malic acid, potassium sodium tartrate, and disodium ethylenediaminetetraacetate; the grain refiner is at least one of sodium saccharin, butynediol, and coumarin; and the wetting agent is at least one of sodium dodecyl sulfate, polyethylene glycol Tween 80, and fatty alcohol polyoxyethylene ether AEO-9.

5. The method for preparing a surface nickel-copper / phosphorus-nickel composite plating layer of a copper alloy for grounding according to claim 1, characterized in that: The DC electroplating process is as follows: the pH of the nickel-copper-phosphorus composite electroplating solution is 1.5~4.5, the temperature is 40~75 ℃, the average cathode current density is 0.5~6 A / dm², the electroplating time is 5~90 ​​min, and the cathode moving speed is 0.05~0.5 m / s or the mechanical stirring speed is 100~600 r / min.

6. The method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface according to claim 1, characterized in that: The pulse electroplating process is as follows: pulse electroplating frequency 50~2000 Hz, duty cycle 20~80%, peak current density 2~12 A / dm², and average current density 0.5~5 A / dm².

7. The method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface according to claim 1, characterized in that: The sealing treatment involves treating the nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy in an aqueous sealing solution containing 0.5–3 g / L benzotriazole and 1–10 g / L γ-glycidyl oxypropyltrimethoxysilane for 5–15 min, followed by drying at 70–90 °C for 30–60 min.

8. The method for preparing a nickel-copper / nickel-copper-phosphorus composite coating on a grounding copper alloy surface according to claim 1, characterized in that: The aforementioned low-temperature heat treatment involves heat-treating the nickel-copper / nickel-copper-phosphorus composite coating on the surface of the grounding copper alloy at a temperature of 160~280 ℃ for 0.5~3 h.