A large-section aluminum bar efficient composite copper plating integrated forming device and preparation process
Through integrated continuous production lines and intelligent control, the problems of low production efficiency and unstable quality in copper plating of large-section aluminum busbars have been solved, achieving efficient, safe, and uniform coating bonding effects and ensuring consistent product quality.
Patent Information
- Application Number
- CN202611317705.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Existing large-section aluminum busbar copper plating technology suffers from problems such as low production efficiency, insufficient coating adhesion, oxide film affecting bonding strength, poor equipment adaptability, and difficulty in ensuring quality consistency.
An integrated continuous production line is adopted, including feeding, pretreatment, pre-plating, main plating, post-treatment and annealing units. Combined with cyanide-free pre-plating, ultrasonic and combined magnetic fields, the entire process of copper plating on aluminum bars is automated. The process parameters are monitored and adjusted in real time through a central control system, and protective atmosphere annealing is used to improve the bonding strength and uniformity.
It enables continuous production of copper plating on large-section aluminum busbars, improving production efficiency and coating bonding strength, ensuring coating uniformity and product quality consistency, and is environmentally friendly and safe.
Smart Images

Figure CN123153137A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of busbar manufacturing technology, specifically to a high-efficiency composite copper-plated integrated forming device and preparation process for large-section aluminum busbars, which is suitable for the large-scale production of copper-clad aluminum composite busbars for power transmission and electrical equipment connection. Background Technology
[0002] Copper-clad aluminum composite busbars combine the excellent conductivity of copper with the lightweight and low-cost advantages of aluminum, making them promising for applications in power transmission and electrical connections. Large-section copper-clad aluminum busbars typically refer to those with a cross-section of 300–1000 mm², where the aluminum core comprises 75%–85% and the copper layer 15%–25%. However, existing copper plating technologies for large-section aluminum busbars still have several shortcomings: First, traditional copper plating of aluminum busbars often adopts a split process route, with cleaning, pre-plating, main plating, and post-treatment processes completed in separate equipment. The workpiece is frequently transferred between these processes, which not only reduces production efficiency but also increases the risk of secondary surface contamination and affects the coating adhesion quality.
[0003] Secondly, copper-clad aluminum busbars produced by existing electroplating methods generally suffer from thin copper plating and insufficient adhesion between the plating and the aluminum substrate, which makes it easy for the bimetal to separate during subsequent rolling and stretching processes, making it difficult to meet the requirements for the use of large-section conductive busbars.
[0004] Third, aluminum is an amphoteric metal, and a dense oxide film (Al2O3) easily forms on its surface. If this oxide film is not completely removed or is not promptly re-plated, it will seriously affect the bonding strength between the coating and the substrate. Existing processes mostly use cyanide pre-plating systems, which not only pose safety hazards and environmental pressures, but also have unstable treatment effects on large-section aluminum busbars.
[0005] Fourth, existing equipment has poor adaptability to large-section aluminum busbars, cannot flexibly adjust process parameters according to different specifications of aluminum busbars, and lacks online monitoring and closed-loop control functions, making it difficult to guarantee product quality consistency.
[0006] To address the aforementioned problems, this invention provides an integrated forming device and manufacturing process for high-efficiency composite copper plating of large-section aluminum busbars that integrates multiple processes and enables continuous production. Summary of the Invention
[0007] The present invention aims to overcome the shortcomings of the prior art and provide an integrated forming device and preparation process for high-efficiency composite copper plating of large cross-section aluminum busbars, so as to realize continuous and automated production of copper plating of large cross-section aluminum busbars, improve the bonding strength between the coating and the aluminum substrate, and ensure the uniformity of coating thickness and the consistency of product quality.
