Aluminum alloy surface fluorinated anticorrosion film and preparation method thereof

By introducing potassium fluoride into the plasma electrolytic fluorination process to generate a composite fluoride phase, the problems of thin film and poor adhesion on the surface of aluminum alloys are solved, resulting in a significant improvement in the corrosion resistance of aluminum alloys. The film thickness is increased and the structure is dense, providing long-term protection.

CN123153133APending Publication Date: 2026-11-24LIAONING UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611677950.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing plasma electrolytic fluorination processes produce thin films on aluminum alloy surfaces with slow growth rates and poor film-substrate adhesion, resulting in insufficient corrosion resistance of aluminum alloys and limiting their application range.

Method used

Potassium fluoride additives are introduced into fluorinated organic electrolytes to participate in the film-forming reaction and generate a composite fluoride phase, thereby improving the film thickness and density. A fluorinated anti-corrosion film is formed on the surface of aluminum alloy using plasma electrolytic fluorination process.

Benefits of technology

It significantly improves the corrosion resistance of aluminum alloys, with the charge transfer resistance of the film reaching the order of 10⁵Ω·cm², the corrosion current density reduced by about two orders of magnitude, the film thickness increased to more than 18μm, the structure is dense and tightly bonded, and the long-term protection effect is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123153133A_ABST
    Figure CN123153133A_ABST
Patent Text Reader

Abstract

This invention discloses a fluorinated anti-corrosion film on aluminum alloy surfaces and its preparation method, belonging to the field of metal surface treatment and anti-corrosion technology. Addressing the problems of thin and insufficient corrosion resistance in existing plasma electrolytic fluorinated films, this invention uses aluminum alloy as the anode and stainless steel plate as the cathode, employing a constant current pulse mode for plasma electrolytic fluorination in an ethylene glycol organic electrolyte containing ammonium fluoride and potassium fluoride. Potassium ions participate in the film-forming reaction, generating a composite fluoride phase of AlF3 and KAlF4. The film thickness is increased from 5-6 μm in a single ammonium fluoride system to over 18 μm, reaching 25 μm under optimal conditions, with a continuous and dense structure. The resulting film has a charge transfer resistance of 10 Ω·cm. 5 Ω·cm 2 The corrosion current density is reduced by about two orders of magnitude compared to bare aluminum alloys. It still maintains good corrosion resistance after immersion for 120 hours. The process is simple and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal surface treatment and corrosion protection technology, and specifically relates to a fluorinated anti-corrosion film on aluminum alloy surface and its preparation method. Background Technology

[0002] Aluminum alloys are widely used in aerospace, transportation, building decoration, and electronic equipment due to their low density, high specific strength, and good thermal and electrical conductivity. However, aluminum alloys themselves have low hardness, and the naturally formed oxide film on their surface is extremely thin (usually only a few nanometers), with high porosity and limited protective ability. They are highly susceptible to corrosion in harsh environments such as humidity, salt spray, and acid / alkali conditions, severely limiting their application range and service life. To improve the corrosion resistance of aluminum alloys, surface treatment technologies such as anodizing, micro-arc oxidation, chemical conversion, and electroplating are commonly used in industry. Among them, micro-arc oxidation (MAO) technology can generate a ceramic oxide film on the surface of aluminum alloys, which has high hardness and wear resistance. However, traditional micro-arc oxidation films have defects such as numerous pores and obvious cracks, allowing corrosive media to easily penetrate into the substrate through the pores, resulting in unsatisfactory long-term protective effects.

[0003] Plasma electrolytic fluorination (PEF) is a novel surface treatment technology that generates a fluoride film on a metal surface through plasma discharge in a fluorinated organic electrolyte. Compared to traditional oxide films, fluorinated films have lower surface energy and better chemical stability, theoretically providing superior corrosion protection. However, existing plasma electrolytic fluorination processes generally suffer from problems such as thin films, slow growth rates, and poor film-substrate adhesion. A single ammonium fluoride electrolyte system is also insufficient for producing high-quality thick films, limiting the practical application of this technology.

