Production process of special non-debris screw for radiator AI liquid cooling plate
Through a process chain of multi-stage ultra-clean pretreatment, pre-plating nickel, bidirectional pulse electroplating of zinc-nickel alloy, nanocomposite sealing, and gradient low-temperature curing, the problem of plating debris generated by radiator screws during fastening and thermal cycling service was solved, achieving the heat dissipation safety and microchannel cleanliness requirements of AI liquid cooling plates.
Patent Information
- Application Number
- CN202611235438.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, radiator screws generate plating debris during fastening and thermal cycling, which blocks the microchannels of the liquid cooling plate and fails to meet the stringent requirements of AI liquid cooling plates for particulate contamination.
The process chain employs multi-stage ultra-clean pretreatment, pre-plating nickel, bidirectional pulse electroplating of zinc-nickel alloy, nanocomposite sealing, and gradient low-temperature curing to control the residual stress of the coating below 80MPa, forming a compressive stress state and suppressing the generation of debris during the fastening and thermal cycling process.
It effectively reduces the amount of debris on screws during fastening and long-term high-temperature cycling, ensuring the heat dissipation safety of the AI liquid cooling plate, meeting the cleanliness requirements of microchannels, and the coating does not blister, crack, or discolor under extreme thermal cycling conditions.
Smart Images

Figure CN123153129A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fastener manufacturing technology, specifically relating to the production process of chip-free screws for AI liquid cooling plates in radiators. Background Technology
[0002] With the soaring thermal design power consumption of AI chips, liquid cooling plates have become the mainstream heat dissipation solution. The interior of the liquid cooling plate is densely covered with microchannels with a width of 0.2 to 0.8 mm, which places extremely stringent requirements on the cleanliness of the circulating coolant. The M2 to M5 stainless steel and carbon steel screws used to fix the cold plate cover, joints and clamps have become the main source of particulate contaminants.
[0003] The conventional electroplating process involves alkaline degreasing, hydrochloric acid activation, DC electroplating of zinc or zinc-nickel alloy, and trivalent chromium passivation. Screws produced using this process suffer from several problems: thread peak plating breaks due to high internal stress; mismatch in thermal expansion coefficients between the plating and the substrate under thermal cycling conditions leads to powdering and peeling; incomplete cleaning of thread valleys results in insufficient plating adhesion (commonly known as "false plating") and subsequent peeling; and unsealed micropores in the plating allow corrosive media to penetrate along defect channels, accelerating failure. Furthermore, in existing technologies, zinc-nickel alloy electroplating of carbon steel screws is typically deposited directly on the substrate without a pre-plated nickel diffusion barrier layer. This leads to the interdiffusion of Zn and Fe during thermal cycling, forming brittle intermetallic compounds that accelerate interface embrittlement and plating peeling. While stainless steel screws have a Cr2O3 passivation film, the activation effect is insufficient due to only hydrochloric acid activation before DC electroplating, and similarly, there is a lack of diffusion barrier protection from a pre-plated nickel intermediate layer. In summary, conventional processes cannot meet the stringent requirements for particulate contamination in AI liquid cooling plates. Summary of the Invention
[0004] The technical problem this invention aims to solve is to address the shortcomings of existing technologies where radiator screws generate plating debris and clog the microchannels of the liquid cooling plate during fastening and thermal cycling. This invention provides a debris-free screw manufacturing process specifically for AI liquid cooling plates. Through a synergistic process chain of multi-stage ultra-clean pretreatment, pre-plating with nickel, bidirectional pulse electroplating of zinc-nickel alloy, nanocomposite sealing, and gradient low-temperature curing, the residual stress of the plating is controlled below 80MPa and placed in a compressive stress state. This effectively reduces the amount of debris generated by the screws during fastening and long-term high-temperature cycling, ensuring the heat dissipation safety of the AI liquid cooling plate.