[0008] To achieve the above objectives, the present invention provides the following technical solution: A high-efficiency composite copper plating integrated forming device for large-section aluminum busbars includes a feeding mechanism, a pre-treatment unit, a pre-plating unit, a main plating unit, a post-treatment unit, an annealing unit, and an unloading mechanism arranged sequentially along the aluminum busbar conveying direction. The units are connected by a closed conveying channel. The pretreatment unit includes a degreasing tank, an alkaline etching tank, an acid pickling tank, and a zinc immersion tank connected in sequence, with a spray water washing section between each tank. The pre-plating unit is a cyanide-free pre-plating tank, which is equipped with an anode copper plate and a cathode conductive clamp. The cathode conductive clamp is an adjustable clamp, suitable for aluminum busbars with different cross-sectional dimensions. The main plating unit is a sulfate copper plating tank, which is equipped with an anode copper ball basket, a cathode conductive device and a circulation filtration system. An ultrasonic generator is installed at the bottom of the sulfate copper plating tank and a combined magnetic field generator is installed on the side wall. The post-processing unit includes a cleaning tank, a passivation tank, and a drying tank connected in sequence. The annealing unit is a continuous protective atmosphere annealing furnace, which is equipped with a temperature zone control device and an atmosphere conditioning device. The device is also equipped with a central control system, which is electrically connected to the actuators and sensors of each unit to achieve fully automated control of the entire process.
[0009] As a further improvement, the combined magnetic field generating device includes a rotating magnetic field generator and a traveling wave magnetic field generator. The rotating magnetic field generator is disposed at the bottom or side wall of the sulfate copper plating tank, and the traveling wave magnetic field generator is arranged along the length of the sulfate copper plating tank.
[0010] As a further improvement, the ultrasonic frequency of the ultrasonic generator is 20~80kHz, and the ultrasonic power density is 0.5~5W / cm².
[0011] As a further improvement, the cathode conductive clamp includes a fixed clamping plate and a movable clamping plate, the movable clamping plate being driven by a cylinder or a hydraulic cylinder, and the clamping surface being provided with a conductive copper pad.
[0012] As a further improvement, the sealed conveying channel is equipped with an inert gas protection device to prevent oxidation of the surface of the treated aluminum busbar during inter-process transfer.
[0013] As a further improvement, the sulfate copper plating tank is equipped with a temperature sensor, a pH sensor, and a copper ion concentration sensor. Each sensor is connected to a central control system, which automatically adjusts the tank temperature and replenishes additives based on the sensor feedback signals.
[0014] As a further improvement, the protective atmosphere of the annealing furnace is nitrogen or argon, and the annealing temperature is 300~450℃.
[0015] A high-efficiency composite copper plating process for large cross-section aluminum busbars, implemented using the above-mentioned apparatus, includes the following steps: Step 1: Feeding and Pre-treatment: Large-section aluminum bars are fed into the pretreatment unit through a feeding mechanism. They are then chemically degreased in a degreasing tank, alkalinely etched in an alkaline etching tank, acid pickling activated in an acid pickling tank, and zinc immersion treated in a zinc immersion tank. Each step is followed by a water spray wash. Step 2, Pre-plating copper: The pretreated aluminum busbar is sent into the cyanide-free pre-plating tank of the pre-plating unit for copper pre-plating. The temperature in the pre-plating tank is 20~50℃ and the pre-plating time is 1~5min, forming a thin and uniform pre-plated copper layer on the surface of the aluminum busbar. Step 3, Main copper plating: The pre-copper-plated aluminum busbar is sent into the main plating unit for sulfate copper plating. During the main plating process, the ultrasonic generator and the combined magnetic field generator are turned on. The electroplating current density is 1~5A / dm², the plating solution temperature is 20~40℃, and the electroplating time is 30~120min. Step 4: Post-processing: The aluminum busbars that have completed the main plating are sequentially sent to the cleaning tank for cleaning, the passivation tank for passivation treatment, and the drying tank for drying. Step 5: Annealing treatment: The dried aluminum busbars are sent into a continuous protective atmosphere annealing furnace for annealing treatment. The annealing temperature is 300~450℃ and the annealing time is 30~90min. Diffusion annealing is completed under a protective atmosphere. Step Six: Material Inspection After annealing, the material is cooled in the cooling section and then output through the unloading mechanism for visual inspection and coating thickness detection.