[0004] Therefore, developing a new plasma electrolytic fluorination process that can significantly improve film thickness and density and effectively enhance the corrosion resistance of aluminum alloys has important engineering application value. Summary of the Invention

[0005] To address the problems of thin and insufficient corrosion resistance of plasma electrolytic fluorinated films on aluminum alloys in existing technologies, this invention provides a fluorinated anti-corrosion film on the surface of aluminum alloys and its preparation method. By introducing potassium fluoride additives into a fluorinated organic electrolyte, potassium ions participate in the film-forming reaction to generate a composite fluoride phase, significantly increasing the film thickness and improving its density, thereby greatly enhancing the corrosion resistance of aluminum alloys.

[0006] The technical solution adopted in this invention is as follows: a method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, comprising the following steps.

[0007] Step 1: Pre-treat the aluminum alloy substrate for later use.

[0008] Step 2: Prepare a fluorinated organic electrolyte containing ammonium fluoride and potassium fluoride.

[0009] Step 3: Using a stainless steel plate as the cathode and a pretreated aluminum alloy substrate as the anode, plasma electrolytic fluorination is performed in a constant current pulse mode.

[0010] Step 4: After processing, remove the sample, clean and dry it to obtain a fluorinated anti-corrosion film on the aluminum alloy surface.

[0011] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, the pretreatment in step 1 specifically involves: grinding the aluminum alloy sample step by step with sandpaper, then washing it with NaOH alkali, then with hydrochloric acid, then ultrasonically cleaning it with ethanol, and finally drying it for later use.

[0012] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 2, the fluorinated organic electrolyte is one or more of the following: an ethylene glycol solution of ammonium fluoride, an ethylene glycol solution of potassium fluoride, an ethylene glycol solution of ammonium hydrogen fluoride, and an ethylene glycol solution of lithium tetrafluoroborate. The concentration of ammonium fluoride is 40~120 g / L, the concentration of potassium fluoride is 20~100 g / L, the concentration of ammonium hydrogen fluoride is 0~58 g / L, and the concentration of lithium tetrafluoroborate is 0~58 g / L.

[0013] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 2, the fluorinated organic electrolyte is an ethylene glycol solution containing 74 g / L ammonium fluoride and / or 90 g / L potassium fluoride.

[0014] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 3, the anolyte current density in the constant current pulse mode is 2~12 A / dm². 2 .

[0015] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 3, the pulse frequency in the constant current pulse mode is 200~2000Hz.

[0016] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 3, the pulse duty cycle in the constant current pulse mode is 5%~50%.

[0017] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, in step 3, the plasma electrolytic fluorination treatment time is 5~30 min.

[0018] In the above-mentioned method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, step 3, the plasma electrolytic fluorination process parameters are: current density 6 A / dm³. 2 The pulse frequency is 800Hz, the duty cycle is 30%, and the processing time is 12min.

[0019] The fluorinated anti-corrosion film on the surface of the aluminum alloy prepared by the above preparation method.

[0020] The beneficial effects of this invention are as follows.

[0021] 1. Significantly improved corrosion resistance. This invention introduces potassium fluoride into the electrolyte, allowing potassium ions to participate in the film-forming reaction and generate a composite fluoride phase. The charge transfer resistance of the film can reach 10 Ω·cm. 5 Ω·cm 2 The corrosion current density is reduced by approximately two orders of magnitude compared to bare aluminum alloy, resulting in a significant improvement in corrosion resistance. After a 120-hour immersion test, the film still maintains good corrosion resistance, demonstrating excellent long-term protective performance.

[0022] 2. Increased film thickness and denser structure. The introduction of potassium fluoride significantly promotes film growth, increasing the film thickness from 5-6 μm in the single ammonium fluoride system to over 18 μm, and reaching 25 μm under optimal process conditions. Simultaneously, the composite fluoride phase fills the intergranular spaces of aluminum fluoride, effectively inhibiting microcrack propagation. The film exhibits good overall continuity, high density, and tight bonding with the substrate.