[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0006] First, the screws undergo a multi-stage ultra-clean pretreatment process, sequentially including hot alkaline degreasing, dual-frequency ultrasonic degreasing and dewaxing, multi-stage pure water washing, acid activation, neutralization, and pure water washing to obtain pre-treated screws. The dual-frequency ultrasonic degreasing and dewaxing process involves first using 40kHz ultrasonic cleaning followed by 80kHz ultrasonic cleaning. Next, a nickel undercoat is pre-plated, with a thickness of 0.8–1.2 μm, onto the surface of the pre-treated screws. Finally, the screws are immersed in an alkaline zinc-nickel alloy plating bath using a 100Hz bidirectional pulsed liquid. The power supply is electroplated with a zinc-nickel alloy coating with a thickness of 8–12 μm and a nickel content of 12–15 wt%. The single-cycle waveform consists of a forward conduction period of 4 ms, an intermittent shutdown period of 1.5 ms, a reverse conduction period of 0.5 ms, and an intermittent shutdown period of 4 ms. The forward pulse current density is 2.0 A / dm² with a duty cycle of 40%, and the reverse pulse current density is 0.5 A / dm² with a duty cycle of 5%. After electroplating, a nanocomposite sealing process is performed. The plated part is immersed in a sealing solution composed of a silane coupling agent KH-560 (5 vol%), nano-silica (5 wt%), and a mixed solvent of water and ethanol in a volume ratio of 3:1. After immersion for 30 seconds, it is pulled up at a speed of 2 mm / s to form an organic-inorganic composite film on the coating surface. Finally, gradient low-temperature curing is performed. The part is first held at 48–52 °C for 20 minutes, and then heated to 78–82 °C and held for 30 minutes to obtain a chip-free screw.
[0007] In the aforementioned process chain, the pre-plated nickel underlayer acts as a diffusion barrier layer, preventing Zn in the zinc-nickel alloy plating from diffusing into the substrate to form brittle intermetallic compounds, while simultaneously providing uniform nucleation sites for subsequent electroplating. Bidirectional pulse electroplating refines grain size and controls the plating to a compressive stress state through periodic forward deposition and reverse anodic dissolution, suppressing the initiation and propagation of microcracks during the bonding process from the source. In the nanocomposite sealing solution, the silane coupling agent hydrolyzes to form a Si-O-Si three-dimensional network, and nano-silica particles embed into the micropores of the plating, providing skeletal support and sealing. The resulting organic-inorganic composite film effectively blocks the penetration of corrosive media and thermal stress along defect channels. Gradient low-temperature curing first slowly evaporates the solvent at low temperatures to prevent cracking of the sealing film, then raises the temperature to promote complete silane condensation and cross-linking, eliminating the additional thermal stress generated by curing shrinkage at the film-plating interface.
[0008] Compared with the prior art, the beneficial effects of the present invention are:
[0009] In terms of debris control, the total amount of debris shed by the screws after repeated tightening 10 times under a torque of 1.2 N·m does not exceed 0.08 mg, and the amount of debris shed after 100 thermal cycles of -20℃ to 120℃ still does not exceed 0.10 mg, which meets the stringent cleanliness requirements of AI liquid-cooled plate microchannels for particulate contamination.
[0010] In terms of coating reliability, bidirectional pulse electroplating controls the residual stress of the coating to below 80MPa and in a compressive stress state, inhibiting the initiation and propagation of microcracks from the source. The pre-plated nickel underlayer blocks the diffusion of Zn-Fe interface and avoids the formation of brittle intermetallic compounds under thermal cycling. The combination of nanocomposite sealing and gradient low-temperature curing ensures that the overall defect channel density of the protection system does not exceed 1.5%. Under extreme thermal cycling conditions of -20℃ to 120℃, the coating is free from blistering, cracking, and discoloration.
[0011] Furthermore, this process is applicable to both 304 stainless steel and 10B21 carbon steel screws, covering the mainstream substrate types for AI liquid-cooled plate fasteners. The process steps and parameters have been verified by the barrel plating production line and are suitable for mass production. Attached Figure Description
[0012] Figure 1 This invention is the present invention.
[0013] Figure 2 This is a waveform timing diagram of a single cycle (10ms) of the bidirectional pulse power supply of the present invention.
[0014] Figure 3 This is a bar chart comparing the amount of chipping after 100 thermal cycles of Embodiment 1 and Comparative Examples 1, 2, and 3 of the present invention. Detailed Implementation
[0015] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0016] Example 1:
[0017] This embodiment describes the preparation of a low-stress zinc-nickel alloy coating on a 304 stainless steel M3 screw. The specific steps are as follows.