[0016] As a further improvement, the alkaline etching treatment in step one uses NaOH solution with a concentration of 40~80g / L, a temperature of 50~70℃, and a treatment time of 1~5min; the acid washing activation uses a mixed acid solution prepared by nitric acid and hydrofluoric acid in a volume ratio of 3:1~5:1, and a treatment time of 0.5~3min.
[0017] As a further improvement, the zinc immersion treatment in step one uses zinc immersion liquid, the immersion time is 30~120s, the immersion temperature is 15~30℃, and after zinc immersion, it is washed with water and then enters the pre-plating unit.
[0018] As a further improvement, the combined magnetic field in step three is a superposition of a rotating magnetic field and a traveling wave magnetic field, with the magnetic induction intensity of the rotating magnetic field being 0.01~0.5T and the magnetic induction intensity of the traveling wave magnetic field being 0.005~0.2T.
[0019] As a further improvement, the ultrasonic waves described in step three are applied continuously during the electroplating process, or applied in segments during the early and / or later stages of electroplating.
[0020] As a further improvement, the annealing process described in step five is carried out under a nitrogen protective atmosphere. The annealing temperature is controlled in sections for heating, holding, and cooling. The heating rate is 5~15℃ / min, the holding time is 30~60min, and the cooling rate is 3~10℃ / min.
[0021] Compared with the prior art, the beneficial effects of the present invention are: 1. Integrated continuous production significantly improves efficiency. This invention integrates multiple processes such as degreasing, alkaline etching, pickling, zinc immersion, pre-plating, main plating, post-treatment, and annealing into an integrated continuous production line. The units are connected by a closed conveyor channel, realizing the entire process of copper plating on large-section aluminum busbars in a continuous and automated manner. This avoids frequent transfer of workpieces between processes and greatly improves production efficiency.
[0022] 2. High coating bonding strength and reliable quality. This invention employs a combined pretreatment process of "alkaline etching → acid pickling → zinc immersion" in the pretreatment stage, effectively removing the oxide film on the aluminum busbar surface and forming an intermediate layer conducive to coating bonding. In the pre-plating stage, a cyanide-free pre-plating process is used to form a uniform pre-plated copper layer on the aluminum busbar surface. In the main plating stage, ultrasonic waves and a combined magnetic field are applied simultaneously. Ultrasonic waves enhance mass transfer in the plating solution and refine grains, while the combined magnetic field ensures uniform coating distribution and improves coating density. Finally, diffusion annealing under a protective atmosphere promotes interfacial diffusion bonding between the copper layer and the aluminum substrate, significantly improving the bonding strength between the coating and the substrate.
[0023] 3. Good coating uniformity and controllable thickness. The adjustable cathode conductive fixture of this invention is suitable for aluminum busbars with different cross-sectional dimensions. The synergistic effect of the combined magnetic field and ultrasonic waves ensures uniform deposition of the coating on all surfaces of large-section aluminum busbars, avoiding the problem of uneven coating thickness caused by edge effects in traditional electroplating.
[0024] 4. High degree of intelligence and consistent product quality. This invention features a central control system and multiple online sensors, which can monitor and automatically adjust key process parameters such as bath temperature, pH value, and copper ion concentration in real time, achieving closed-loop control and ensuring consistent product quality between batches.
[0025] 5. Green and environmentally friendly, safe and reliable. This invention adopts a cyanide-free pre-plating process, avoiding the use of cyanide and eliminating safety hazards and environmental pollution risks; at the same time, each tank operates in a closed manner, reducing the emission of harmful gases and improving the working environment. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0027] Figure 1 This is a structural block diagram of a high-efficiency composite copper plating integrated forming device for large-section aluminum busbars; Figure 2 This is a flowchart of a high-efficiency composite copper plating process for large-section aluminum busbars. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] Example 1 The apparatus and process of this invention are used to perform composite copper plating on large cross-section aluminum busbars with a cross-section size of 100mm×20mm and a length of 3000mm.