[0023] 3. Simple process, suitable for industrialization. This invention adopts a one-step plasma electrolytic fluorination process, eliminating the need for complex post-processing steps. The process flow is short and the operation is simple. The electrolyte system is stable, the process parameter window is wide, and it is easy to achieve large-scale production, showing broad application prospects in the field of aluminum alloy corrosion protection. Attached Figure Description

[0024] Figure 1 (a) Time-voltage curves for preparing fluorinated films with different electrolytes and (b) Comparison of film thicknesses.

[0025] Figure 2 The surface SEM images of aluminum fluoride films prepared in different electrolytes are shown, where (a) F; (b) F / H; (c) F / K; and (d) F / B.

[0026] Figure 3 The cross-sectional elemental distribution diagrams of aluminum fluoride films prepared in different electrolytes are shown, where (a) F; (b) F / H; (c) F / K; and (d) F / B.

[0027] Figure 4 XRD patterns of aluminum fluoride films prepared in different electrolytes.

[0028] Figure 5 Potential dynamic polarization curves of aluminum fluoride films prepared in different electrolytes.

[0029] Figure 6Electrochemical impedance spectroscopy (EIS) of aluminum fluoride films prepared in different electrolytes is shown, where (a) is the Nyquist plot; (b) is the Bode impedance plot; and (c) is the Bode phase angle plot.

[0030] Figure 7 The following are the impedance spectra of the samples corresponding to the orthogonal experimental table: (a) is the Nyquist plot of samples 1-4, (b) is the Bode impedance plot of samples 1-4, (c) is the Bode phase angle plot of samples 1-4, (d) is the Nyquist plot of samples 5-8, (e) is the Bode impedance plot of samples 5-8, (f) is the Bode phase angle plot of samples 5-8, (g) is the Nyquist plot of samples 9-12, (h) is the Bode impedance plot of samples 9-12, (i) is the Bode phase angle plot of samples 9-12, (j) is the Nyquist plot of samples 13-16, (k) is the Bode impedance plot of samples 13-16, and (l) is the Bode phase angle plot of samples 13-16.

[0031] Figure 8 Cross-sectional elemental surface scans of the optimal sample F / K-optimized, where (a) is the SEM image of F / K-optimized, (b) is the nitrogen element distribution map, (c) is the oxygen element distribution map, (d) is the fluorine element distribution map, and (e) is the aluminum element distribution map.

[0032] Figure 9 This is a schematic diagram of the formation mechanism of plasma electrolytic fluorinated film, where 1 is the aluminum alloy substrate, 2 is the AlF3 phase, and 3 is the KAlF4 phase. Detailed Implementation

[0033] The present invention will be further described in detail below with reference to specific embodiments.

[0034] Example 1.

[0035] In this embodiment, an aluminum alloy fluorinated film is prepared using a single ammonium fluoride electrolyte. The specific steps are as follows.

[0036] (1) Pretreatment: Cut 6061 aluminum alloy into 20mm×30mm×3mm samples and drill holes on the short side; polish with 200, 400, 800, 1200 and 2000 grit sandpaper in sequence, rinse with deionized water; soak in 0.5mol / L NaOH solution for 5s, rinse with deionized water for 5s; soak in 5wt% hydrochloric acid solution for 5s, rinse with deionized water for 10s; finally place in ethanol for ultrasonic cleaning for 15s, blow dry with nitrogen and set aside.

[0037] (2) Electrolyte preparation: Use ethylene glycol as solvent to prepare an ammonium fluoride (NH4F) solution with a concentration of 74 g / L and stir until completely dissolved.

[0038] (3) Plasma electrolytic fluorination: Single-pulse constant current mode was used, with a stainless steel plate as the cathode and an aluminum alloy sample as the anode; process parameters: anode current density 6A / dm 2 The pulse frequency is 800Hz, the duty cycle is 20%, and the reaction time is 12min; the electrolyte temperature is controlled below 30℃ during the reaction.

[0039] (4) Post-processing: Take out the sample, ultrasonically clean it with deionized water for 10 min, dehydrate it with anhydrous ethanol, and dry it with hot air at 60℃ for 15 min. The prepared sample is named F.

[0040] Example 2.