[0018] Step (1) Multi-stage ultra-clean pretreatment
[0019] Hot alkaline degreasing: Immerse the screws in a solution containing 50 g / L sodium hydroxide, 40 g / L sodium carbonate, 25 g / L trisodium phosphate, and 8 g / L octylphenol polyoxyethylene ether at 65 ± 2 °C for 10 minutes. This alkaline system removes stamping oil and polishing wax from the screw surface through saponification and emulsification.
[0020] Dual-frequency ultrasonic degreasing and dewaxing: The screws are immersed in a water-based dewaxing cleaner with a pH of 9.5±0.2. First, they are ultrasonically cleaned for 5 minutes at a frequency of 40kHz and a power density of 0.5W / cm², followed by ultrasonic cleaning for another 5 minutes at a frequency of 80kHz and a power density of 0.3W / cm², at a temperature of 60±2℃. The 40kHz low-frequency ultrasound generates strong cavitation bubble collapse impact force, suitable for removing macroscopic oil stains from the screw head and shank. The 80kHz high-frequency ultrasound generates cavitation bubbles with a diameter of approximately 5–10μm at the grooves of M3 threads, effectively penetrating the groove dead zones (approximately 160μm wide) for deep cleaning of the groove area. After three-stage countercurrent pure water rinsing, the conductivity of the final rinse water is ≤10μS / cm.
[0021] Acid activation: The screw was immersed in a mixed acid solution consisting of 80 ml / L hydrochloric acid and 15 ml / L hydrofluoric acid, and activated at 25±5℃ for 90 seconds. In the mixed acid system, the Cl⁻ of hydrochloric acid penetrated the passivation film on the stainless steel surface, and the F⁻ dissociated from hydrofluoric acid reacted with Cr₂O₃ to form a soluble [CrF₆]³⁻ complex ion. The two synergistically broke through the Cr₂O₃ passivation film on the 304 stainless steel surface, exposing the active metal surface. After activation, the screw was neutralized with a 5% sodium carbonate solution for 30 seconds, followed by two stages of pure water washing. The conductivity of the final stage water was ≤10 μS / cm.
[0022] Step (2) Pre-plating nickel base
[0023] The pretreated screws were placed in a Watt-type pre-plating nickel bath with a composition of 250 g / L nickel sulfate, 50 g / L nickel chloride, and 35 g / L boric acid, pH 4.0–4.4, and temperature 50 ± 2 °C. Pre-plating was performed for 3 minutes at a cathode current density of 1.0 A / dm² to obtain a uniform and dense nickel underlayer with a thickness of approximately 0.8–1.2 μm. The function of this nickel underlayer is twofold: as an activation layer, it provides uniform nucleation sites on the acid-activated stainless steel surface, improving the initial deposition uniformity of the subsequent zinc-nickel alloy plating; as a diffusion barrier layer, it prevents Zn in the zinc-nickel alloy plating from diffusing into the stainless steel substrate to form brittle intermetallic compounds and inhibits the migration of Fe elements from the substrate into the plating, avoiding interface embrittlement under high-temperature service conditions.
[0024] Step (3): Bidirectional pulse electroplating of zinc-nickel alloy
[0025] The pre-plated screws were placed in an alkaline zinc-nickel alloy plating bath. The bath composition consisted of 12 g / L zinc oxide, 120 g / L sodium hydroxide, 20 g / L nickel sulfate, 25 ml / L triethanolamine, 8 ml / L ethylenediamine, and 3 ml / L alkaline zinc-nickel alloy brightener. The pH value was 12.8–13.2, and the temperature was 25 ± 2℃. Triethanolamine acted as a nickel ion complexing agent to prevent nickel hydroxide precipitation, ethylenediamine assisted in complexation and grain refinement, and the brightener contained polyoxyethylene-polyoxypropylene block copolymer and coumarin derivatives, providing a bright and smooth plating appearance.