[0030] Step 1: Feeding and Pre-treatment: The aluminum busbar is fed into the pre-processing unit via a feeding mechanism and undergoes the following processing in sequence: (1) Chemical degreasing: Alkaline degreasing solution (sodium hydroxide 30g / L, sodium carbonate 20g / L, sodium phosphate 15g / L, surfactant 5g / L) is used in the degreasing tank at a temperature of 65℃ for 3 minutes, followed by spray washing with water; (2) Alkaline etching: Sodium hydroxide solution (60g / L) is used in the alkaline etching tank at a temperature of 60℃ for 3 minutes, followed by spraying with water for washing; (3) Pickling activation: A mixed acid solution (nitric acid and hydrofluoric acid volume ratio 4:1) is used in the pickling tank and treated at room temperature for 1.5 min, followed by spraying with water. (4) Zinc immersion: Zinc immersion solution (zinc oxide 20g / L, sodium hydroxide 120g / L, potassium sodium tartrate 15g / L, ferric chloride 2g / L) is used in zinc immersion tank at 25℃ for 60s, followed by spraying with water.
[0031] Step 2, Pre-plating copper: The pretreated aluminum busbar is fed into the cyanide-free pre-plating tank of the pre-plating unit for copper pre-plating. The pre-plating solution consists of 30 g / L copper pyrophosphate, 280 g / L potassium pyrophosphate, and 15 g / L potassium citrate, with a pH of 8.5, a temperature of 40℃, a current density of 1.5 A / dm², and a pre-plating time of 3 min, forming a uniform pre-plated copper layer on the surface of the aluminum busbar.
[0032] Step 3, Main copper plating: The pre-copper-plated aluminum busbar is then fed into the sulfate copper plating bath of the main plating unit for primary copper plating. The main plating solution consists of: 180 g / L copper sulfate, 60 g / L sulfuric acid, 60 mg / L chloride ions, and an appropriate amount of brightener. The temperature is 25℃, the current density is 3 A / dm², and the plating time is 60 min. During the primary plating process, an ultrasonic generator is activated at a frequency of 40 kHz and a power density of 2 W / cm². Simultaneously, a combined magnetic field generator is activated, with a rotating magnetic field magnetic induction intensity of 0.1 T and a traveling wave magnetic field magnetic induction intensity of 0.05 T.
[0033] Step 4: Post-processing: After the main plating is completed, the aluminum busbar is sequentially sent to the cleaning tank for three-stage countercurrent cleaning, the passivation tank for passivation treatment (passivation solution composition: chromium anhydride 5g / L, sulfuric acid 2ml / L, room temperature treatment for 30s), and the drying tank for hot air drying (temperature 80℃).
[0034] Step 5: Annealing treatment: The dried aluminum busbars are fed into a continuous protective atmosphere annealing furnace and annealed under a nitrogen protective atmosphere. The heating rate is 10℃ / min, the temperature is raised to 350℃ and held for 45 min, and then the temperature is lowered to below 100℃ at a rate of 5℃ / min before being removed from the furnace.
[0035] Step Six: Material Inspection After annealing, the material is cooled in a cooling section and then output through a feeding mechanism. Testing showed that the coating thickness was 150μm (thickness deviation of the four sides of the aluminum busbar cross-section ≤ ±8μm), the adhesion between the coating and the substrate passed both cross-cut adhesion and thermal shock tests, and the conductivity met design requirements.
[0036] Example 2 The apparatus and process of this invention are used to perform composite copper plating on another type of large-section aluminum busbar with a cross-sectional size of 150mm×30mm and a length of 4000mm.