[0041] In this embodiment, an aluminum alloy fluorinated film is prepared using a mixed electrolyte of ammonium fluoride and ammonium hydrogen fluoride. The specific steps are as follows.

[0042] (1) Pretreatment: Same as in Example 1.

[0043] (2) Electrolyte preparation: Using ethylene glycol as solvent, prepare a mixed solution containing 74 g / L ammonium fluoride (NH4F) and 57 g / L ammonium hydrogen fluoride (NH4HF2), and stir until completely dissolved.

[0044] (3) Plasma electrolytic fluorination: Same as Example 1.

[0045] (4) Post-processing: Same as in Example 1, the prepared sample is named F / H.

[0046] Example 3.

[0047] In this embodiment, an aluminum alloy fluorinated composite membrane is prepared using a mixed electrolyte of ammonium fluoride and potassium fluoride. The specific steps are as follows.

[0048] (1) Pretreatment: Same as in Example 1.

[0049] (2) Electrolyte preparation: Using ethylene glycol as solvent, prepare a mixed solution containing 74 g / L ammonium fluoride (NH4F) and 90 g / L potassium fluoride (KF), and stir until completely dissolved.

[0050] (3) Plasma electrolytic fluorination: Single-pulse constant current mode was used, with a stainless steel plate as the cathode and an aluminum alloy sample as the anode; process parameters: anode current density 6A / dm 2 The pulse frequency is 800Hz, the duty cycle is 20% or 30%, and the reaction time is 12min; the electrolyte temperature is controlled below 30℃ during the reaction.

[0051] (4) Post-processing: Same as in Example 1, the prepared sample is named F / K.

[0052] Example 4.

[0053] In this embodiment, an aluminum alloy fluorinated film is prepared using a mixed electrolyte of ammonium fluoride and lithium tetrafluoroborate. The specific steps are as follows.

[0054] (1) Pretreatment: Same as in Example 1.

[0055] (2) Electrolyte preparation: Using ethylene glycol as solvent, prepare a mixed solution containing 74 g / L ammonium fluoride (NH4F) and 58 g / L lithium tetrafluoroborate (LiBF4) and stir until completely dissolved.

[0056] (3) Plasma electrolytic fluorination: Same as Example 1.

[0057] (4) Post-processing: Same as in Example 1, the prepared sample is named F / B.

[0058] Performance testing.

[0059] (1) Growth of fluorinated film: Figure 1 (a) Time-voltage curves of fluorinated films prepared in different electrolytes. As can be seen from the figure, all samples experienced a rapid voltage rise and a slow voltage rise. For the same energizing time, the voltages of the four samples from highest to lowest are: F, F / H, F / B, and F / K. The final cutoff voltages of these four samples are 420V, 370V, 350V, and 350V, respectively. This indicates that the addition of NH4HF2, KF, and LiBF4 during plasma electrolytic fluorination reduces the plasma electrolytic fluorination voltage.

[0060] The thickness of the fluorinated film prepared in different electrolytes was measured using a thickness gauge, and the results are as follows: Figure 1 As shown in (b), the F / K sample has the largest film thickness, approximately 18.5 μm, significantly higher than the other samples. The F / B sample has the second thickest film thickness, approximately 11.5 μm. The F and F / H samples have relatively thinner film thicknesses, at 5.8 μm and 4.7 μm, respectively. In summary, the electrolyte composition has a decisive influence on film thickness: the addition of potassium fluoride significantly increases film thickness, while ammonium bifluoride tends to inhibit film growth.

[0061] (2) Surface morphology of different fluorinated films: Figure 2 SEM images of fluorinated membranes prepared in different electrolytes. Figure 2(a) It can be seen that the surface of sample F is composed of a lamellar structure, which is formed by the stacking of small, irregular particles. The film surface has a large number of small and irregularly shaped pores, and the overall structure is relatively loose. Compared with sample F, the surface particles of sample F / H are even smaller, and the surface smoothness is slightly improved, but small microcracks can still be observed in some areas. Sample F / K exhibits unique morphological characteristics, with increased surface pore size and crater-like ridges around the pores. The high degree of sintering between particles indicates that the addition of potassium fluoride significantly enhances the discharge intensity and forms a larger discharge channel. The surface of sample F / B presents a fragmented lamellar structure with extremely small and uniform pores.