[0026] A bidirectional pulse power supply was activated at a frequency of 100Hz. Within a single 10ms cycle, the waveform timing was: forward conduction 4ms, intermittent shutdown 1.5ms, reverse conduction 0.5ms, and intermittent shutdown 4ms. The forward pulse current density was 2.0A / dm² with a duty cycle of 40%, and the reverse pulse current density was 0.5A / dm² with a duty cycle of 5%. Electroplating was performed for 25 minutes, yielding a zinc-nickel alloy coating with a thickness of 8–12μm and a nickel content of 12–15wt%.
[0027] The bidirectional pulse electroplating mechanism of this specific waveform is as follows: during the forward conduction period, zinc-nickel alloy electrodeposition is achieved; during the forward turn-off period, the ion concentration near the cathode is restored, reducing concentration polarization; during the reverse conduction period, high-energy atoms at the microscopic protrusions of the coating are briefly dissolved by anodic polarization, preferentially leveling the surface and dissolving the fragile phases with stress concentration at grain boundaries; during the reverse turn-off period, the surface potential is restored. Through this periodic leveling and grain boundary repair, the coating grain size is refined to 200–500 nm, and the residual stress is reduced to approximately 72 MPa, exhibiting a compressive stress state, significantly different from the 180–250 MPa tensile stress of DC electroplating coatings. Compressive stress can effectively suppress the initiation and propagation of microcracks during the bonding process, while tensile stress accelerates crack propagation and coating peeling.
[0028] Steps (2) and (3) are completed entirely on the barrel plating production line. The screws are loaded into the cylindrical barrel plating basket, with a loading capacity of 50% of the effective volume of the basket, and the rotation speed is set to 6 r / min. This coordinated control of the loading capacity and rotation speed ensures that the screws remain in loose contact during the tumbling process, avoiding micro-cracks and potential debris sources in the uncured plating layer due to excessive compression and collision. After electroplating, a two-stage pure water rinse is performed, with the final stage water conductivity ≤10 μS / cm.
[0029] Step (4) Nanocomposite sealing
[0030] The preparation method of the nanocomposite blocking solution is as follows: First, 5 vol% of silane coupling agent KH-560 is hydrolyzed in an aqueous acetic acid solution with a pH of 4.3–4.7 at room temperature for 25 minutes to form a hydrolysate; separately, 5 wt% of nano-silica (particle size 20–40 nm, specific surface area approximately 200 m² / g) is ultrasonically dispersed in anhydrous ethanol for 20 minutes until homogeneous; then, the KH-560 hydrolysate and the nano-silica ethanol dispersion are mixed and brought to a final volume with a mixed solvent of deionized water and anhydrous ethanol at a volume ratio of 3:1 to ensure uniform particle dispersion and no agglomeration. The blocking solution should be prepared immediately and used within 4 hours.
[0031] The electroplated parts are immersed in the above-mentioned sealing solution at 25±5℃ for 30 seconds, and then slowly pulled out of the solution at a speed of 2mm / s. After hydrolysis of KH-560, a three-dimensional Si-O-Si network is formed. Nano-silica particles are embedded in the micropores of the coating (pore size of about 50-200nm) to provide skeletal support, while organosiloxane segments provide flexibility, forming a dense organic-inorganic composite film with a certain degree of deformability on the coating surface.
[0032] Step (5) Gradient low-temperature curing
[0033] The sealed screws are then subjected to gradient drying in a clean oven: the first stage involves holding at 50±2℃ for 20 minutes to allow the solvent to evaporate slowly, preventing rapid boiling that could cause the sealing film to crack; the second stage involves raising the temperature to 80±2℃ and holding for 30 minutes to promote complete silane condensation and crosslinking reactions. After curing, a composite protective film with a thickness of approximately 200–400 nm is formed. This gradient curing process, in conjunction with the low-stress coating obtained by pulse electroplating, further releases residual thermal stress at the interface, ensuring the structural integrity of the coating-sealing film system during thermal cycling at 80–120℃.
[0034] Comparative Example 1:
[0035] The only difference between Comparative Example 1 and Example 1 was the electroplating method. Using the exact same substrate, pretreatment process, and pre-nickel plating process as Example 1, the substrate was immersed in the same alkaline zinc-nickel alloy plating bath as Example 1 and electroplated using direct current at a current density of 2.0 A / dm² for approximately 14 minutes to obtain a zinc-nickel alloy coating with a thickness of 8–12 μm. After electroplating, a two-stage pure water rinse was performed, followed by nanocomposite sealing and gradient low-temperature curing, just like in Example 1. The only difference between Comparative Example 1 and Example 1 was that bidirectional pulse electroplating was replaced with direct current electroplating.