[0037] Except for the following parameter adjustments, the remaining steps are the same as in Example 1: In the pretreatment, the alkaline etching temperature was adjusted to 65℃ and the treatment time was 4 minutes; the zinc immersion time was adjusted to 90 seconds.
[0038] During the copper pre-plating process, the temperature was 45℃, the current density was 2A / dm², and the pre-plating time was 4min.
[0039] In the main copper plating process, the current density was 4A / dm², the plating time was 90min, the ultrasonic frequency was 60kHz, the power density was 3W / cm², the magnetic induction intensity of the rotating magnetic field was 0.15T, and the magnetic induction intensity of the traveling wave magnetic field was 0.08T.
[0040] During the annealing process, the temperature is raised to 380℃ and held for 50 minutes.
[0041] Tests showed that the coating thickness was 200μm (thickness deviation on each surface ≤ ±10μm), and the coating was uniform, dense, and had good adhesion.
[0042] Example 3 The apparatus and process of this invention are used to perform composite copper plating on a third type of large-section aluminum busbar with a cross-sectional size of 80mm×15mm and a length of 2500mm.
[0043] Except for the following parameter adjustments, the remaining steps are the same as in Example 1: In the pretreatment, the alkaline etching temperature was 55℃ and the treatment time was 2 min; the pickling time was 1 min; and the zinc immersion time was 40 s.
[0044] During the copper pre-plating process, the temperature was 35℃, the current density was 1A / dm², and the pre-plating time was 2min.
[0045] During the main copper plating process, the current density was 2A / dm², the plating time was 45min, the ultrasonic frequency was 35kHz, the power density was 1.5W / cm², the magnetic induction intensity of the rotating magnetic field was 0.08T, and the magnetic induction intensity of the traveling wave magnetic field was 0.03T.
[0046] During the annealing process, the temperature is raised to 320℃ and held for 35 minutes.
[0047] The coating thickness was found to be 120 μm (with a thickness deviation of ≤ ±5 μm on each surface), indicating good coating quality.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A high-efficiency composite copper plating integrated forming device for large-section aluminum busbars, comprising a feeding mechanism, a pre-treatment unit, a pre-plating unit, a main plating unit, a post-treatment unit, an annealing unit, and a unloading mechanism arranged sequentially along the aluminum busbar conveying direction, wherein the units are connected by a closed conveying channel, characterized in that, The sealed conveying channel is equipped with an inert gas protection device. The pretreatment unit includes a degreasing tank, an alkaline etching tank, an acid pickling tank, and a zinc immersion tank connected in sequence, with a spray water washing section between each tank. The pre-plating unit is a cyanide-free pre-plating tank, which is equipped with an anode copper plate and a cathode conductive clamp. The cathode conductive clamp is an adjustable clamp suitable for aluminum bars with different cross-sectional sizes. The cathode conductive clamp includes a fixed clamp plate and a movable clamp plate. The movable clamp plate is driven by a cylinder or a hydraulic cylinder, and the clamping surface is equipped with a conductive copper pad. The main plating unit is a sulfate copper plating tank, which is equipped with an anode copper ball basket, a cathode conductive device and a circulation filtration system. An ultrasonic generator is installed at the bottom of the sulfate copper plating tank and a combined magnetic field generator is installed on the side wall. The post-processing unit includes a cleaning tank, a passivation tank, and a drying tank connected in sequence. The annealing unit is a continuous protective atmosphere annealing furnace, which is equipped with a temperature zone control device and an atmosphere conditioning device. The device is also equipped with a central control system, which is electrically connected to the actuators and sensors of each unit to achieve fully automated control of the entire process.
2. The integrated forming device for high-efficiency composite copper plating of large cross-section aluminum busbars according to claim 1, characterized in that, The combined magnetic field generating device includes a rotating magnetic field generator and a traveling wave magnetic field generator. The rotating magnetic field generator is located at the bottom or side wall of the sulfate copper plating tank, and the traveling wave magnetic field generator is arranged along the length of the sulfate copper plating tank.