[0062] (3) Elemental surface scans of different fluorinated film cross-sections: such as Figure 3 As shown in the elemental distribution diagram, the substrate is mainly composed of Al. While the film thickness varies across all samples, they all contain F, which originates from fluorides in the electrolyte. Figure 3 (a) It can be seen that the cross-sectional thickness of each sample is uniform, and the interface between the film and the substrate is clear. From Figure 3 (b) It can be seen that the F / H sample has the smallest film thickness, but a more compact overall structure with a significantly reduced number of internal pores. This indicates that the addition of ammonium bifluoride promotes the formation of a thinner film structure. Figure 3 (c) It can be seen that the F / K sample has the largest cross-sectional thickness, significantly exceeding that of the previous two groups, and is comparable to... Figure 1 (b) The results are consistent. The interface between the film and the substrate is tight, with almost no obvious cavities or cracks observed. The presence of potassium in the film indicates that potassium ions participated in the film-forming reaction, forming the KAlF4 compound. Figure 3 (d) It can be seen that the film thickness of the cross section of the F / B sample is significantly thinner and the fluorine signal is weaker, indicating that there is less fluorine in the film.

[0063] (4) XRD patterns of different fluorinated films: such as Figure 4 As shown, in samples F, F / H, and F / B, only the characteristic peaks of AlF3 were observed besides the diffraction peaks of the Al substrate, indicating that the film is mainly composed of AlF3 with no other phases. In sample F / K, in addition to the diffraction peaks of the aluminum substrate and aluminum fluoride, new diffraction peaks appeared, corresponding to the KAlF4 compound. This indicates that potassium ions participated in the film-forming reaction during the preparation of sample F / K, generating the new phase KAlF4. It can be inferred that the formation of KAlF4 is an important reason for the increase in film thickness. In sample F / B, the diffraction peaks of the aluminum substrate are dominant, while the diffraction peaks of aluminum fluoride are very weak, indicating that the aluminum fluoride content in the film is very low.

[0064] (5) Polarization curves of different fluorinated films: such as Figure 5 As shown, the corrosion current density (I) of the Al matrix is...corr The maximum value is 1.156 × 10⁻⁶. -5 A·cm -2 The corrosion rate (CR) was 1.26 × 10⁻⁶. -1 mm / a, corrosion potential (E) corr The most negative value indicates the fastest corrosion rate and the worst corrosion resistance. All four film samples showed a significant positive shift in corrosion potential and a significant decrease in corrosion current density, indicating that all films effectively inhibited the corrosion reaction of the aluminum alloy. The F / K sample had the most positive corrosion potential at -1.232V, a positive shift of 0.102V compared to the Al sample (-1.334V), indicating a higher thermodynamic corrosion resistance. From a corrosion kinetics perspective, the corrosion current density of the F / K sample was 2.291 × 10⁻⁶. -7 A / cm 2 This is far lower than the 1.156 × 10⁻⁶ for the Al sample. -5 A / cm 2 The corrosion rate decreased by approximately two orders of magnitude, indicating a significant reduction in corrosion rate. The corrosion resistance of the four film materials, from highest to lowest, were samples F / K, F / H, F / B, and F.

[0065] (6) Impedance spectra of different fluorinated films: from Figure 6 (a) The Nyquist plot shows that the Al substrate has the smallest impedance arc radius. Among the four film types, F / H and F / K have the largest impedance arc radii, followed by F / B, and F has the smallest. This indicates that the F / H and F / K systems have better corrosion resistance, while the F system has relatively weaker protective capabilities. Figure 6 (b) The Bode plot shows that the impedance modulus |Z| of the matrix Al is the lowest across the entire frequency range, while the |Z| values ​​of F / K and F / B are the highest in the low-frequency region, indicating that they have the strongest barrier ability against corrosive media, followed by F / H, while F is relatively weaker. From Figure 6 (c) From the phase angle diagram, the peak phase angle of the film sample is significantly higher than that of the substrate Al, and the peak phase angle of F / K is higher and occurs less frequently. This indicates that the film is denser, has more obvious capacitance behavior, and has a stronger inhibitory effect on corrosion reaction.