[0036] Comparative Example 2:
[0037] The nano-sealing was removed, and all the steps were exactly the same as in Example 1. However, after the pure water wash in step (3) after plating, the nano-composite sealing and gradient low-temperature curing were not performed. Instead, the nano-composite sealing and gradient low-temperature curing were replaced by hot air drying at 60°C for 20 minutes.
[0038] Comparative Example 3:
[0039] The curing method was changed, and all the steps were exactly the same as in Example 1, but the gradient low temperature curing was replaced with a one-time drying with 80°C hot air for 50 minutes. The total curing time was the same as in Example 1, only the temperature program was changed.
[0040] Performance testing methods:
[0041] Debris shedding test: Ten samples (n=10) were taken. Each sample was tightened with a 304 stainless steel nut (nut roughness Ra≤0.8μm) at a torque of 1.2 N·m. The tightening (screwing in and out) was repeated 10 times. Before each tightening, the threads were cleaned with a lint-free cloth soaked in isopropyl alcohol and then dried. The total mass of debris from each sample was collected and weighed in a Class 100 clean environment, with an electronic balance accuracy of 0.01 mg. The torque curve was monitored during the test. If a sudden change in torque occurred, the sample data was discarded and the nut was replaced for retesting.
[0042] Residual stress test of coating: According to GB / T7704 standard, X-ray diffraction sin²ψ method, Cu-Kα radiation, characteristic diffraction peaks of zinc-nickel alloy are selected, ψ tilt angle range is 0°~45°, and residual stress value is calculated by linear fitting of sin²ψ.
[0043] Coating adhesion test: According to GB / T5270-2005 thermal shock test, after heating at 200±5℃ for 1 hour, quench in deionized water at 25±5℃, cycle 3 times, and inspect with a stereomicroscope at 50×.
[0044] High-temperature cycling test: Thermal cycling conditions are 120℃ / -20℃, with a heating / cooling rate of approximately 10℃ / min, and holding at both high and low temperatures for 30 minutes each. Five parallel samples (three samples per group, subjected to 20 / 40 / 60 / 80 / 100 cycles respectively) are prepared and tested simultaneously with the main sample group. After each group of cycles, the amount of chipping is measured according to the chipping amount test method.
[0045] Overall defect channel density test of the protection system: The potassium ferricyanide-sodium chloride filter paper method was used, and the test was conducted at 25±5℃ for 10 minutes. The results reflect the density of defect channels that penetrate the closed film-coating composite system and reach the substrate.
[0046] Test results:
[0047] The test results of Example 1 and each comparative example are shown in Table 1.
[0048] Table 1. Performance comparison between Example 1 and the comparative example.
[0049] Test Project Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Desquamation amount (mg) 0.05±0.02 0.46±0.08 0.75±0.18 0.22±0.05 Residual stress of coating (MPa) 72±6 (compressive stress) 195±15 (tensile stress) 78±5 (compressive stress) 85±7 (compressive stress) Thermal shock test (3 cycles) No bubbling, no peeling Microbubbles appeared in the second cycle. Microbubbles appeared in the second cycle. Localized blistering during the third cycle Desquamation amount (mg) after 20 thermal cycles ≤0.06 0.25~0.40 0.40~0.65 0.08~0.15 Desquamation amount (mg) after 40 thermal cycles ≤0.07 0.40~0.65 0.70~1.10 0.10~0.18 Shedding amount (mg) after 60 thermal cycles ≤0.08 0.55~0.90 1.00~1.60 0.12~0.22 Shedding amount (mg) after 80 thermal cycles ≤0.09 0.70~1.20 1.30~2.20 0.15~0.27 Shedding amount (mg) after 100 thermal cycles ≤0.10 0.80~1.50 1.80~3.20 0.30~0.60 Defect channel density (%) ≤1.5 ≥8 ≥6 ≥5
[0050] As shown in Table 1, Example 1 is significantly better than the comparative examples in terms of both the amount of chipping during fastening and the amount of chipping during thermal cycling.