3. The integrated forming device for high-efficiency composite copper plating of large cross-section aluminum busbars according to claim 1, characterized in that, The ultrasonic frequency of the ultrasonic generator is 20~80kHz, and the ultrasonic power density is 0.5~5W / cm².
4. The integrated forming device for high-efficiency composite copper plating of large cross-section aluminum busbars according to claim 1, characterized in that, The sulfate copper plating tank is equipped with a temperature sensor, a pH sensor, and a copper ion concentration sensor. Each sensor is connected to a central control system, which automatically adjusts the tank temperature and replenishes additives based on the sensor feedback signals.
5. The integrated forming device for high-efficiency composite copper plating of large cross-section aluminum busbars according to claim 1, characterized in that, The protective atmosphere of the annealing furnace is nitrogen or argon, and the annealing temperature is 300~450℃.
6. A process for preparing a high-efficiency composite copper plating of a large cross-section aluminum busbar, implemented using the apparatus described in any one of claims 1 to 7, characterized in that... Includes the following steps: S1 Feeding and Pretreatment: The large cross-section aluminum busbar is fed into the pretreatment unit through the feeding mechanism. It passes through the degreasing tank for chemical degreasing, the alkaline etching tank for alkaline etching, the pickling tank for pickling activation, and the zinc immersion tank for zinc immersion. Each step is followed by a water spray wash. S2 Copper Pre-plating: The pre-treated aluminum busbar is sent into the cyanide-free pre-plating tank of the pre-plating unit for copper pre-plating. The temperature in the pre-plating tank is 20~50℃ and the pre-plating time is 1~5min. S3 Main Copper Plating: The pre-copper-plated aluminum busbar is sent into the main plating unit for sulfate copper plating. During the main plating process, the ultrasonic generator and the combined magnetic field generator are turned on. The electroplating current density is 1~5A / dm², the plating solution temperature is 20~40℃, and the electroplating time is 30~120min. The combined magnetic field is the superposition of a rotating magnetic field and a traveling wave magnetic field. The magnetic induction intensity of the rotating magnetic field is 0.01~0.5T, and the magnetic induction intensity of the traveling wave magnetic field is 0.005~0.2T. S4 post-processing: The aluminum busbars that have been plated are sequentially sent to the cleaning tank for cleaning, the passivation tank for passivation treatment, and the drying tank for drying. S5 Annealing: The dried aluminum busbar is sent into a continuous protective atmosphere annealing furnace for annealing. The annealing temperature is 300~450℃ and the annealing time is 30~90min. S6 Material Inspection: After annealing, the material is cooled in the cooling section and then output through the material feeding mechanism.
7. The preparation process of a high-efficiency composite copper plating of a large cross-section aluminum busbar according to claim 6, characterized in that, The alkaline etching treatment in S1 uses NaOH solution with a concentration of 40~80g / L, a temperature of 50~70℃, and a treatment time of 1~5min; the acid washing activation uses a mixed acid solution prepared by nitric acid and hydrofluoric acid in a volume ratio of 3:1~5:1, and a treatment time of 0.5~3min.
8. The preparation process of a high-efficiency composite copper plating of a large cross-section aluminum busbar according to claim 6, characterized in that, The zinc immersion treatment described in S1 uses a zinc immersion solution, with an immersion time of 30~120s and an immersion temperature of 15~30℃.
9. The preparation process of a high-efficiency composite copper plating of a large cross-section aluminum busbar according to claim 6, characterized in that, The ultrasonic waves described in S3 are applied continuously during the electroplating process, or applied in segments at the beginning or end of the electroplating process.
10. The preparation process of a high-efficiency composite copper plating of a large cross-section aluminum busbar according to claim 6, characterized in that, The annealing process described in S5 is carried out under a nitrogen protective atmosphere. The annealing temperature is controlled in zones: heating, holding, and cooling. The heating rate is 5~15℃ / min, the holding time is 30~60min, and the cooling rate is 3~10℃ / min.