[0066] (7) Design of orthogonal experiments to obtain the optimal F / K film: Based on the above experimental results, it is concluded that the F / K film prepared by this invention has the strongest ability to improve the corrosion resistance of aluminum alloys. Orthogonal experiments were then conducted, and the orthogonal experimental results are shown in Table 1. The impedance spectra of each sample are as follows: Figure 7As shown in (a) the Nyquist plot, sample No. 14 has the largest capacitive arc radius, indicating that it has the highest film resistance and charge transfer resistance, and the strongest barrier ability against corrosive media. The capacitive arc radii of other samples are relatively small, indicating weaker protective performance. From (b) the Bode plot, it can be seen that the samples with excellent protective performance have higher and wider phase angles in the mid-to-low frequency region, indicating better film uniformity and interfacial capacitance behavior closer to that of an ideal capacitor. Figure 7 (c) As can be seen from the phase angle diagram, the superior sample has a higher impedance modulus across the entire frequency band, further confirming its stronger corrosion inhibition capability.

[0067] Table 1. Orthogonal experimental table for optimizing F / K film properties.

[0068]

[0069] Therefore, the optimal process was determined to be 74 g / L + 90 g / L KF-EG, with a current density of 6 A / dm³. 2 The sample obtained with a duty cycle of 30%, a pulse frequency of 800 Hz, and a duration of 12 min was named F / K-optimized. Figure 8 As can be seen, the interface between the film layer and the aluminum alloy substrate in the F / K-optimized sample is distinct, and the film layer thickness is approximately 25 μm. The elements in the film layer are uniformly distributed, and no local enrichment phenomenon is observed.

Claims

1. A method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface, characterized in that, Includes the following steps: Step 1: Pre-treat the aluminum alloy substrate and set it aside for later use; Step 2: Prepare a fluorinated organic electrolyte, wherein the electrolyte contains ammonium fluoride and potassium fluoride; Step 3: Using a stainless steel plate as the cathode and a pretreated aluminum alloy substrate as the anode, plasma electrolytic fluorination process is carried out in constant current pulse mode. Step 4: After processing, remove the sample, clean and dry it to obtain a fluorinated anti-corrosion film on the aluminum alloy surface.

2. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 1, the pretreatment specifically involves: grinding the aluminum alloy sample step by step with sandpaper, then washing it with NaOH alkali, then with hydrochloric acid, then ultrasonically cleaning it with ethanol, and finally drying it for later use.

3. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 2, the fluorinated organic electrolyte is one or more of the following: an ethylene glycol solution of ammonium fluoride, an ethylene glycol solution of potassium fluoride, an ethylene glycol solution of ammonium bifluoride, and an ethylene glycol solution of lithium tetrafluoroborate. The concentration of ammonium fluoride is 40-120 g / L, the concentration of potassium fluoride is 20-100 g / L, the concentration of ammonium bifluoride is 0-58 g / L, and the concentration of lithium tetrafluoroborate is 0-58 g / L.

4. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 2, the fluorinated organic electrolyte is an ethylene glycol solution containing 74 g / L ammonium fluoride and / or 90 g / L potassium fluoride.

5. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 3, the anode current density in the constant current pulse mode is 2~12 A / dm². 2 .

6. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 3, the pulse frequency in the constant current pulse mode is 200~2000Hz.

7. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 3, the pulse duty cycle in the constant current pulse mode is 5%~50%.

8. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 3, the plasma electrolytic fluorination process takes 5 to 30 minutes.

9. The method for preparing a fluorinated anti-corrosion film on an aluminum alloy surface according to claim 1, characterized in that, In step 3, the plasma electrolytic fluorination process parameters are: current density 6 A / dm³. 2 The pulse frequency is 800Hz, the duty cycle is 30%, and the processing time is 12min.

10. The fluorinated anti-corrosion film on the surface of aluminum alloy prepared by the preparation method according to any one of claims 1-9.