[0051] In Comparative Example 1, after replacing bidirectional pulse electroplating with direct current electroplating, the residual stress reversed from 72 MPa compressive stress to 195 MPa tensile stress, and the amount of chipping during bonding increased from 0.05 mg to 0.46 mg (an increase of approximately 9 times). After 100 thermal cycles, the amount of chipping increased from ≤0.10 mg to 0.80–1.50 mg (an increase of approximately 8–15 times). This demonstrates that bidirectional pulse electroplating is the core step in controlling the stress state of the coating and reducing chipping. Direct current electroplating lacks a pulse off-phase, and under high current density, it is accompanied by a strong hydrogen evolution side reaction. Ion depletion is severe near the cathode, resulting in coarse coating grains and a tensile stress state. During bonding and thermal cycling, microcracks rapidly initiate and propagate. Notably, the defect channel density of Comparative Example 1 (≥8%) was abnormally higher than that of Comparative Example 2 (≥6%). This is because the high-stress, coarse-grained coating produced by DC electroplating contains a network of penetrating cracks. The sealing film can only fill the surface micropores and cannot completely repair the structural cracks. The sealing film fails locally at the crack tips, allowing the reagent to rapidly penetrate along the cracks. This further confirms that the dense, fine-grained coating obtained by pulse electroplating is a prerequisite for effective sealing.
[0052] In Comparative Example 2, after the removal of the nanocomposite sealing, the amount of chip removal after 100 thermal cycles increased sharply from ≤0.10 mg to 1.80–3.20 mg (an increase of approximately 18–32 times), demonstrating that the nanocomposite sealing plays a decisive role in chip prevention under thermal cycling conditions. During long-term thermal cycling, the micropores of the coating become concentrated channels for corrosive media and thermal stress. Without the protection of the sealing film, stress corrosion cracking preferentially occurs at the micropores and gradually expands, ultimately leading to large-area peeling of the coating.
[0053] In Comparative Example 3, replacing gradient low-temperature curing with a single high-temperature drying process only increased the residual stress from 72 MPa to 85 MPa (an increase of 13 MPa), making it difficult for XRD to detect a significant change. However, localized blistering appeared in the thermal shock test, and the amount of shedding material increased from 0.05 mg to 0.22 mg, and after 100 thermal cycles, the amount of shedding material increased to 0.30–0.60 mg. The reason for this is that gradient curing eliminates the localized additional thermal stress at the sealed film-coating interface. The single high-temperature drying process causes rapid curing and shrinkage of the sealed film, resulting in micro-area tensile stress concentration at the film-coating interface. This interfacial stress cannot be reflected in XRD macroscopic residual stress testing (detection depth is typically 5–20 μm) due to limitations in spatial resolution and detection scale, but it is sufficient to induce localized blistering under thermal shock conditions and interfacial delamination during thermal cycling. This demonstrates that gradient low-temperature curing plays an irreplaceable role in interfacial stress regulation.
[0054] The univariate comparative experiments revealed the cross-scale synergistic effect between the steps: pulse electroplating controls the stress source, crack density, and stress properties within the bulk phase at the grain scale (200–500 nm); nano-sealing blocks corrosion and stress concentration channels at the micropore scale (50–200 nm); and gradient curing eliminates the additional thermal stress generated by curing shrinkage at the film-coating interface scale (200–400 nm). Without any step, the failure mechanism at the corresponding scale is not suppressed, and there is a coupling amplification effect between the failure mechanisms at different scales—the through-crack network of the high-stress coarse-grained coating causes local failure of the sealing film, while the absence of the sealing film accelerates the penetration of the corrosive medium along the cracks, and the interface peeling under thermal stress is drastically amplified, resulting in a significant increase in the final amount of chipping.
[0055] Example 2:
[0056] The process steps and parameters were exactly the same as in Example 1, except that the substrate was replaced with 10B21 carbon steel (boron steel for cold heading, with main components of C 0.18-0.23%, Mn 0.70-1.00%, and B ≥ 0.0005%) instead of 304 stainless steel. The acid activation in step (1) was adjusted to immerse the screw in an acid solution of 150 ml / L hydrochloric acid and activate it at 25±5°C for 60 seconds. Carbon steel does not have a Cr2O3 passivation film, so hydrofluoric acid is not required.
[0057] Comparative Example 4:
[0058] Using the same 10B21 carbon steel M3 substrate as in Example 2, the substrate was treated with a conventional electroplating process: alkaline degreasing (sodium hydroxide 50g / L, 65℃, 10min) → hydrochloric acid activation (hydrochloric acid 150ml / L, 25±5℃, 60s) → DC electroplating of zinc-nickel alloy (2.0A / dm², approximately 14min, plating solution same as in Example 2, thickness 8-12μm) → trivalent chromium passivation (25±5℃, 20s) → hot air drying at 60℃ for 20min. Trivalent chromium passivation only provides a surface passivation film and has no micropore filling capability; it is a conventional passivation method in the art.
[0059] Test results of Example 2 and Comparative Example 4:
[0060] Table 2 Performance comparison between Example 2 and Comparative Example 4
[0061] Test Project Example 2 Comparative Example 4 Desquamation amount (mg) 0.06±0.02 2.20±0.50 Residual stress of coating (MPa) 68±5 (compressive stress) 210±18 (tensile stress) Thermal shock test (3 cycles) No bubbling, no peeling Bubbling occurs on the first cycle. Shedding amount (mg) after 100 thermal cycles ≤0.10 4.50~7.00 Defect channel density (%) ≤1.5 ≥10
[0062] As shown in Table 2, the average chip loss of Example 2 (0.06 mg) is at the same level as Example 1 (0.05 mg), and the residual stress (68 MPa) is comparable to that of Example 1 (72 MPa), proving that the process is also applicable to carbon steel substrates. The chip loss of Comparative Example 4 (2.20 mg) is significantly higher than that of Comparative Example 1 (0.46 mg, DC electroplating of stainless steel). This is because the carbon steel substrate lacks a Cr2O3 passivation film and a pre-plated nickel diffusion barrier layer, leading to severe interdiffusion at the Zn-Fe interface during thermal cycling, generating brittle intermetallic compounds and drastically exacerbating interface corrosion and plating peeling. This further confirms the crucial role of pre-plated nickel for carbon steel screws.
[0063] The above embodiments use M3 specification 304 stainless steel and 10B21 carbon steel screws as examples to illustrate the process of the present invention in detail. For screws of other specifications in the range of M2 to M5, the process parameters such as ultrasonic power density, electroplating time, and barrel plating load can be adjusted accordingly according to the screw size, and the implementation effect is the same as that of the above embodiments.
[0064] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0065] The above description is only used to illustrate the technical solution of the present invention and is not intended to limit it. Any other modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention, as long as they do not depart from the spirit and scope of the technical solution of the present invention, should be covered within the scope of the claims of the present invention.
Claims
1. A manufacturing process for chip-free screws specifically designed for AI liquid cooling plates in radiators, characterized by: Includes the following steps: Step (1) Multi-stage ultra-clean pretreatment: The screws are subjected to hot alkaline degreasing, dual-frequency ultrasonic degreasing and dewaxing, multi-stage pure water washing, acid activation, neutralization and pure water washing in sequence to obtain pretreated screws; the dual-frequency ultrasonic degreasing and dewaxing includes first using 40kHz ultrasonic cleaning and then using 80kHz ultrasonic cleaning. Step (2) Pre-plating nickel base layer: Electroplating a nickel base layer with a thickness of 0.8 to 1.2 μm on the surface of the pre-treated screw; Step (3) Bidirectional pulse electroplating of zinc-nickel alloy: On the nickel substrate, in an alkaline zinc-nickel alloy plating bath, a zinc-nickel alloy coating is electroplated using a bidirectional pulse power supply with a frequency of 100Hz. The thickness of the zinc-nickel alloy coating is 8-12μm, and the nickel content is 12-15wt%. The single-cycle waveform of the bidirectional pulse power supply includes forward conduction for 4ms, intermittent shutdown for 1.5ms, reverse conduction for 0.5ms, and intermittent shutdown for 4ms. The forward pulse current density is 2.0A / dm², and the duty cycle is 40%. The reverse pulse current density is 0.5A / dm², and the duty cycle is 5%. Step (4) Nanocomposite sealing: Immerse the plated part obtained in step (3) into the nanocomposite sealing solution, and after immersion for 30 seconds, pull it up at a speed of 2 mm / s to form an organic-inorganic composite film on the surface of the zinc-nickel alloy plating layer; the nanocomposite sealing solution is composed of silane coupling agent KH-560 5 vol%, nano silica 5 wt%, and the balance water and ethanol mixed solvent, the particle size of the nano silica is 20-40 nm, the volume ratio of water to ethanol is 3:1, and the pH value of the nanocomposite sealing solution is 4.3-4.7; Step (5) Gradient low temperature curing: The screws treated in step (4) are first kept at 48-52℃ for 20 minutes, and then heated to 78-82℃ and kept for 30 minutes to obtain the chip-free screws for the AI liquid cooling plate of the heat sink.
2. The production process according to claim 1, characterized in that, In step (1), the power density of the 40kHz ultrasound is 0.5W / cm², and the cleaning time is 5 minutes; the power density of the 80kHz ultrasound is 0.3W / cm², and the cleaning time is 5 minutes; the cleaning temperature is 58~62℃.
3. The production process according to claim 1, characterized in that, In step (1), when the screw is a stainless steel screw, the acid activation uses a mixed acid solution composed of 250 ml / L hydrochloric acid and 15 ml / L hydrofluoric acid, and the activation time is 75 to 105 seconds; when the screw is a carbon steel screw, the acid activation uses a solution of 150 ml / L hydrochloric acid, and the activation time is 50 to 70 seconds.
4. The production process according to claim 1, characterized in that, In step (2), the plating solution used for the pre-plating of nickel is composed of: 240 g / L nickel chloride and 120 g / L hydrochloric acid, and the temperature is room temperature; the cathode current density for electroplating is 3.0 A / dm², and the electroplating time is 15~20 minutes.
5. The production process according to claim 1, characterized in that, In step (3), the alkaline zinc-nickel alloy plating solution consists of: 12 g / L zinc oxide, 120 g / L sodium hydroxide, 20 g / L nickel sulfate, 25 ml / L triethanolamine, 8 ml / L ethylenediamine, and 3 ml / L alkaline zinc-nickel alloy brightener. The pH value is 12.8–13.2, the temperature is 23–27°C, and the electroplating time is 25 minutes.
6. The production process according to claim 1, characterized in that, Steps (2) and (3) are both completed on the barrel plating production line. The barrel plating load is 50% of the effective volume of the barrel, and the barrel speed is 6 r / min.
7. The production process according to claim 1, characterized in that, When the screw is an M3 specification 304 stainless steel or 10B21 carbon steel screw; In step (1), the power density of the 40kHz ultrasound is 0.5W / cm², the cleaning time is 5 minutes, the power density of the 80kHz ultrasound is 0.3W / cm², the cleaning time is 5 minutes, and the cleaning temperature is 58-62℃. When the screw is a stainless steel screw, the acid activation uses a mixed acid solution composed of 250ml / L hydrochloric acid and 15ml / L hydrofluoric acid, and the activation time is 75-105 seconds. When the screw is a carbon steel screw, the acid activation uses a solution of 150ml / L hydrochloric acid, and the activation time is 50-70 seconds. In step (2), the plating solution used for the pre-plating of nickel is composed of 240 g / L nickel chloride and 120 g / L hydrochloric acid, and the temperature is room temperature; the cathode current density for electroplating is 3.0 A / dm², and the electroplating time is 15~20 minutes; In step (3), the alkaline zinc-nickel alloy plating solution consists of 12 g / L zinc oxide, 120 g / L sodium hydroxide, 20 g / L nickel sulfate, 25 ml / L triethanolamine, 8 ml / L ethylenediamine, and 3 ml / L alkaline zinc-nickel alloy brightener. The pH value is 12.8–13.2, the temperature is 23–27°C, and the electroplating time is 25 minutes. Both steps (2) and (3) are completed on the barrel plating production line, with the barrel plating load being 50% of the effective volume of the barrel and the barrel speed being 6 r / min.